Magnetoplumbite type barium ferrite and preparation method thereof

Magnetic barium ferrite prepared by sol-gel method, solving the problem of poor absorption performance of microwave absorbing materials in the high-frequency band in the prior art, achieving excellent absorption performance and dielectric performance, and satisfying the radar wave impedance matching requirements.

CN118908706APending Publication Date: 2024-11-08ARMOR ACADEMY OF CHINESE PEOPLES LIBERATION ARMY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410934063.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing microwave absorbing materials have poor absorption performance in the high-frequency band and have poor dielectric properties, making it difficult to effectively match radar waves, affecting the impedance matching of magnetic losses and electromagnetic waves.

Method used

The sol-gel method is used to prepare the magnetic barium ferrite. By controlling the molar ratio, calcining temperature and pH value of barium ions and iron ions, combined with citric acid as a complexing agent, it is heated and evaporated, preheated and calcined. Magnetic lithoplasmic barium ferrite with excellent wave absorption properties was prepared.

Benefits of technology

The prepared magnetic lead-like barium ferrite has excellent attenuation capability and impedance matching conditions, achieving a maximum absorbance bandwidth of 6.16GHz and a minimum reflection loss of -34.86dB, and a particle size distribution between 300 and 500nm. The main loss mechanisms are natural loss, polarization relaxation and eddy current loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908706A_ABST
    Figure CN118908706A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of microwave absorbing materials, and provides magnetoplumbite type barium ferrite and a preparation method thereof. The preparation method comprises the following steps: mixing an iron salt, a barium salt, a complexing agent and water, then carrying out a reaction to obtain a product solution, and sequentially carrying out heating evaporation, preheating treatment and calcination treatment on the product solution to obtain the magnetoplumbite type barium ferrite. According to the system disclosed by the invention, the influence of process parameters such as calcination temperature and reaction raw material ratio on ferrite microstructure and electromagnetic parameters is researched, so that the ferrite morphology performance is effectively regulated and controlled, and a microwave absorbing material with more excellent performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microwave absorbing materials, and in particular to a magnetoplumbite type barium ferrite and a preparation method thereof. Background Art

[0002] In the high-frequency band of radar waves, the magnetic properties of absorbing materials are particularly important. They not only affect the magnitude of magnetic loss, but also the large loss of high-frequency electromagnetic waves in the medium, making impedance matching difficult. Appropriate magnetic parameters are needed to increase the amount of radar waves entering the medium.

[0003] From the principle of electromagnetic wave absorption, we know that the selection of magnetic components has a significant impact on the wave absorption performance of the material. Ferrite has good magnetic properties (higher saturation magnetization, stronger high-frequency magnetic permeability, larger Snoek limit, thicker skin depth, good impedance matching characteristics and better magnetocrystalline anisotropy), excellent chemical stability and low preparation cost, so it has become one of the most widely used absorbers in magnetic components with wave absorption performance. There are many types of ferrites with different properties. In order to obtain magnetic materials faster and better, it is necessary to further optimize and improve the preparation of ferrite materials.

[0004] Combined with the characteristics of the commonly used preparation technology of magnetoplumbite ferrite, the sol-gel method can realize the preparation of ferrite nano-scale materials, and the stoichiometry of the sample components is easy to control, the purity of the target product is high, the calcination temperature is low, the preparation process is simple and economical, and it is an important technical means to meet the requirements of ferrite powder characterization and analysis. In addition, during the preparation process, process parameters such as the sol environment, calcination temperature, and reaction raw material ratio will have a significant impact on the morphology and structure of the ferrite powder. A reasonable preparation process can obtain a higher specific saturation strength and a reasonable coercive force, and then obtain ferrite powder with excellent absorbing performance. Therefore, how to provide a preparation method for ferrite with excellent absorbing performance has become a problem that technicians in this field urgently need to solve. Summary of the invention

[0005] In view of this, the present invention provides a magnetoplumbite type barium ferrite and a preparation method thereof, which aims to solve the technical problems that the existing microwave absorbing materials have unsatisfactory microwave absorbing performance in high frequency bands and poor dielectric properties.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention provides a method for preparing magnetoplumbite type barium ferrite, comprising the following steps:

[0008] Mixing iron salt, barium salt, complexing agent and water to obtain a product solution, and sequentially subjecting the product solution to heating evaporation, preheating treatment and calcination treatment to obtain magnetoplumbite type barium ferrite;

[0009] The calcination temperature is 800-1400° C., and the calcination time is 3-10 hours.

[0010] Furthermore, the molar ratio of barium ions in the barium salt to iron ions in the iron salt is 1:10-14.

[0011] Furthermore, the molar ratio of the complexing agent to the total content of metal ions is 1 to 5:1.

[0012] Furthermore, before the reaction, a pH regulator is added to the reaction system to adjust the pH of the reaction system to 6-9; the pH regulator includes aqueous ammonia.

[0013] Furthermore, the reaction temperature is 0-80° C., and the reaction time is 0.5-2 h.

[0014] Furthermore, the iron salt includes iron chloride or iron nitrate; the barium salt includes barium chloride or barium nitrate.

[0015] Furthermore, the complexing agent includes citric acid.

[0016] Furthermore, the heating evaporation temperature is 80-100° C., and the heating evaporation time is 30-40 hours.

[0017] Furthermore, the preheating treatment temperature is 400-500° C., and the preheating treatment time is 1-3 hours.

[0018] The present invention also provides magnetoplumbite type barium ferrite prepared by the above preparation method.

[0019] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] The magnetoplumbite barium ferrite prepared by the present invention is mainly in the form of hexagonal blocks, and its particle size is mainly distributed between 300 and 500 nm, and its main loss mechanisms are natural loss, polarization relaxation and eddy current loss. The magnetoplumbite barium ferrite prepared by the present invention has excellent attenuation capability and impedance matching conditions, and has a maximum absorption bandwidth of 6.16 GHz at a matching thickness of 2.34 mm; when the matching thickness is 3.1 mm, a minimum reflection loss of -34.86 dB is achieved at 39.92 GHz. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The phase structure diagrams of the magnetoplumbite type barium ferrite obtained at different molar ratios of barium and iron at different calcination temperatures, wherein (a) corresponds to Examples 1 to 3, (b) corresponds to Examples 4 to 6, (c) corresponds to Examples 7 to 9, and (d) corresponds to Examples 10 to 12;

[0022] Figure 2XRD patterns of the magnetoplumbite-type barium ferrite obtained in Examples 5, 8 and 11;

[0023] Figure 3 are SEM images of magnetoplumbite-type barium ferrite obtained at different calcination temperatures when the molar ratio of barium ions to iron ions is 1:12, wherein the calcination temperature of (a) and (b) is 800°C, the calcination temperature of (c) and (d) is 1000°C, the calcination temperature of (e) and (f) is 1200°C, and the calcination temperature of (g) and (h) is 1400°C;

[0024] Figure 4 TEM images of the magnetoplumbite-type barium ferrite obtained at different calcination temperatures when the molar ratio of barium ions to iron ions is 1:12, wherein (a) is a microscopic morphology of the product calcined at 800°C at different magnifications, (b) is a microscopic morphology of the product calcined at 1000°C at different magnifications, and (c) is a microscopic morphology of the product calcined at 1400°C at different magnifications;

[0025] Figure 5 The XPS spectrum of the magnetoplumbite-type barium ferrite obtained in Example 8, wherein (a) is the XPS general spectrum of the calcined product, (b), (c), and (d) are the detailed spectra of the O, Ba, and Fe elements in the calcined product, respectively;

[0026] Figure 6 As raw material 2+ with Fe 3+ Magnetic hysteresis loop diagram of the embodiment with a molar ratio of 1:12 at different calcination temperatures;

[0027] Figure 7 The graphs are the change of the real part (a), imaginary part (b) and electric loss angle (c) of the dielectric constant of the barium ferrite powder calcined at different temperatures;

[0028] Figure 8 It is the Cole-Cole curve equation diagram of barium ferrite powder calcined at different temperatures;

[0029] Fig. 9 The graphs are the change of the real part (a), imaginary part (b) and magnetic loss angle (c) of the magnetic permeability of barium ferrite powder sintered at different temperatures;

[0030] Fig.10 is the curve diagram of eddy current loss changing with frequency;

[0031] Fig.11 Attenuation coefficient and characteristic impedance diagram of barium ferrite, where (a) is the attenuation coefficient diagram and (b) is the characteristic impedance diagram;

[0032] Fig.12: is a curve diagram of reflection loss of barium ferrite varying with frequency, wherein (a) is a curve diagram of reflection loss of different barium ferrites at a thickness of 2.5 mm of the absorbing medium varying with frequency, and (b) is a curve diagram of reflection loss of barium ferrite powder calcined at 1200° C. at different thicknesses varying with frequency;

[0033] Fig.13 To match the thickness d and the reflection loss R of the electromagnetic wave frequency f L 3D model diagram, (a), (b) and (c) show the reflection loss diagrams of barium ferrite powder sintered at 1000℃, 1200℃ and 1400℃ respectively. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing magnetoplumbite type barium ferrite, comprising the following steps:

[0035] The iron salt, barium salt, complexing agent and water are mixed and reacted to obtain a product solution, and the product solution is heated for evaporation, preheated and calcined in sequence to obtain magnetoplumbite type barium ferrite.

[0036] In the present invention, the molar ratio of barium ions in the barium salt to iron ions in the iron salt is 1:10 to 14, preferably 1:11 to 13, and more preferably 1:12.

[0037] In the present invention, the molar ratio of the complexing agent to the total content of metal ions is 1 to 5:1, preferably 2 to 4:1, and more preferably 3:1.

[0038] In the present invention, a pH adjuster is added to the reaction system before the reaction to adjust the pH of the reaction system to 6 to 9, preferably 6.5 to 8.5, and more preferably 7 to 8; the pH adjuster includes ammonia water, and the pH adjuster used in the present invention does not introduce new impurities.

[0039] In the present invention, the reaction temperature is 0 to 80° C., preferably 10 to 60° C., and more preferably 20 to 30° C.; the reaction time is 0.5 to 2 h, preferably 0.8 to 1.6 h, and more preferably 1 to 1.5 h.

[0040] In the present invention, the iron salt includes ferric chloride or ferric nitrate, preferably ferric chloride; the barium salt includes barium chloride or barium nitrate, preferably barium chloride.

[0041] In the present invention, the complexing agent includes citric acid. The complexing agent used in the present invention can form a complex with metal ions to prevent component segregation.

[0042] In the present invention, the heating evaporation temperature is 80-100°C, preferably 85-95°C, and more preferably 90°C; the heating evaporation time is 30-40h, preferably 32-38h, and more preferably 34-36h.

[0043] In the present invention, the heating rate from the temperature of the heating evaporation to the temperature of the preheating treatment is 1 to 10° C. / min, preferably 2 to 8° C. / min, and more preferably 5° C. / min.

[0044] In the present invention, the temperature of the preheat treatment is 400-500°C, preferably 420-480°C, and more preferably 440-460°C; the time of the preheat treatment is 1-3h, preferably 1.5-2.5h, and more preferably 2h.

[0045] In the present invention, the heating rate from the temperature of the preheat treatment to the temperature of the calcination treatment is 5 to 15° C. / min, preferably 8 to 12° C. / min, and more preferably 10° C. / min.

[0046] In the present invention, the calcination temperature is 800-1400°C, preferably 900-1300°C, and more preferably 1000-1200°C; the calcination time is 3-10h, preferably 4-8h, and more preferably 5-6h.

[0047] In the present invention, the preheat treatment and the calcination treatment are both carried out under a protective atmosphere, and the protective atmosphere includes any one of nitrogen, argon, helium, and neon, preferably nitrogen or argon, and more preferably argon.

[0048] The present invention also provides magnetoplumbite type barium ferrite prepared by the above preparation method.

[0049] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0050] Example 1

[0051] FeC13·6H2O and BaCl2·2H2O were weighed to make the molar ratio of barium ions to iron ions 1:10, and FeC13·6H2O and BaCl2·2H2O were dissolved in 400mL of deionized water to prepare a solution, and citric acid was dissolved in the solution, wherein the molar ratio of citric acid to the total content of metal ions was 2:1. Then, the pH of the solution was adjusted to 8 using ammonia water, and the solution was stirred quickly to be fully mixed and reacted. After the reaction was completed, the product solution was heated and evaporated at 88°C for 36h to dehydrate it to obtain a sol. The sol was placed in a muffle furnace, heated to 450°C at a rate of 5°C / min in an argon atmosphere, and preheated for 2h; then heated to 800°C at a rate of 10°C / min for calcination, and magnetoplumbite-type barium ferrite was obtained after calcination for 5h.

[0052] Example 2

[0053] The same as Example 1, except that the molar ratio of barium ions to iron ions is 1:12.

[0054] Example 3

[0055] The same as Example 1, except that the molar ratio of barium ions to iron ions is 1:14.

[0056] Example 4

[0057] Weigh FeC13·6H2O and BaCl2·2H2O, so that the molar ratio of barium ions to iron ions is 1:10, dissolve FeC13·6H2O and BaCl2·2H2O in 400mL of deionized water to prepare a solution, and dissolve citric acid in the solution, wherein the molar ratio of citric acid to the total content of metal ions is 2:1. Then adjust the pH of the solution to 8 with ammonia water, stir the solution quickly to mix thoroughly and react. After the reaction is completed, continue to heat and evaporate the product solution at 88°C for 36h to dehydrate it to obtain a sol. Put the sol into a muffle furnace, heat it to 450°C at a rate of 5°C / min in an argon atmosphere, and preheat it for 2h; then heat it to 1000°C at a rate of 10°C / min for calcination, and obtain a magnetoplumbite-type barium ferrite after calcination for 4h.

[0058] Example 5

[0059] The same as Example 4, except that the molar ratio of barium ions to iron ions is 1:12.

[0060] Example 6

[0061] The same as Example 4, except that the molar ratio of barium ions to iron ions is 1:14.

[0062] Example 7

[0063] FeC13·6H2O and BaCl2·2H2O were weighed to make the molar ratio of barium ions to iron ions 1:10, and FeC13·6H2O and BaCl2·2H2O were dissolved in 400mL of deionized water to prepare a solution, and citric acid was dissolved in the solution, wherein the molar ratio of citric acid to the total content of metal ions was 2:1. Then, the pH of the solution was adjusted to 8 using ammonia water, and the solution was stirred quickly to be fully mixed and reacted. After the reaction was completed, the product solution was heated and evaporated at 90°C for 36h to dehydrate it to obtain a sol. The sol was placed in a muffle furnace, heated to 450°C at a rate of 5°C / min in an argon atmosphere, and preheated for 2.5h; then heated to 1200°C at a rate of 10°C / min for calcination, and magnetoplumbite-type barium ferrite was obtained after calcination for 3h.

[0064] Example 8

[0065] The same as Example 7, except that the molar ratio of barium ions to iron ions is 1:12.

[0066] Example 9

[0067] The same as Example 7, except that the molar ratio of barium ions to iron ions is 1:14.

[0068] Example 10

[0069] Weigh FeC13·6H2O and BaCl2·2H2O, so that the molar ratio of barium ions to iron ions is 1:10, dissolve FeC13·6H2O and BaCl2·2H2O in 400mL of deionized water to prepare a solution, and dissolve citric acid in the solution, wherein the molar ratio of citric acid to the total content of metal ions is 3:1. Then adjust the pH of the solution to 8 with ammonia water, stir the solution quickly to mix thoroughly and react. After the reaction is completed, continue to heat and evaporate the product solution at 90°C for 36h to dehydrate it to obtain a sol. Put the sol into a muffle furnace, heat it to 480°C at a rate of 5°C / min in an argon atmosphere, and preheat it for 2h; then heat it to 1400°C at a rate of 10°C / min for calcination, and obtain a magnetoplumbite-type barium ferrite after calcination for 3h.

[0070] Embodiment 11

[0071] The same as Example 10, except that the molar ratio of barium ions to iron ions is 1:12.

[0072] Example 12

[0073] The same as Example 10, except that the molar ratio of barium ions to iron ions is 1:14.

[0074] Figure 1The phase structure diagrams of the magnetoplumbite type barium ferrite obtained at different molar ratios of barium and iron at different calcination temperatures, wherein (a) corresponds to Examples 1 to 3, (b) corresponds to Examples 4 to 6, (c) corresponds to Examples 7 to 9, and (d) corresponds to Examples 10 to 12. Figure 1 It can be seen that when the calcination temperature is 800°C, no obvious BaFe 12 O 19 The characteristic peak of Ba 2+ with Fe 3+ The molar ratio of raw materials is 1:10. The 2θ=28.2°, 28.4°, 32.7°, 33.2°, 34.6°, 37.8°, 39.2°, 39.8°, 42.8°, 43.6°, 44.1°, 54.9°, 55.5°, 56.1°, 58.1°, and 59.0° diffraction peaks correspond to the (402), (212), (610), (020), (701), (800), (612), (503), (004), (802), (422), (614), (1012), (224), (1200), and (630) crystal planes of BaFe2O4, respectively. The data of this group of powders are consistent with those of JCPDS25-1191 through comparison and analysis. The main component of this group of powders is BaFe2O4. In addition, the spectrum also shows the characteristic peak of α-Fe2O3, and with the increase of Fe in the raw material, the 3+ With the increase of molar ratio, the characteristic peak intensity increases continuously.

[0075] When the calcination temperature is 1000℃, BaFe 12 O 19 Characteristic peaks. Figure 1 It can be seen from (b) that obvious diffraction peaks appear at 30.3°, 32.2°, 34.1°, 35.1°, 37.1°, 40.2°, 42.4°, 56.2°, 56.6°, and 63.1°, which correspond to the (110), (107), (114), (200), (203), (2011), (205), (206), (304), and (220) crystal planes of the barium ferrite with a magnetoplumbite structure, respectively. The data analyzed by JCPDS comparison are consistent with (JCPDS27-1029). In addition, the characteristic peaks of α-Fe2O3 and BaFe2O4 still exist in the XRD patterns of the embodiments with different raw material ratios, and the characteristic peaks of α-Fe2O3 and BaFe2O4 are also found in the raw material BaFe2O4. 2+ with Fe 3+ In the embodiment with a molar ratio of 1:14, the characteristic peak of α-Fe2O3 is obvious, while in the embodiment with a molar ratio of 1:10, the characteristic peak of BaFe2O4 is more obvious.

[0076] When the calcination temperature is increased to 1200°C, the BaFe 12 O 19 The characteristic peaks are already very obvious. Raw material Ba 2+ with Fe 3+ The main component of the embodiment with a molar ratio of 1:12 is BaFe 12 O 19 The embodiment with a molar ratio of 1:10 still has the characteristic peak of BaFe2O4, and the embodiment with a molar ratio of 1:14 still has the characteristic peak of α-Fe2O3.

[0077] When the calcination temperature is increased to 1400°C, the BaFe 12 O 19 The characteristic peaks continue to strengthen and the impurity peaks continue to weaken, but the BaFe2O4 and α-Fe2O3 phases still exist.

[0078] Figure 2 The XRD patterns of the magnetoplumbite type barium ferrites obtained in Examples 5, 8 and 11 are as follows: Figure 2 It can be seen that with the increase of calcination temperature, BaFe 12 O 19 The characteristic peaks are continuously strengthened.

[0079] From the above analysis, it can be seen that when calcined at a temperature range of 1000-1200°C, BaFe begins to appear in the calcined powder. 12 O 19 phase. And at the same calcination temperature, the embodiment with a raw material molar ratio of 1:12 has the best calcination effect, BaFe 12 O 19 The relative content is higher and the characteristic peaks are more obvious, which is consistent with its chemical formula. 12 O 19 When calcined at a temperature range of 1200-1400°C, the calcined powder is almost completely converted into BaFe 12 O 19 In the examples with calcination temperatures of 1200°C and 1400°C and a molar ratio of 1:12, BaFe 12 O 19 Single phase. And the rise in temperature promotes the growth of material grains, the crystal form tends to be complete, the degree of crystallization is higher, and the corresponding diffraction peak intensity continues to increase.

[0080] In order to further analyze the microstructure of the calcined powder, the powder was further characterized using scanning electron microscopy. Figure 3The SEM images of the magnetoplumbite type barium ferrite obtained at different calcination temperatures when the molar ratio of barium ions to iron ions is 1:12. Among them, (a) and (b) are products calcined at 800℃, and the product particles are long rods with a long diameter distribution of about 1μm, a short diameter of about 60nm, and an aspect ratio of 33.3; (c) and (d) are products calcined at 1000℃, the product particles become smaller, and the aspect ratio also decreases at the same time, attached to the hexagonal block particles; the average long diameter of the rod-like particles is about 100nm, and the hexagonal block size is mainly distributed in 200-300nm. (e) and (f) are products calcined at 1200℃, (g) and (h) are products calcined at 1400℃. From (e) to (h), it can be seen that as the temperature continues to rise, the rod-like particles gradually disappear, and the powder is hexagonal block. During the calcination process, in order to reduce the surface energy of the particles, the barium ferrite calcined powder often agglomerates with each other to form hexagonal blocks. The rod-like powder formed by low temperature calcination is mainly related to α-Fe2O3. The existence of α-Fe2O3 phase has an important influence on the 12 O 19 The material morphology has a huge impact. When some second phase structures are attached around the hexagonal particles, the hexagonal grains will be distorted, resulting in a large difference in the morphology of the products calcined at 1000℃ and those calcined at 1200℃ and 1400℃. As the temperature rises, the powder particle size continues to increase and the dispersibility gradually improves. When calcined at 1200℃, the particle size of the powder is mainly distributed in the range of 300-400nm; when the calcination temperature is 1400℃, the powder particle size is mainly distributed in the range of 400-500nm.

[0081] Figure 4 The following are TEM images of the magnetoplumbite-type barium ferrite obtained at different calcination temperatures when the molar ratio of barium ions to iron ions is 1:12. Among them, (a) is the microscopic morphology of the product calcined at 800°C at different magnifications. It can be found that the rod ends are basically α-Fe2O3 grains, and clear diffraction spots (012) and (110) are obtained. The lower right figure is the result of filtering processing in the red frame area. It can be found that the grains grow along the (110) crystal plane, and the interplanar spacing is 0.251nm. (b) is the microscopic morphology of the product calcined at 1000°C at different magnifications. Its diffraction pattern is a standard diffraction ring of a polycrystalline material, and different grains are mainly separated by large-angle grain boundaries (>10°). (c) is the microscopic morphology of the product calcined at 1400°C at different magnifications. BaFe 12 O 19 (107) and (110) crystal planes. In the red frame area, the grains grow along the (107) crystal planes, and the interplanar spacing is 0.278nm.

[0082] In order to further understand the composition and element distribution of the magnetoplumbite barium ferrite powder prepared by the calcination process, multi-point EDS detection was performed on each type of powder particles and the average value was taken. The atomic percentage of each element in the powder is shown in Table 1 (the molar ratio of Ba to Fe is 1:12).

[0083] Table 1 Element distribution of magnetoplumbite type barium ferrite

[0084] Barium Ferrite Ba Fe O Rod-shaped particles (800℃) 1.06 39.97 58.97 Hexagonal block particles (1000℃) 7.65 35.74 56.61 Rod-shaped particles (1000℃) 0.26 39.90 59.84 Hexagonal block particles (1200℃) 3.12 37.44 59.44 Hexagonal block particles (1400℃) 2.34 26.04 71.62

[0085] As shown in Table 1, as the temperature rises, the atomic percentage ratio of Ba to Fe in hexagonal block particles decreases continuously. At a temperature of 1200-1400°C, the atomic percentage of the component elements in hexagonal block particles is close to the design value of barium ferrite. The main components of rod-shaped particles are Fe and O, and the content of Ba is relatively low. This is consistent with the fact that α-Fe2O3 is relatively 12 O 19 The inference that material morphology has a huge impact is consistent.

[0086] X-ray photoelectron spectroscopy is used to further analyze the elemental composition and chemical state of the powder surface. Figure 5 The XPS spectrum of the magnetoplumbite-type barium ferrite obtained in Example 8, wherein (a) is the XPS general spectrum of the calcined product, and (b), (c), and (d) are the detailed spectra of the O, Ba, and Fe elements in the calcined product, respectively. Figure 7 It can be seen that there are two sets of characteristic peaks at 780.1eV and 795.0eV, corresponding to the 3d 5 / 2 and 3d 3 / 2 electron spin orbits of divalent barium ions; two sets of characteristic peaks at 711.7eV and 724.9eV, corresponding to the 3d 3 / 2 and 3d 1 / 2 electron spin orbits of trivalent iron ions, 730.9eV and 715.9eV are iron species satellite peaks; a characteristic peak also appears at 530.4eV, corresponding to the 1s electron spin orbit of divalent oxygen ions. Combined with the previous XRD, SEM, EDS, and XPS analysis results, it can be known that the main component of the calcined product is magnetoplumbite-type barium ferrite.

[0087] The wave absorption performance of ferrite is closely related to its magnetic properties. Ferrite and other magnetic materials will produce hysteresis during the magnetization process, causing energy loss, that is, the magnetic flux density lags behind the change of magnetic field intensity, and the two are in a hysteresis loop relationship. In a single cycle, the loss energy generated by the hysteresis phenomenon per unit volume is related to the area of ​​the hysteresis loop. And it is an important criterion for judging the wave absorption performance of materials, which is higher than the saturation magnetization intensity and coercive force. Figure 6 It is raw material 2+ with Fe 3+ Magnetic hysteresis loops of the example with a molar ratio of 1:12 at different calcination temperatures.

[0088] According to the test curve, the corresponding magnetic parameter Ms can be obtained by fitting the material magnetization intensity and magnetic field to satisfy the near saturation law (LAS). The fitting curve is as follows: Figure X (b) is shown in the following formula 1:

[0089]

[0090] In formula 1, A is the electromagnetic field parameter, χ P is a strong magnetic field environment, and B is a parameter that characterizes the magnetocrystalline anisotropy field. Under high magnetic field conditions, M and 1 / H 2 The coercive force can be obtained through the magnetocrystalline anisotropy field parameter B, the effective magnetocrystalline anisotropy constant Keff and other parameters.

[0091]

[0092]

[0093] In formula 3, N is the demagnetization factor. According to the calculation results, as the calcination temperature increases from 800℃ to 1200℃, the specific saturation magnetization increases from 36.57emu / g to 117.08emu / g, and at the same time the coercive force increases from 1154.86Oe to 2442.19Oe. However, as the calcination temperature increases from 1200℃ to 1400℃, the specific saturation strength and coercive force both decrease to a certain extent, decreasing to 97.89emu / g and 2093.14Oe respectively.

[0094] Figure 7 (a), (b), (c) are the curves of the real part, imaginary part and electric loss angle of the dielectric constant of barium ferrite calcined at 1000℃, 1200℃ and 1400℃ in the frequency band of 26.5~40GHz. Figure 7 It can be seen that the real part of the dielectric constant of the products calcined at 1000℃, 1200℃ and 1400℃ fluctuates slightly and decreases with the increase of frequency. The imaginary part of the dielectric constant of the three groups of products fluctuates slightly and increases with the increase of frequency. The trend of the change of the electric loss angle with frequency is consistent with the imaginary part of the dielectric constant. When only the dielectric loss is considered, the dipole change lags behind the electric field change, and energy loss is generated in the repeated turning process, affecting the value of the dielectric parameter.

[0095] Polarization relaxation under an alternating electric field of frequency ω can be expressed as follows:

[0096]

[0097] α(t)=α0e -t / τ ...Formula 5;

[0098] Where ε ∞is the material dielectric constant of the infinite frequency alternating electromagnetic field, α(t) is the attenuation factor, and τ is the relaxation time. The dielectric constant is further derived as follows:

[0099]

[0100] By introducing the static dielectric constant ε s , we can get the famous Debye equation, whose specific expression is as follows:

[0101]

[0102] T is temperature, σ(T) is the temperature-related conductivity, and ω is the angular frequency. According to the free electron theory, the conductivity loss mechanism is introduced, and its expression can be expressed as:

[0103]

[0104] Represent the dielectric loss and resistance loss respectively. From the above, we can know that It is negatively correlated with the frequency, and in the experimental data, the imaginary part of the dielectric constant increases with a small fluctuation as the frequency increases, which shows that dielectric loss occupies an important position in electrical loss. By comparing the dielectric performance parameters of the products calcined at different temperatures, it is found that the average values ​​of the real part, imaginary part and magnetic loss angle of the products calcined at 1000°C are the highest, followed by the three groups of parameters of the products calcined at 1200°C, and the three groups of parameters of the products calcined at 1400°C are the lowest. This is mainly because when the calcination temperature is low, the powder grains are smaller, the microstructure is looser, and there are more void defects. In addition, the powder calcined at low temperature still contains a certain amount of impurities, resulting in more interfaces, which is conducive to improving the dielectric loss capacity.

[0105] According to the above derived Debye formula, the ωτ term in is eliminated, and the Cole-Cole curve equation (Equation 11) consisting of the real part and the imaginary part of the complex dielectric constant is obtained:

[0106]

[0107] It can be seen from formula 11 that in the plane with ε', ε" as coordinates, there exists a Cole-Cole circle with center and radius, also known as the Debye circle. In the physical sense, each Cole-Cole circle in the curve represents a Debye relaxation process, and its number and size can respectively characterize the dielectric electrical loss mechanism and capacity. Figure 8The Cole-Cole plots of barium ferrite materials calcined at different temperatures are shown. It can be observed that the three groups of barium ferrite material samples have similar Cole-Cole curves with increasing frequency, with multiple Debye semicircles, which indicates that there are multiple relaxation mechanisms in barium ferrite materials and the dielectric loss mechanisms of the three groups of materials are similar. And as the calcination temperature decreases, its Cole-Cole curve is more complete, the radius is larger, and the dielectric properties are better.

[0108] Fig. 9 (a), (b), and (c) are the curves of the real part, imaginary part, and magnetic loss angle of the three groups of barium ferrite powders calcined at different temperatures in the 26.5-40 GHz frequency band. Fig. 9 It can be seen that the real part of the permeability of the powders calcined at 1200℃ and 1400℃ first decreases with the increase of frequency in the low frequency band, and then fluctuates with the increase of frequency. The 1000℃ powder decreases slightly in the low frequency band and fluctuates in the high frequency band; the imaginary part of the permeability of the three groups of powders has a similar change trend, with a small fluctuation in the low frequency band and a significant increase in the range of 36-40GHz, and the change trend of the magnetic loss angle of the three groups of powders is similar to the change trend of the imaginary part of the permeability.

[0109] By comparing the dynamic magnetic parameters of powders calcined at different temperatures, it was found that the average values ​​of the real part, imaginary part of the magnetic permeability and the magnetic loss angle of the powder calcined at 1200°C were the highest, the three groups of parameters of the powder calcined at 1400°C were second, and the three groups of parameters of the powder calcined at 1000°C were the lowest.

[0110] Under radar wave conditions, the magnetic permeability is related to the static magnetic parameters, and its expression is as follows:

[0111]

[0112] Among them, δ is the phase angle between the magnetic induction intensity and the magnetic field intensity, which is related to the coercive force. From the above formula, it can be seen that the magnetic permeability is positively correlated with the magnetic induction intensity, and the experimental results of dynamic magnetic properties and static magnetic parameters are consistent with the theory. In short, compared with the powder calcined at 1000°C, the powder calcined at 1200°C has advantages in terms of densification and purity of barium ferrite, while compared with the powder calcined at 1400°C, it has advantages in terms of uniformity and magnetic domain state, so it has the best magnetic properties.

[0113] From the above content, it can be seen that magnetic loss mainly comes from hysteresis loss, eddy current loss and residual loss. The hysteresis loss power can be closely derived from the hysteresis loop, and its expression is:

[0114]

[0115] In equation 14, μ0 is the initial magnetic permeability, η is the Rayleigh constant, and Hm is the peak value of the applied magnetic field. It can be seen that the greater the frequency, the greater the Rayleigh constant, and the greater the amplitude of the applied magnetic field, the more conducive to the improvement of hysteresis loss. And compared with the above three parameters, the amplitude of the applied magnetic field has a greater impact on hysteresis loss. However, for the weak electromagnetic field of radar waves, the contribution of hysteresis loss is small and is not on the same order of magnitude as other magnetic losses.

[0116] According to the absorption theory of absorbing materials, in the radar band, the remaining loss is mainly natural resonance and exchange resonance. In particular, natural resonance is particularly important in the magnetic loss of ferrite materials. From formula 15, it can be seen that the natural resonance frequency is related to anisotropy, and the anisotropy field can be estimated by the LAS law. In the hexagonal crystal system of magnetoplumbite type barium ferrite, the expressions of anisotropy field and magnetocrystalline anisotropy field parameter B are as follows:

[0117]

[0118] In addition, the magnetic gyrometry ratio γ in equation 15 is related to the Lande factor g, which is expressed as follows:

[0119]

[0120] As we all know, the Lande factor of trivalent iron ions is 2.0. Combined with the above static magnetic properties analysis, it can be seen that the natural resonance frequencies of the three groups of calcined barium ferrite are approximately 39.17, 44.68, and 41.67 GHz, respectively. Therefore, the magnetic loss angle of barium ferrite powder is significantly improved in the high frequency band (34-40 GHz).

[0121] Exchange resonance is another important form of residual loss in the process of radar wave absorption of materials. It is mainly generated between nanoscale magnetic particles and is an important supplement to the natural resonance of materials. For standard spherical particles, the exchange resonance frequency can be expressed as:

[0122]

[0123] In formula 17, μ kn is the spherical Bessel eigenvalue, C is the exchange constant, and R is the radius of the spherical particle. It can be seen from the formula that for smaller nano-M-type barium ferrite materials, exchange resonance mainly occurs in the high frequency band, which also helps to improve the magnetic loss angle in the high frequency band (34-40GHz). And Landau-Lifschitz et al. further studied the internal mechanism of magnetic resonance, derived the internal relationship between magnetic permeability and resonance frequency, and obtained the Lorentzian equation as follows:

[0124]

[0125] In formula (18), M≈1, K is the static magnetic susceptibility, and f Ris the resonant frequency, and λ is the damping coefficient. From the above formula, the relationship between the real part of magnetic permeability and frequency can be derived as follows:

[0126]

[0127] Therefore, the real part of the magnetic permeability decreases rapidly near the resonant frequency, and the imaginary part increases significantly at the resonant frequency. This phenomenon is consistent with the test curve, and is particularly evident in the high frequency band.

[0128] Eddy current loss is another important magnetic loss mechanism, and its severity C0 is mainly related to the conductivity σ and the material thickness d:

[0129]

[0130] Since the right-hand side of the formula is a constant, if eddy current losses occur, the left-hand side of the formula should also be a constant. Fig.10 is the curve of C0 changing with frequency. Fig.10 It can be seen that the C0 of the three groups of barium ferrite powders calcined at different temperatures is basically constant in the frequency range of 32 to 40 GHz, so the eddy current losses of the three groups of powders mainly occur in the above frequency band.

[0131] The attenuation coefficient and characteristic impedance of barium ferrite are as follows Fig.11 As shown. It can be seen that the intrinsic impedance of each group of powders fluctuates with the increase of frequency. And the impedance matching of the powders calcined at 1200℃ and 1400℃ is better. Impedance matching is mainly related to the closeness of the ratio of the real and imaginary parts of the magnetic permeability to the real and imaginary parts of the dielectric constant. Compared with the powders calcined at 1000℃, the above two groups have higher magnetic permeabilities, smaller dielectric constants, and better impedance matching performance. In terms of attenuation capacity, the attenuation coefficient of each group of powders increases continuously with the increase of frequency. And the attenuation coefficient of the powder calcined at 1200℃ is the best overall. It has better magnetic loss capacity than the powder calcined at 1000℃, and has better electrical loss and magnetic loss capacity than the powder calcined at 1400℃.

[0132] Fig.12 (a) in the figure is the reflection loss curve of different barium ferrites with a thickness of 2.5mm absorbing medium versus frequency. As shown in Figure (a), the powder sintered at 1200℃ has the strongest reflection loss, which is -34.86dB, which is consistent with the attenuation coefficient and characteristic impedance characterization. And the reflection loss peak frequency is the highest, about 39.33GHz. This is mainly related to the higher natural resonance frequency caused by its higher magnetocrystalline anisotropy. Fig.12(b) is the reflection loss curve of barium ferrite powder sintered at 1200°C at different thicknesses. As shown in Figure (b), as the thickness decreases, the frequency of the reflection loss peak increases, which is consistent with the interference destructive theory, and when the thickness is 2.3mm, there is no peak at 40GHz.

[0133] Fig.12 (a) in the figure is the reflection loss curve of different barium ferrites with a thickness of 2.5mm absorbing medium versus frequency. As shown in Figure (a), the powder sintered at 1200℃ has the strongest reflection loss, which is -34.86dB, which is consistent with the attenuation coefficient and characteristic impedance characterization. And the reflection loss peak frequency is the highest, about 39.33GHz. This is mainly related to the higher natural resonance frequency caused by its higher magnetocrystalline anisotropy. Fig.12 (b) is the reflection loss curve of barium ferrite powder sintered at 1200°C at different thicknesses. As shown in Figure (b), as the thickness decreases, the frequency of the reflection loss peak increases, which is consistent with the interference destructive theory, and when the thickness is 2.3mm, there is no peak at 40GHz.

[0134] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing magnetoplumbite type barium ferrite, characterized in that: The following steps are involved: The iron salt, the barium salt, the complexing agent and water are mixed and reacted to obtain a product solution, and the product solution is subjected to heating evaporation, preheating treatment and calcination treatment in sequence to obtain a magnetoplumbite type barium ferrite; The calcination temperature is 800-1400° C., and the calcination time is 3-10 hours.

2. The preparation method according to claim 1, characterized in that: The molar ratio of barium ions in the barium salt to iron ions in the iron salt is 1:10-14.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the complexing agent to the total content of metal ions is 1 to 5:

1.

4. The preparation method according to any one of claims 1 to 3, characterized in that: Before the reaction, a pH regulator is added to the reaction system to adjust the pH of the reaction system to 6-9; the pH regulator includes ammonia water.

5. The preparation method according to claim 4, characterized in that: The reaction temperature is 0-80°C, and the reaction time is 0.5-2h.

6. The preparation method according to claim 1, 2, 3 or 5, characterized in that: The iron salt includes iron chloride or iron nitrate; the barium salt includes barium chloride or barium nitrate.

7. The preparation method according to claim 6, characterized in that: The complexing agent includes citric acid.

8. The preparation method according to claim 1, 2, 3, 5 or 7, characterized in that: The heating evaporation temperature is 80-100° C., and the heating evaporation time is 30-40 hours.

9. The preparation method according to claim 8, characterized in that: The temperature of the preheating treatment is 400-500° C., and the time of the preheating treatment is 1-3 hours.

10. Magnetoplumbite type barium ferrite prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of M-type barium ferrite magnetic powder

    CN102674825A

  • Barium ferrite preparation method

    CN106495230A

  • Preparation method and application of porous magnetoplumbite barium ferrite

    CN107684893A

  • Process for synthesizing barium ferrite micro powder by self combustion method