Preparation method of cross-linked polyvinylpyrrolidone surface modified perfluorosulfonic acid membrane
By forming a crosslinked polyvinylpyrrolidone layer on the perfluorosulfonic acid film, the problem of insufficient stability of vanadium ion permeation and vanadium resisting layer in vanadium batteries is solved, and the film performance with high stability and high ion selectivity is achieved, which improves the The battery performance and service life of vanadium batteries.
Patent Information
- Application Number
- CN202411399831.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing perfluorosulfonic acid films have vanadium ion permeability problems in vanadium batteries, resulting in a reduction in battery bank efficiency and insufficient chemical stability and conductivity of the vanadium resisting layer, making it difficult to meet the needs of high stability and high ion selectivity.
The perfluorosulfonic acid film prepared by the surface modified crosslinked polyvinylpyrrolidone is prepared by forming a crosslinked polyvinylpyrrolidone layer on the perfluorosulfonic acid resin, and N-vinyl-2-pyrrolidone and alkali metal hydroxide are used in the The crosslinking reaction is carried out at high temperature to form a crosslinking layer with water absorption and swelling properties and vanadium-resistance properties, and is embedded in the perfluorosulfonic acid base film to improve stability.
It effectively reduces the shuttle of vanadium ions, maintains the ionic conductivity of the membrane, improves the chemical and mechanical stability of the battery, and extends the service life of the battery.
Smart Images

Figure CN118909288A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of all-vanadium liquid flow battery diaphragm, in particular to a method for preparing a cross-linked polymer surface-modified perfluorosulfonic acid membrane. Background Art
[0002] Electrochemical energy storage system is a large-scale energy storage technology that realizes the conversion of electrical energy and chemical energy. It can quickly and effectively store and release a large amount of energy to meet people's needs. Among them, all-vanadium liquid flow battery (abbreviated as vanadium battery) energy storage has the advantages of large energy storage capacity, flexible design, recyclable electrolyte, safety and reliability, economic and long-term, etc. It has become one of the most mature and promising technologies in large-scale energy storage technology. It has been greatly developed and applied in the fields of day and night peak load regulation and load balancing of power grids, electric vehicle power supply, solar and wind power station power storage, etc. As one of the key components of vanadium battery, ion exchange membrane not only plays the role of isolating positive and negative electrolytes in vanadium battery, but also serves as a medium for transferring protons. The performance of ion exchange membrane directly affects the performance and service life of vanadium battery. The ideal ion exchange membrane should have excellent ion conductivity, high ion selectivity, excellent mechanical and chemical stability, low cost and other characteristics. At present, perfluorosulfonic acid membrane has become the most widely used ion exchange membrane for vanadium batteries due to its excellent electrochemical performance and chemical stability. However, during the long-term operation of the battery, the ion exchange membrane will experience serious vanadium ion penetration, which will greatly reduce the coulombic efficiency of the battery and gradually decay the discharge capacity of the battery, greatly increasing the maintenance cost of the vanadium battery. Therefore, it is necessary to modify the perfluorosulfonic acid membrane to improve its vanadium barrier ability. The commonly used method is to use some inorganic or organic components to compound with the sulfonic acid groups in the membrane to block the hydrophilic groups (such as hydrated vanadium ions) from passing through the membrane. Among them, using the perfluorosulfonic acid membrane as a matrix and introducing a layer of water-soluble organic vanadium barrier layer (such as polyethyleneimine, polypyrrole, polyvinylpyrrolidone, etc.) on its surface is considered to be a relatively economical and effective method. In this structure, the special properties of the composite membrane provide excellent chemical and mechanical stability, as well as high ion conductivity, and the thinner vanadium barrier surface layer introduced can reduce the vanadium ion permeability of the composite membrane. However, this method also has some disadvantages. First, some vanadium barrier layers are not resistant to strong acidity and strong oxidation, and have poor chemical stability; second, these vanadium barrier layers have high surface resistance, which reduces the conductivity of the composite membrane; third, some vanadium barrier layers are compounded with the sulfonic acid resin matrix through weak interaction forces, which are not resistant to long-term erosion of the electrolyte, and once separated from the membrane surface, these water-soluble polymers will be adsorbed on the electrode surface under the action of electrostatic force, causing the electrode performance to decline. Therefore, finding a perfluorosulfonic acid proton exchange membrane with high stability, high ion selectivity, and high ion conductivity for vanadium batteries and its modification method has become one of the hot spots and difficulties in the field of vanadium batteries. Summary of the invention
[0003] In view of the above problems or shortcomings, the present invention provides a method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane. The technical solution adopted by the present invention is as follows: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane comprises at least the following steps: S1: ultrasonically clean the commercial perfluorosulfonic acid resin with hydrogen peroxide, and then repeatedly clean it with deionized water and dry it to obtain perfluorosulfonic acid resin powder; S2: Weigh 10-30 parts by mass of perfluorosulfonic acid resin powder and add it to 70-90 parts by mass of solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2μm pore size polytetrafluoroethylene microporous filter membrane to obtain a perfluorosulfonic acid solution with a mass fraction of 10%-30%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.1-0.5 parts by mass of alkali metal hydroxide powder and add it to 20-50 parts by mass of N-vinyl-2-pyrrolidone (NVP), stir evenly to form a suspension with a mass fraction of 0.5%-1%; S5: 10-20 parts by weight of the suspension is applied by knife coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 140-180° C. for 2-3 hours to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: tearing off the semi-finished sulfonic acid film modified by cross-linked polyvinyl pyrrolidone from the glass plate, soaking it in a sulfuric acid solution and washing it with deionized water, and drying it at room temperature to obtain a perfluorosulfonic acid film modified by the surface of cross-linked polyvinyl pyrrolidone.
[0004] Preferably, the mass percentage of hydrogen peroxide in step S1 is 5%-10%, and the drying temperature is 60-90°C.
[0005] Preferably, the organic solvent in step S2 is at least one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP).
[0006] Preferably, the alkali metal hydroxide in step S4 is at least one of sodium hydroxide and potassium hydroxide.
[0007] Preferably, the particle size of the alkali metal hydroxide powder in step S4 is 0.1-0.3 μm.
[0008] Preferably, in step S6, the concentration of the sulfuric acid solution is 1-4 mol / L, and the soaking time is 2-4 h.
[0009] Preferably, the perfluorosulfonic acid membrane surface-modified with cross-linked polyvinyl pyrrolidone is applied to the all-vanadium redox flow battery, and the side containing the cross-linked polyvinyl pyrrolidone is placed in contact with the negative electrode of the all-vanadium redox flow battery.
[0010] The beneficial effects of the present invention include at least: 1. N-vinyl-2-pyrrolidone undergoes a proliferation cross-linking reaction under alkali metal hydroxide and high temperature conditions, forming cross-linked polyvinyl pyrrolidone (PVPP) in situ. When the modified surface of the perfluorosulfonic acid membrane modified by cross-linked polyvinyl pyrrolidone faces the negative electrode, the cross-linked polyvinyl pyrrolidone has a certain water absorption and swelling property. After contacting the electrolyte, its pyrrole ring structure is positively charged, has good vanadium resistance, and can reduce the shuttle of vanadium, especially the shuttle of divalent vanadium ions. 2. Cross-linked polyvinyl pyrrolidone is insoluble in water, and its cross-linked layer has well-developed pores, which does not affect the transmission of hydrated protons, that is, it does not affect the ionic conductivity of the sulfonic acid membrane; 3. Cross-linked polyvinyl pyrrolidone is formed after the perfluorosulfonic acid solution is pre-dried and before the film is completely formed. Its polymer skeleton is partially embedded in the micropores of the perfluorosulfonic acid-based membrane and has a strong bonding force with the base membrane. It is not easily washed away by the electrolyte when running in the battery stack, and its stability is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is a flow chart for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane of the present invention; Figure 2 This is a schematic diagram of an application method of a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane of the present invention; Figure 3 is the reaction formula of cross-linked polyvinyl pyrrolidone in the present invention; Figure 4 The infrared spectrum of the cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane of the present invention. DETAILED DESCRIPTION
[0012] The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] The present invention is a cross-linked polyvinyl pyrrolidone surface modified perfluorosulfonic acid membrane using Figure 1 The preparation method shown is obtained and is further illustrated by the following examples.
[0014] Embodiment 1: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 5% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 60°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 10 g of perfluorosulfonic acid resin powder and add it to 90 g of N,N-dimethylacetamide (DMAc) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2 μm pore size polytetrafluoroethylene microporous filter membrane to obtain a 10% perfluorosulfonic acid solution; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.1 g of sodium hydroxide powder with a particle size of 0.1 μm and add it to 20 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.5%; S5: 10 g of the suspension was applied by blade coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 140° C. for 2 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone was torn off from the glass plate, immersed in a 1 mol / L sulfuric acid solution for 2 h and washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid film with a cross-linked polyvinyl pyrrolidone surface modified perfluorosulfonic acid film.
[0015] Embodiment 2: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 6% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 65°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 14 g of perfluorosulfonic acid resin powder and add it to 86 g of N,N-dimethylformamide (DMF) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a polytetrafluoroethylene microporous filter membrane with a pore size of 2 μm to obtain a perfluorosulfonic acid solution with a mass fraction of 14%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.15 g of potassium hydroxide powder with a particle size of 0.15 μm and add it to 25 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.6%; S5: 12 g of the suspension was applied by knife coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 150° C. for 2 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone was torn off from the glass plate, immersed in a 1.5 mol / L sulfuric acid solution for 2 h and washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid film with a cross-linked polyvinyl pyrrolidone surface modified perfluorosulfonic acid film.
[0016] Embodiment 3: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 7% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 70°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 18 g of perfluorosulfonic acid resin powder and add it to 82 g of dimethyl sulfoxide (DMSO) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a polytetrafluoroethylene microporous filter membrane with a pore size of 2 μm to obtain a perfluorosulfonic acid solution with a mass fraction of 18%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.2 g of sodium hydroxide powder with a particle size of 0.15 μm and add it to 30 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.66%; S5: 14 g of the suspension was applied by knife coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 155° C. for 2.5 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone was torn off from the glass plate, soaked in a 2 mol / L sulfuric acid solution for 2.5 h and washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid film with a cross-linked polyvinyl pyrrolidone surface modified perfluorosulfonic acid film.
[0017] Example 4: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 8% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 70°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 20 g of perfluorosulfonic acid resin powder and add it to 80 g of N,N-dimethylacetamide (DMAc) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2 μm pore size polytetrafluoroethylene microporous filter membrane to obtain a 20% perfluorosulfonic acid solution; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.2 g of sodium hydroxide powder with a particle size of 0.2 μm and add it to 35 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.57%; S5: 15 g of the suspension was applied by knife coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 160° C. for 2.5 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone is torn off from the glass plate, immersed in a 2 mol / L sulfuric acid solution for 3 h and washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid film modified with the surface of cross-linked polyvinyl pyrrolidone.
[0018] Example 5: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 8% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 75°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 22g of perfluorosulfonic acid resin powder and add it to 78g of N-methylpyrrolidone (NMP) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a polytetrafluoroethylene microporous filter membrane with a pore size of 2μm to obtain a perfluorosulfonic acid solution with a mass fraction of 22%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.3 g of potassium hydroxide powder with a particle size of 0.25 μm and add it to 40 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.74%; S5: 16 g of the suspension was applied by knife coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 165° C. for 2.5 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone was torn off from the glass plate, soaked in a 2.5 mol / L sulfuric acid solution for 3.5 h and washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid film modified with the surface of cross-linked polyvinyl pyrrolidone.
[0019] Example 6: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 9% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 80°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 26 g of perfluorosulfonic acid resin powder and add it to 74 g of N,N-dimethylformamide (DMF) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2 μm pore size polytetrafluoroethylene microporous filter membrane to obtain a perfluorosulfonic acid solution with a mass fraction of 26%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.4 g of sodium hydroxide powder with a particle size of 0.25 μm and add it to 45 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.88%; S5: 20 g of the suspension was scraped onto the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 170° C. for 3 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone was torn off from the glass plate, soaked in a 3 mol / L sulfuric acid solution for 3.5 h and washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid film with a cross-linked polyvinyl pyrrolidone surface modified perfluorosulfonic acid film.
[0020] Example 7: A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 10% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 90°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 30 g of perfluorosulfonic acid resin powder and add it to 70 g of N,N-dimethylacetamide (DMAc) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2 μm pore size polytetrafluoroethylene microporous filter membrane to obtain a perfluorosulfonic acid solution with a mass fraction of 30%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.5 g of potassium hydroxide powder with a particle size of 0.3 μm and add it to 50 g of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 1%; S5: 20 g of the suspension was scraped onto the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 180° C. for 3 h to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: The semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone is torn off from the glass plate, immersed in a 4 mol / L sulfuric acid solution for 4 h and washed with deionized water, and dried at room temperature to obtain a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid film.
[0021] Comparative Example 1: The preparation process comprises the following steps: S1: The commercial perfluorosulfonic acid resin was ultrasonically cleaned with 8% hydrogen peroxide, and then repeatedly cleaned with deionized water and dried at 70°C to obtain perfluorosulfonic acid resin powder; S2: Weigh 20 g of perfluorosulfonic acid resin powder and add it to 80 g of N,N-dimethylacetamide (DMAc) solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2-micron pore size polytetrafluoroethylene microporous filter membrane to obtain a 20% perfluorosulfonic acid solution; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Drying at 160° C. for 2.5 h to obtain a semi-finished sulfonic acid membrane; S5: The semi-finished sulfonic acid membrane is torn off from the glass plate, soaked in a 2 mol / L sulfuric acid solution for 3 h, washed with deionized water, and dried at room temperature to obtain a perfluorosulfonic acid membrane.
[0022] Comparative Example 2: The preparation process is consistent with that of Example 4, except that step S4, that is, no sodium hydroxide powder is added to 35 g of N-vinyl-2-pyrrolidone.
[0023] The membranes prepared in Examples 1-7 and Comparative Examples 1-2 were assembled into a stack, with the modified surface of the cross-linked polyvinyl pyrrolidone-modified perfluorosulfonic acid membrane, i.e., the membrane surface containing cross-linked polyvinyl pyrrolidone, facing the negative electrode. This is because the radius of the divalent vanadium ion measured at the negative electrode is small and is most likely to migrate through the membrane. The stack was tested under the same operating conditions and the coulombic efficiency, voltage efficiency, and energy efficiency at the 10th and 1000th cycles were recorded. The test results are shown in Table 1: Table 1 Battery stack performance test table
[0024] As shown in Table 1, compared with Comparative Example 1, Examples 1-7 have little difference in voltage efficiency in the initial test and after 1000 cycles, mainly because the coulombic efficiency and energy efficiency of the former are higher than those of the latter. This is because N-vinyl-2-pyrrolidone undergoes a proliferation cross-linking reaction under alkali metal hydroxide and high temperature conditions, such as Figure 3 As shown, cross-linked polyvinyl pyrrolidone was formed in situ, such as Figure 4 As shown, N-vinyl-2-pyrrolidone monomer has a peak at 1705 cm -1 There is a carbonyl stretching vibration absorption peak at 1629 cm -1 There is a strong C=C double bond stretching vibration absorption peak at 1286 cm -1There is an absorption peak of CN bond stretching vibration in the pyrrolidone ring at 1286 cm, which is a characteristic band of the amide group, indicating the presence of N-vinyl-2-pyrrolidone monomer. In the infrared spectrum of cross-linked polyvinyl pyrrolidone, there is also an absorption peak of CN bond stretching vibration in the pyrrolidone ring at 1286 cm -1 The characteristic absorption peaks of pyrrolidone ring appeared at 3110 and 1629 cm -1 No absorption peaks appeared at all places, indicating that there was no C=C double bond in the cross-linked polyvinyl pyrrolidone product, that is, the monomers had all been converted into polymers, indicating that the cross-linked polyvinyl pyrrolidone was successfully prepared; Figure 2 As shown, when the modified surface of the perfluorosulfonic acid membrane modified by cross-linked polyvinyl pyrrolidone faces the negative electrode, the cross-linked polyvinyl pyrrolidone has a certain water absorption and swelling property. After contacting the electrolyte, its pyrrole ring structure is positively charged, has good vanadium resistance, can reduce the shuttling of vanadium, especially reduce the shuttling of divalent vanadium ions, and in addition, the cross-linked polyvinyl pyrrolidone is insoluble in water, and its cross-linked layer has developed pores, which does not affect the transmission of hydrated protons, that is, it does not affect the ionic conductivity of the sulfonic acid membrane; compared with Comparative Example 2, the voltage efficiency, coulomb efficiency and energy efficiency of Examples 1 to 7 are quite different in the initial test and after 1000 cycles. This is because, in Comparative Example 2, no alkali metal hydroxide is added, and N-vinyl-2-pyrrolidone cannot form a cross-linked polyvinyl pyrrole At the same time, N-vinyl-2-pyrrolidone itself has insulating properties, which affects the ionic conductivity of the membrane and leads to low voltage efficiency. After 1000 cycles of testing, N-vinyl-2-pyrrolidone gradually falls off the membrane and dissolves in the electrolyte, resulting in a decrease in coulombic efficiency. At the same time, N-vinyl-2-pyrrolidone in the electrolyte is gradually adsorbed by the electrode, affecting the electrode activity, resulting in a further decrease in voltage efficiency. The cross-linked polyvinyl pyrrolidone is formed after the perfluorosulfonic acid solution is pre-dried and before the film is completely formed. Its polymer skeleton is partially embedded in the micropores of the perfluorosulfonic acid-based membrane, and has a strong bonding force with the base membrane. It is not easily washed away by the electrolyte when running in the battery stack, and its stability is greatly improved.
[0025] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane, comprising at least the following steps: S1: ultrasonically clean the commercial perfluorosulfonic acid resin with hydrogen peroxide, and then repeatedly clean it with deionized water and dry it to obtain perfluorosulfonic acid resin powder; S2: Weigh 10-30 parts by mass of perfluorosulfonic acid resin powder and add it to 70-90 parts by mass of solvent, heat it to 120°C and stir it to dissolve it, and filter it through a sand core filter device with a 2μm pore size polytetrafluoroethylene microporous filter membrane to obtain a perfluorosulfonic acid solution with a mass fraction of 10%-30%; S3: The perfluorosulfonic acid solution is slowly poured onto a flat glass plate by a casting method to form a film, and dried at 70°C for 1 hour to obtain a pre-dried sulfonic acid-based film; S4: Weigh 0.1-0.5 parts by mass of alkali metal hydroxide powder and add it to 20-50 parts by mass of N-vinyl-2-pyrrolidone, stir evenly to form a suspension with a mass fraction of 0.5%-1%; S5: 10-20 parts by weight of the suspension is applied by knife coating on the pre-dried sulfonic acid-based film on the flat glass plate in S3, and dried at 140-180° C. for 2-3 hours to obtain a semi-finished sulfonic acid film modified with cross-linked polyvinyl pyrrolidone; S6: tearing off the semi-finished sulfonic acid film modified by cross-linked polyvinyl pyrrolidone from the glass plate, soaking it in a sulfuric acid solution and washing it with deionized water, and drying it at room temperature to obtain a perfluorosulfonic acid film modified by the surface of cross-linked polyvinyl pyrrolidone.
2. The method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane according to claim 1, characterized in that: The mass percentage of hydrogen peroxide in step S1 is 5%-10%, and the drying temperature is 60-90°C.
3. The method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane according to claim 1, characterized in that: The solvent in step S2 is at least one of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.
4. The method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane according to claim 1, characterized in that: In step S4, the alkali metal hydroxide is at least one of sodium hydroxide and potassium hydroxide.
5. The method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane according to claim 1, characterized in that: In step S4, the particle size of the alkali metal hydroxide powder is 0.1-0.3 μm.
6. The method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane according to claim 1, characterized in that: In step S6, the concentration of the sulfuric acid solution is 1-4 mol / L, and the soaking time is 2-4 h.
7. The method for preparing a cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane according to claim 1, characterized in that: The cross-linked polyvinyl pyrrolidone surface-modified perfluorosulfonic acid membrane is applied to an all-vanadium redox flow battery, and the side containing the cross-linked polyvinyl pyrrolidone is in contact with the negative electrode of the all-vanadium redox flow battery.
Citation Information
Patent Citations
Application of ion exchange group grafting type porous diaphragm to liquid flow energy storage battery
CN103840110A
Redox flow secondary battery and electrolyte membrane for redox flow secondary batteries
CN105845958A
Composite proton exchange membrane for vanadium redox flow battery and preparation method of composite proton exchange membrane
CN116247256A
Modification method of perfluorosulfonic acid proton exchange membrane, modified perfluorosulfonic acid proton exchange membrane and application of modified perfluorosulfonic acid proton exchange membrane
CN118738481A
Polymer electrolyte membrane, membrane electrode assembly, and solid polymer electrolyte fuel cell
US20200358119A1