A method for preparing layered barium carbonate
By using urea, melamine, and g-C3N4 as additives to control the morphology of barium carbonate, the problems of high preparation cost, long preparation time, and poor dispersibility in the existing technology were solved, and high-purity layered barium carbonate was successfully prepared, improving the material performance and reaction efficiency.
Patent Information
- Application Number
- CN202611458471.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing barium carbonate suffer from problems such as high cost, demanding conditions, long processing time, difficulty in large-scale application, and poor particle dispersibility. In particular, the preparation of layered barium carbonate is relatively rare.
Layered barium carbonate was prepared by using urea, melamine, and graphite-like carbon nitride (g-C3N4) as chemical additives, controlling the molar ratio of the additives to barium salts and carbonates, forming a suspension, and adding it dropwise under magnetic stirring. The suspension was then aged, filtered, washed, dried, and calcined.
This method enables the low-cost, short-time, and efficient preparation of layered barium carbonate with a purity of up to 99.6%. It features excellent morphology control and a large specific surface area, thereby improving material properties and chemical reaction efficiency.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials preparation technology and relates to a method for preparing layered barium carbonate. Background Technology
[0002] Barium carbonate is an important inorganic chemical raw material and one of the most important barium salt products. Barium carbonate products are widely used in barium salts, optical glass, pigments, ceramics, rubber, electron tubes, barium ferrites, and as a precursor material for the preparation of superconductors and ceramic materials. Furthermore, barium carbonate isotopes have broad application prospects as tracers in the biomedical field. my country is a major producer and consumer of barium carbonate. In recent years, with the rapid development of other industries, the application fields of barium carbonate have been expanding, and the requirements for its quality and morphology have become increasingly stringent.
[0003] Currently, the main methods for preparing barium carbonate include microemulsion, hydrothermal, template synthesis, ultrasonic chemistry, and hypergravity. However, each method has its own drawbacks: for example, the microemulsion method requires high-cost raw materials and has harsh reaction conditions; the hydrothermal method requires high-temperature and high-pressure equipment and is time-consuming; the template synthesis method has difficulty in solving the dispersion of nanoparticles; the ultrasonic chemistry method has high energy consumption and is difficult to apply on a large scale; and the hypergravity method requires special chemical reaction equipment.
[0004] Studies have shown that in the synthesis of barium carbonate crystals, adding a certain amount of chemical additives to the reaction solution to occupy active sites on the crystal surface can control the growth of barium carbonate crystals and change their morphology. Commonly used chemical additives include fatty acids, oxycarboxylic acids, aromatic carboxylic acids, aldehydes, aromatic sulfonic acids, organic polymers containing -CN groups, and water-soluble metal salts (such as Na+). + Zn 2+ Mg 2+ Fe 3+ Barium carbonate particles synthesized using the above additives can take various shapes, including linear, columnar, spherical, flake-like, dumbbell-shaped, flocculent, and oval, with particle sizes ranging from a few micrometers to tens of micrometers. However, layered barium carbonate is rarely seen. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing layered barium carbonate.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A method for preparing layered barium carbonate, characterized by comprising the following steps: (1) Dissolve barium salts such as barium chloride, barium nitrate, and barium acetate in distilled water to form a solution A with a mass concentration of 0.1-42.9%; (2) Dissolve the carbonates such as ammonium carbonate, ammonium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate in distilled water to form a solution B with a mass concentration of 0.1-55.8%; (3) Add at least one of urea, melamine, and graphitic carbon nitride (g-C3N4) solid to solution A, control the molar ratio of the additive to the barium salt to be greater than 1:10, sonicate for 5~30 min to form suspension C; (4) Add at least one of urea, melamine, and graphite-like carbon nitride (g-C3N4) solid to solution B, control the molar ratio of the additive to carbonate to be greater than 1:10, sonicate for 5~30 min to form suspension D; (5) Under magnetic stirring conditions, solution A is added dropwise to suspension D, or solution B is added dropwise to suspension C, or suspension C is added dropwise to suspension D; this dropwise addition ensures that the additive is encapsulated during the precipitation process, the additive is more evenly distributed in the precipitate, and the morphology of barium carbonate is better controlled. (6) After the addition is finished, continue stirring (10~50 min), age for 1~6 h, filter and wash the obtained product with anhydrous ethanol and deionized water in sequence, then dry the product (dry at 60~120 ℃ for 10~24 h), collect the powder and grind it to obtain a white solid mixture; (7) The white mixed solid was placed in a tube furnace and calcined at 700~1000℃ for 2-12 hours. After grinding, a white layered barium carbonate product was obtained.
[0007] Furthermore, the white layered barium carbonate product is relatively flat on a two-dimensional plane, with a transverse diameter of 1-150 μm and a diameter-to-thickness ratio of 10-1500. Its appearance has many stacked or stepped heights, which can provide a large specific surface area, effective contact area and active sites, thereby significantly improving material performance and chemical reaction efficiency.
[0008] Furthermore, the reaction temperature of ammonium carbonate in step (5) is 5-60℃.
[0009] Furthermore, the optimal reaction temperature for ammonium carbonate in step (5) is 20-40℃.
[0010] Furthermore, the reaction temperature of ammonium bicarbonate in step (5) is 5-50℃.
[0011] Furthermore, the optimal reaction temperature for ammonium bicarbonate in step (5) is 20-35℃.
[0012] Furthermore, step (7) adopts the following heating program: heating to 500-600℃ at a rate of 2-20℃ / min, holding for 2-4 hours, and then continuing to heat to 700-1000℃.
[0013] Furthermore, the method described in this invention can also be used to prepare carbonates such as layered strontium carbonate and layered lithium carbonate.
[0014] Melamine and urea react at 500-600℃ for 2-4 hours to form g-C3N4, which is a typical layered material. This ensures that barium carbonate with different morphologies obtained by liquid-phase precipitation is initially uniformly dispersed on the surface of layered g-C3N4. As the temperature increases, g-C3N4 gradually decomposes, mass transfer of barium carbonate particles intensifies, grain boundary movement accelerates, grains grow and deform, and pores further shrink, promoting the formation of layered barium carbonate. Furthermore, when the temperature exceeds 700℃, g-C3N4 completely decomposes into gas, leaving almost no solid residue, thus ensuring the layered morphology and high purity of the barium carbonate product.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The preparation method of this invention is low in cost, short in time, low in energy consumption, green and efficient, with simple reaction conditions and no need for special equipment; 2. The product prepared by this invention has precise control over particle morphology, exhibits a layered structure, and has a purity of up to 99.6%. Attached Figure Description
[0016] Figure 1 To obtain the XRD pattern of the barium carbonate product; Figure 2 SEM images of barium carbonate obtained before (a) and after (b) the addition of g-C3N4 (barium chloride dihydrate added to ammonium bicarbonate). Figure 3 SEM images of barium carbonate obtained before (a) and after (b) the addition of g-C3N4 (ammonium bicarbonate added to barium chloride dihydrate). Figure 4 SEM images of barium carbonate before (a) and after (b) the addition of urea and graphitic carbon nitride solid (ammonium carbonate added to barium chloride dihydrate). Figure 5 SEM images of barium carbonate obtained before (a) and after (b) the addition of melamine (barium chloride dihydrate was added to ammonium carbonate). Detailed Implementation
[0017] A method for preparing layered barium carbonate, the specific implementation steps of which are as follows: Example 1
[0018] Dissolve 1.2213 g of barium chloride dihydrate in 50.00 mL of distilled water to form solution A; Dissolve 0.3953 g of ammonium bicarbonate in 50.00 mL of distilled water to form solution B; then add 0.0460 g of graphitic carbon nitride (g-C3N4) solid to solution B and sonicate for 20 min to form suspension D; At 25°C, solution A was added dropwise to suspension D under magnetic stirring. After the addition was completed, stirring was continued for 15 min. The mixture was aged for 2 h, filtered, and the product was washed with anhydrous ethanol and deionized water. The product was then dried (drying at 100°C for 11 h), the powder was collected and ground to obtain a white solid mixture. The white mixture was placed in a tube furnace and heated to 530°C at a rate of 12°C / min. After holding at this temperature for 2.5 hours, the temperature was further increased to 850°C and calcined for 10 hours. The mixture was then ground to obtain a white orthorhombic barium carbonate product (e.g., ...). Figure 1 As shown in the figure, the morphology of barium carbonate before and after adding g-C3N4 is compared as follows. Figure 2 As shown.
[0019] The white orthorhombic barium carbonate product has a purity of 99.5%. It is relatively flat on a two-dimensional plane, with a transverse diameter of 48 μm and an aspect ratio of up to 480. Its morphology is a layered structure with many stacks or steps, which can provide a large specific surface area, effective contact area and active sites, thereby significantly improving material properties and chemical reaction efficiency. Example 2
[0020] 1.2213 g of barium chloride dihydrate was dissolved in 50.00 mL of distilled water to form solution A; then 0.0691 g of graphitic carbon nitride (g-C3N4) solid was added to solution A and sonicated for 25 min to form suspension C. Dissolve 0.3953g of ammonium bicarbonate in 50.00mL of distilled water to form solution B; At 30°C, solution B was added dropwise to suspension C under magnetic stirring. After the addition was completed, stirring was continued for 30 min. The mixture was aged for 4 h, filtered, and the product was washed with anhydrous ethanol and deionized water. The product was then dried (drying at 80°C for 18 h), the powder was collected and ground to obtain a white solid mixture. The white mixture was placed in a tube furnace and heated to 550°C at a rate of 16°C / min. After holding at this temperature for 3.5 hours, the temperature was further increased to 950°C and calcined for 4 hours. The resulting product was then ground to obtain a white orthorhombic barium carbonate product. The morphology of the barium carbonate obtained before and after adding g-C3N4 is compared as follows: Figure 3 As shown.
[0021] The white orthorhombic barium carbonate product has a purity of 99.5%. It is relatively flat on a two-dimensional plane, with a lateral diameter of 70 μm and an aspect ratio of up to 700. Its morphology is a layered structure with many stacks or steps, which can provide a large specific surface area, effective contact area and active sites, thereby significantly improving material performance and chemical reaction efficiency. Example 3
[0022] 2.4426 g of barium chloride dihydrate was dissolved in 50.00 mL of distilled water to form solution A; then 0.6006 g of urea and 0.9207 g of graphite-like carbon nitride solid were added to solution A and sonicated for 15 min to form suspension C. Dissolve 0.9609 g of ammonium carbonate in 50.00 mL of distilled water to form solution B; (3) At 35°C, solution B was added dropwise to suspension C under magnetic stirring. After the addition was completed, stirring was continued for 20 min. After aging for 5 h, the product was filtered and washed with anhydrous ethanol and deionized water in sequence. The product was then dried (dried at 90°C for 12 h), the powder was collected and ground to obtain a white solid mixture. (4) The white mixture was placed in a tube furnace and heated to 580°C at a rate of 3°C / min. After holding at this temperature for 3 hours, the temperature was further increased to 900°C and calcined for 5 hours. After grinding, a white orthorhombic barium carbonate product was obtained. The morphology of the barium carbonate obtained before and after the addition of melamine was compared as follows: Figure 4 As shown.
[0023] The white orthorhombic barium carbonate product has a purity of 99.6%. It is relatively flat on a two-dimensional plane, with a lateral diameter of 50 μm and an aspect ratio of up to 500. Its morphology is a layered structure with many stacks or steps, which can provide a large specific surface area, effective contact area and active sites, thereby significantly improving material properties and chemical reaction efficiency. Example 4
[0024] Dissolve 2.4426 g of barium chloride dihydrate in 50.00 mL of distilled water to form solution A; Dissolve 0.9609 g of ammonium carbonate in 50.00 mL of distilled water to form solution B; then add 1.2612 g of melamine solid to solution B and sonicate for 10 min to form suspension D; At 25°C, solution A was added dropwise to suspension D with magnetic stirring. After the addition was completed, stirring was continued for 10 min. The mixture was aged for 3 h, filtered, and the product was washed with anhydrous ethanol and deionized water in sequence. The product was then dried (drying at 60°C for 24 h), the powder was collected and ground to obtain a white solid mixture. The white mixture was placed in a tube furnace and heated to 520°C at a rate of 10°C / min. After holding at this temperature for 4 hours, the temperature was further increased to 800°C and calcined for 6 hours. The resulting product was then ground to obtain a white barium carbonate product, which exhibited an orthorhombic crystalline phase. A comparison of the morphology of the barium carbonate obtained before and after the addition of melamine is shown below. Figure 5 As shown.
[0025] The white barium carbonate product has a purity of 99.4%, is relatively flat on a two-dimensional plane, has a transverse diameter of 78 μm, and an aspect ratio of up to 780. Its morphology is a layered structure with many stacks or steps, which can provide a large specific surface area, effective contact area and active sites, thereby significantly improving material performance and chemical reaction efficiency.
Claims
1. A method for preparing layered barium carbonate, characterized in that... Includes the following steps: (1) Dissolve barium chloride, barium nitrate or barium acetate in distilled water to form solution A with a mass concentration of 0.1-42.9%; (2) Dissolve ammonium carbonate, ammonium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate or potassium bicarbonate in distilled water to form a solution B with a mass concentration of 0.1-55.8%; (3) Add at least one of urea, melamine, and graphite-like carbon nitride solid to solution A, control the molar ratio of the additive to barium salt to be greater than 1:10, sonicate for 5~30 min to form suspension C; (4) Add at least one of urea, melamine, and graphite-like carbon nitride solid to solution B, control the molar ratio of the additive to carbonate to be greater than 1:10, sonicate for 5~30 min to form suspension D; (5) Under magnetic stirring conditions, add solution A dropwise to suspension D, or add solution B dropwise to suspension C, or add suspension C dropwise to suspension D; (6) After the addition is finished, continue stirring and age for 1-6 hours. Filter and wash the product with anhydrous ethanol and deionized water in sequence. Then dry the product, collect the powder and grind it to obtain a white solid mixture. (7) The white mixed solid was placed in a tube furnace and calcined at 700~1000℃ for 2-12 hours. After grinding, a white layered barium carbonate product was obtained.
2. The method for preparing layered barium carbonate according to claim 1, characterized in that: The reaction temperature of ammonium carbonate in step (5) is 5-60℃.
3. The method for preparing layered barium carbonate according to claim 1, characterized in that: The reaction temperature of ammonium carbonate in step (5) is 20-40℃.
4. The method for preparing layered barium carbonate according to claim 1, characterized in that: The reaction temperature of ammonium bicarbonate in step (5) is 5-50℃.
5. The method for preparing layered barium carbonate according to claim 1, characterized in that: The reaction temperature of ammonium bicarbonate in step (5) is 20-35℃.
6. The method for preparing layered barium carbonate according to claim 1, characterized in that: The drying temperature in step (6) is 60~120℃ and the drying time is 10~24 h.
7. The method for preparing layered barium carbonate according to claim 1, characterized in that: The (7) process uses the following heating procedure: heating to 500-600℃ at a rate of 2-20℃ / min, holding for 2-4 hours, then continuing to heat to 700-1000℃ and calcining for 2-12 hours.
8. A method for preparing layered barium carbonate according to any one of claims 1 to 7, characterized in that: The white layered barium carbonate product is relatively flat on a two-dimensional plane, with a transverse diameter of 1-150 μm and a diameter-to-thickness ratio of 10-1500. Its appearance has many layers or steps, which can provide a large specific surface area, effective contact area and active sites, and can significantly improve material performance and chemical reaction efficiency.
9. The method for preparing layered barium carbonate according to claim 1, characterized in that: Depending on the preparation requirements, the reaction raw materials can be replaced to prepare layered strontium carbonate and layered lithium carbonate.