Portland cement reinforcing agent as well as preparation method and application thereof

The silicate cement reinforcement prepared by high-temperature calcination and quenching treatment solves the problem that the existing cement-based early strength and late strength are difficult to take into account in silicate cement, and the early and late compressive strength of cement is achieved. Improved and optimized durability performance.

CN118908611AActive Publication Date: 2024-11-08BEIJING UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411026646.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

When existing cement-based early strength agents improve the early strength of silicate cement, it is difficult to ensure late strength and durability at the same time. Commonly used accelerators have the risk of steel bar corrosion or toxicity problems, and the preparation process is complex and high temperature, making it difficult to prepare.

Method used

The silicate cement reinforcement prepared by using CaO, SiO2 and CaCl2 as raw materials for high-temperature calcination, quench cooling and grinding, is composed of Ca3SiO4Cl2, Ca2SiO4 and a small amount of SiO2. By accelerating the cement hydration rate and reducing porosity, it improves the early and later stages of cement. Compressive strength.

Benefits of technology

It significantly improves the early compressive strength and later flexural strength of silicate cement, reduces the free chloride ion content, reduces the porosity, optimizes the pore size distribution, and improves the overall strength and durability of the cement.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of cement-based admixtures, in particular to a Portland cement reinforcing agent and a preparation method and application thereof.The Portland cement reinforcing agent is prepared by taking CaO, Si O2 and CaC12 as raw materials through high-temperature calcination, quenching and grinding and comprises the components of Ca3Si O4C12, Ca2Si O4 and a small amount of Si O2, the hydration rate of a mineral phase of Portland cement clinker can be increased by adding the Portland cement reinforcing agent into a cementing material, and the mineral phase of the Portland cement clinker can be increased by adding the Portland cement reinforcing agent into the cementing material; the compressive strength of the cement-based material is obviously improved, the early-stage breaking strength of the cement-based material can be improved, and the later-stage breaking strength of cement mortar is not damaged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-based admixtures, and in particular to a silicate cement reinforcing agent and a preparation method and application thereof. Background Art

[0002] Cement concrete is widely used in the field of construction, but its slow setting and hardening speed and long early strength development time limit the application of cement concrete in some special cases. As an admixture, early strength agent can accelerate the hydration speed of cement and promote the development of early strength of concrete, making up for the application of cement concrete in cold climate areas, emergency projects and road repairs, which require rapid hardening and strength generation.

[0003] At present, commonly used early strength agents include two categories: chlorine-based and non-chlorine-based. Chlorine-based agents include calcium chloride (CaCl2), alkali metal chlorides, etc., and non-chlorine-based agents include nitrates, nitrites, thiocyanates, formates and alcohol amines. CaCl2 can promote the hydration rate of cement, shorten the setting time of cement, and improve the strength of cement; alkali metal chlorides can also promote the improvement of cement strength, but the improvement effect is limited, and it will also increase the risk of alkali-aggregate reaction, causing problems such as reduced strength and durability in the later stage. Chlorine-based accelerators are easily soluble in water, forming a large amount of free chlorine, which will destroy the passivation film formed by the steel bars in the highly alkaline environment in reinforced concrete, thereby accelerating the corrosion of steel bars. Among the non-chlorine-based accelerators, nitrates have a smaller promoting effect on cement strength, and nitrite and thiocyanate accelerators have weak toxicity, so they are less used; alcohol amine accelerators can improve the early strength of cement, but have little effect on the later strength of cement, and the amount of alcohol amine accelerators used is not easy to control. The effect is not obvious when the amount is small, and the use of a large amount is likely to cause problems with the working performance of cement.

[0004] The prior art US4119467A and JPS534033A patents disclose an early-strength cement mainly composed of alite, belite, calcium chloroaluminate, calcium chlorosilicate and calcium chloroaluminoferrate. However, the preparation temperature of the cement is high and the preparation method is complicated. The early strength of the cement mainly comes from the hydration of chlorine-containing minerals with a high chlorine content, so the preparation is difficult. In this technology, when the content of alite and belite is high, the 3d strength of the cement is less than 5MPa. When the content of chlorine-containing minerals is high, the later strength of the cement is insufficient. As the most widely used cement, silicate cement requires not only high early strength but also sufficient later strength. The two mineral phases C3A and C3S provide the early strength in silicate cement, while C2S provides the later strength. Therefore, this patented technology cannot be used to guide how to improve the strength performance of silicate cement, and its application scenarios are limited. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a silicate cement strengthener, which is prepared by high-temperature calcination, rapid cooling and grinding with CaO, SiO2 and CaCl2 as raw materials, and the components are Ca3SiO4Cl2, Ca2SiO4 and a small amount of SiO2. The silicate cement strengthener is added to the cementitious material to increase the hydration rate of the silicate cement clinker mineral phase, has a significant effect on improving the compressive strength of the cement-based material, and can improve the early flexural strength of the cement-based material without damaging the later flexural strength of the cement mortar.

[0006] Specifically, the preparation method of the silicate cement strengthener of the present invention is prepared by the following steps:

[0007] 1) Weigh 110-120 parts of CaO, 55-65 parts of SiO2, and 110-115 parts of CaCl2 by weight.

[0008] 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes.

[0009] 3) Calcine the cake at 850-950°C for 1.5-2h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

[0010] The main components of the silicate cement enhancer of the present invention are Ca3SiO4Cl2, Ca2SiO4 and a small amount of SiO2, wherein Ca3SiO4Cl2 can provide calcium ions required for part of cement hydration through its own dissolution, and can also provide CSH gel as a nucleation site to promote cement hydration through its hydration. The present invention studies show that the Ca3SiO4Cl2 component has little effect on the induction period in the early stage of cement hydration, and mainly improves the hydration rate of cement in the acceleration period and increases the hydration exothermic peak, and can also accelerate the hydration of C2S and C4AF in the late stage of cement hydration, and increase the content of hydration products such as CSH gel, so that Ca3SiO4Cl2 can promote the hydration rate of cement clinker phase and improve the strength performance of cement at the same age.

[0011] In addition, the silicate cement enhancer prepared by the present invention has part of chlorine dissolved from the mineral, which reacts with the aluminum phase in the cement to form F salt, which can reduce the content of free chloride ions on the one hand, and the small-particle F salt formed can also fill pores, reduce porosity and optimize pore size distribution, increase the proportion of gel pores, and help improve the strength and durability of cement. Ca3SiO4Cl2 can accelerate the hydration rate of C3S and aluminum phase (C3A, C4AF) in cement in the early stage, and can accelerate the hydration rate of C2S in the later stage, and improve the compressive strength of cement in 1-28d by reducing porosity and optimizing pore size distribution.

[0012] Preferably, in step 1), 115 parts of CaO, 60 parts of SiO2, and 111 parts of CaCl2 are weighed by weight.

[0013] Preferably, the grinding in step 2) is performed using a planetary ball mill, and the grinding time is 12-17 min.

[0014] Preferably, step 2) is performed by pressing using a press with a pressure of 100 KN.

[0015] Preferably, the diameter of the cake in step 2) is 10 cm.

[0016] Preferably, the calcination in step 3) is carried out in a muffle furnace.

[0017] Preferably, the rapid cooling in step 3) is performed by air cooling.

[0018] The present invention also relates to a silicate cement reinforcing agent, which is specifically prepared by the above-mentioned preparation method.

[0019] The present invention also relates to the application of the above-mentioned silicate cement reinforcing agent in improving the strength of cement. Preferably, the addition amount of the silicate cement reinforcing agent in the cementitious material is 0.1-10%. DETAILED DESCRIPTION

[0020] To prove the technical effect of the present invention, a silicate cement strengthener was prepared and added to the mortar as an admixture. The compressive strength of the mortar was measured in accordance with GBT17671-2021 "Test method for strength of cement mortar (ISO method)", wherein P·O42.5 cement was used and the amount of silicate cement strengthener added was 5% of the mass of the cementitious material.

[0021] Example 1

[0022] The silicate cement reinforcing agent is prepared by the following steps:

[0023] 1) Weigh 115 parts of CaO, 60 parts of SiO2, and 111 parts of CaCl2 by weight.

[0024] 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes.

[0025] 3) Calcine the cake at 850°C for 2h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

[0026] After testing, the mortar's 3d compressive strength was 37.3MPa, 7d compressive strength was 49.6MPa, and 28d compressive strength was 66.3MPa.

[0027] Example 2

[0028] The silicate cement reinforcing agent is prepared by the following steps:

[0029] 1) Weigh 120 parts of CaO, 55 parts of SiO2, and 115 parts of CaCl2 by weight.

[0030] 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes.

[0031] 3) Calcine the cake at 950°C for 1.5h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

[0032] After testing, the mortar's 3d compressive strength was 36.5MPa, 7d compressive strength was 47.9MPa, and 28d compressive strength was 65.0MPa.

[0033] Comparative Example 1

[0034] The silicate cement reinforcing agent is prepared by the following steps:

[0035] 1) Weigh 160 parts of CaO, 65 parts of SiO2, and 75 parts of CaCl2 by weight.

[0036] 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes.

[0037] 3) Calcine the cake at 950°C for 1.5h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

[0038] After testing, the mortar's 3d compressive strength was 31.3MPa, 7d compressive strength was 40.5MPa, and 28d compressive strength was 52.4MPa.

[0039] Comparative Example 2

[0040] The silicate cement reinforcing agent is prepared by the following steps:

[0041] 1) Weigh 90 parts of CaO, 45 parts of SiO2, and 155 parts of CaCl2 by weight.

[0042] 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes.

[0043] 3) Calcine the cake at 950°C for 1.5h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

[0044] After testing, the mortar's 3d compressive strength was 31.7MPa, 7d compressive strength was 41.4MPa, and 28d compressive strength was 51.2MPa.

[0045] Comparative Example 3

[0046] The silicate cement reinforcing agent is prepared by the following steps:

[0047] 1) Weigh 120 parts of CaO, 55 parts of SiO2, and 115 parts of CaCl2 by weight.

[0048] 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes.

[0049] 3) Calcine the cake at 1050°C for 1.5h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

[0050] After testing, the mortar's 3d compressive strength was 33.4MPa, 7d compressive strength was 42.5MPa, and 28d compressive strength was 56.9MPa.

[0051] Blank example

[0052] In the blank case, no cement enhancer was added during the preparation of the mortar specimens.

[0053] After testing, the mortar's 3d compressive strength was 27.8MPa, 7d compressive strength was 36.1MPa, and 28d compressive strength was 47.6MPa.

[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a silicate cement reinforcing agent, characterized in that: Prepared by the following steps: 1) Weigh 110-120 parts of CaO, 55-65 parts of SiO2, and 110-115 parts of CaCl2 by weight. 2) Mix CaO, SiO2 and CaCl2 evenly, grind and press into cakes. 3) Calcine the cake at 850-950°C for 1.5-2h, quench, grind, and pass through a 200-mesh sieve to obtain the product.

2. The method for preparing a silicate cement reinforcing agent according to claim 1, characterized in that: In step 1), 115 parts of CaO, 60 parts of SiO2, and 111 parts of CaCl2 were weighed by weight.

3. The method for preparing the silicate cement reinforcing agent according to claim 1, characterized in that: Step 2) grinding is performed using a planetary ball mill, and the grinding time is 12-17 minutes.

4. The method for preparing the silicate cement reinforcing agent according to claim 1, characterized in that: Step 2) Pressing is performed using a press machine with a pressure of 100KN.

5. The method for preparing the silicate cement reinforcing agent according to claim 1, characterized in that: Step 2) The diameter of the cake is 10 cm.

6. The method for preparing the silicate cement reinforcing agent according to claim 1, characterized in that: Step 3) calcination is carried out using a muffle furnace.

7. The method for preparing the silicate cement reinforcing agent according to claim 1, characterized in that: Step 3) Rapid cooling is performed by air cooling.

8. A silicate cement reinforcing agent, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the silicate cement reinforcing agent according to claim 8 in improving cement strength.

10. The use according to claim 9, characterized in that: The amount of the silicate cement reinforcing agent added to the cementitious material is 0.1-10%.

Citation Information

Patent Citations

  • Ultra-retarding cement formula and retarding agent

    CN102381857A

  • Eu<2+>-activated chorine calcium silicate salt fluorescent powder and preparation method and application thereof

    CN102660263A

  • CEMENT AND PROCESS FOR MANUFACTURING THEREOF

    DK153320C

  • Cement-based material having freezing-suppressing function

    JP1999268935A

  • Environmentally friendly hydraulic composition

    JP2004002193A