Cross-linked sulfonated polybenzimidazole composite membrane for vanadium battery and preparation method of cross-linked sulfonated polybenzimidazole composite membrane
By crosslinking the anthracene cross-linking structure and dimer large volume and butterfly-like rigid structure of the sulfonated polystyrene phenylazole composite film, the low proton conductivity and voltage efficiency of the polybenzimidazole film in all vanadium flow batteries is solved. The problem of this problem achieves higher water absorption and acid absorption and mechanical stability, and improves the voltage and Coulomb efficiency of vanadium batteries.
Patent Information
- Application Number
- CN202411428499.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polybenzimidazole membranes in all vanadium flow cells have low proton conductivity and low voltage efficiency due to high surface resistance and close molecular packing, and the introduction of ion exchange groups impairs mechanical strength and chemical stability.
The preparation method of crosslinked sulfonated polystyrenepropizole composite film is adopted. Through the anthracene crosslinking structure, the large volume of dimer and the butterfly-like rigid structure, the water absorption and acid absorption capacity and mechanical stability of the film are improved, and swelling is limited to maintain resistance. Vanadium capacity.
The proton conductivity and voltage efficiency of vanadium batteries are improved, while the mechanical stability and Coulomb efficiency of the membrane are improved, and excellent vanadium resistance capability is maintained.
Smart Images

Figure CN118955988A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ion exchange membranes for all-vanadium liquid flow batteries, and in particular to a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries and a preparation method thereof. Background Art
[0002] Polybenzimidazole membranes are used in all-vanadium flow batteries and have excellent vanadium resistance, which can show up to 99% Coulomb efficiency. However, due to the high surface resistance of polybenzimidazole membranes, assembled all-vanadium flow batteries usually cannot provide satisfactory voltage efficiency. The benzimidazole groups in the polybenzimidazole chain tend to be parallel oriented during solvent evaporation, and the intermolecular hydrogen bond interaction makes the molecular chains densely stacked, which leads to the low acid absorption capacity of the polybenzimidazole membrane for the supporting electrolyte (such as 3MH2SO4) of the all-vanadium flow battery, making it difficult to form a continuous proton transport network in the membrane, resulting in low proton conductivity. Therefore, to realize the practical application of PBI membranes, it is necessary to further improve the ionic conductivity of polybenzimidazole membranes while maintaining their high ion selectivity and chemical stability. Generally, the introduction of ion exchange groups is an effective way to improve the ionic conductivity of polybenzimidazole membranes, but it usually damages the mechanical strength, chemical stability and ion selectivity of the membrane, and even makes the polybenzimidazole membrane soluble in water. Summary of the invention
[0003] The object of the present invention is to provide a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries and a preparation method thereof to solve the above problems.
[0004] The technical solution adopted by the present invention is as follows: A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, dissolving 2-5 parts by mass of anthrone, 9-20 parts by mass of dibromoalkane and 14-30 parts by mass of a catalyst in 120-150 parts by mass of a solvent, heating under reflux for 12-18 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by vacuum rotary evaporation to obtain compound 1; Step S2, adding 50-100 parts by mass of solvent and 1-2 parts by mass of sulfonated polyphenylimidazole powder into a reactor, dissolving them at 80° C., adding 1-2 parts by mass of a catalyst, stirring at 90-100° C. for 1-2 hours under a nitrogen atmosphere, fully mixing 0.3-0.6 parts by mass of compound 1 with 10-20 parts by mass of solvent, pouring into a reactor to react for 24-36 hours, and after the reaction is completed, pouring the solution into deionized water for precipitation, then washing with deionized water and acetone, and drying in an oven at 80° C. for 8-12 hours to obtain a polymer 1; Step S3, adding 10-20 parts by mass of solvent and 0.3-0.6 parts by mass of polymer 1 to a reactor, dissolving them at 25°C, adding 0.3-0.6 parts by mass of catalyst, heating to 90-100°C under a nitrogen atmosphere, stirring and reacting for 1-2h, then mixing 0.6-1.2 parts by mass of compound 2 with 2-4 parts by mass of solvent, pouring into a reactor and reacting for 24-36h, after the reaction is completed, pouring the reaction solution into deionized water for precipitation, then washing with deionized water and acetone, and drying in an oven at 80°C for 8-12h to obtain polymer 2; Step S4, dissolving 0.1-0.2 parts by mass of polymer 2 in 10-20 parts by mass of solvent at 80°C, casting it in a clean glass tank, coating it with a scraper, performing photocrosslinking reaction under ultraviolet light, and then placing it in an oven at 80°C to dry for 18-24 hours to obtain a cross-linked sulfonated polyphenylimidazole composite membrane.
[0005] Preferably, the dibromoalkane in step S1 is any one of 1,4-dibromobutane, 1,6-dibromohexane, 1,7-dibromoheptane, 1,10-dibromodecane and 1,12-dibromododecane.
[0006] Preferably, the catalyst in steps S1, S2 and S3 is any one of potassium carbonate, 4-dimethylaminopyridine, ammonium formate and sodium hydride.
[0007] Preferably, the solvent in steps S1, S2, S3 and S4 is any one of dimethyl sulfoxide, acetone, N,N-dimethylacetamide and N,N-dimethylformamide.
[0008] Preferably, in step S3, compound 2 is any one of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane, 2-(2-bromoethoxy)ethyl-trimethylammonium, and 2-(2-bromoethoxy)ethanol.
[0009] Preferably, the photocrosslinking reaction condition in step S4 is irradiation under 365 nm ultraviolet lamp for 1-2 h.
[0010] Preferably, in step S4, the thickness of the cross-linked sulfonated polyphenylimidazole composite membrane is 40-60 μm.
[0011] A cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries is obtained by adopting the preparation method of the cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries.
[0012] The beneficial effects of the present invention are: 1. The cross-linked sulfonated polyphenylimidazole composite membrane of the present invention has an anthracene photo-cross-linked structure. The large volume and butterfly-shaped rigid structure of the dimer hinder the close stacking of the polymer, so that the membrane has a higher water and acid absorption level, thereby improving the proton conductivity of the membrane, and further improving the voltage efficiency of the vanadium battery; 2. The cross-linked sulfonated polyphenylimidazole composite membrane of the present invention has an anthracene photo-cross-linked structure, which limits the swelling of the membrane, so that it maintains excellent vanadium resistance and inhibits the penetration of vanadium ions, thereby improving the coulombic efficiency of the vanadium battery; 3. The cross-linked sulfonated polyphenylimidazole composite membrane of the present invention has an anthracene photo-cross-linked structure, which can improve the tensile strength of the membrane and thus improve the mechanical stability of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a diagram showing the preparation mechanism of cross-linked sulfonated polybenzimidazole according to Example 1 of the present invention; Figure 2 1 is an infrared spectra of the sulfonated polybenzimidazole, polymer 1 and cross-linked sulfonated polybenzimidazole in Example 1 of the present invention. DETAILED DESCRIPTION
[0014] The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] The present invention provides a method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery, comprising the following steps: Step S1, dissolving 2-5 parts by mass of anthrone, 9-20 parts by mass of dibromoalkane and 14-30 parts by mass of catalyst in 120-150 parts by mass of solvent, heating and reflux for 12-18 hours under nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by vacuum rotary evaporation to obtain compound 1. Wherein, the dibromoalkane is any one of 1,4-dibromobutane, 1,6-dibromohexane, 1,7-dibromoheptane, 1,10-dibromodecane and 1,12-dibromododecane; the catalyst is any one of potassium carbonate, 4-dimethylaminopyridine, ammonium formate and sodium hydride; the solvent is any one of dimethyl sulfoxide, acetone, N,N-dimethylacetamide and N,N-dimethylformamide; Step S2, add 50-100 parts by mass of solvent and 1-2 parts by mass of sulfonated polyphenylimidazole powder to the reactor, dissolve at 80°C, add 1-2 parts by mass of catalyst, stir at 90-100°C for 1-2h under nitrogen atmosphere, fully mix 0.3-0.6 parts by mass of compound 1 with 10-20 parts by mass of solvent, pour into the reactor to react for 24-36h, pour the solution into deionized water for precipitation after the reaction, then wash with deionized water and acetone, put into an oven at 80°C for drying for 8-12h, and obtain polymer 1. Wherein, the solvent is any one of dimethyl sulfoxide, acetone, N,N-dimethylacetamide, and N,N-dimethylformamide; the catalyst is any one of potassium carbonate, 4-dimethylaminopyridine, ammonium formate, and sodium hydride; Step S3, add 10-20 parts by mass of solvent and 0.3-0.6 parts by mass of polymer 1 to the reactor, dissolve at 25°C, add 0.3-0.6 parts by mass of catalyst, heat to 90-100°C in a nitrogen atmosphere, stir and react for 1-2h, then mix 0.6-1.2 parts by mass of compound 2 with 2-4 parts by mass of solvent, pour into the reactor and react for 24-36h, after the reaction is completed, pour the reaction solution into deionized water for precipitation, then wash with deionized water and acetone, and dry in an oven at 80°C for 8-12h to obtain polymer 2. Wherein, the catalyst is any one of potassium carbonate, 4-dimethylaminopyridine, ammonium formate, and sodium hydride; compound 2 is any one of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane, 2-(2-bromoethoxy)ethyl-trimethylammonium, and 2-(2-bromoethoxy)ethanol; Step S4, dissolving 0.1-0.2 parts by mass of polymer 2 in 10-20 parts by mass of solvent at 80°C, casting it in a clean glass tank, applying it with a scraper, irradiating it under 365nm ultraviolet light for 1-2h for photocrosslinking reaction, and then placing it in an oven at 80°C for drying for 18-24h to obtain a cross-linked sulfonated polyphenylimidazole composite membrane, the thickness of the composite membrane is 40-60μm.
[0016] Example 1
[0017] A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, dissolving 2 parts by mass of anthrone, 9 parts by mass of 1,4-dibromobutane and 14 parts by mass of catalyst potassium carbonate in 120 parts by mass of solvent acetone, heating to reflux for 12 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by reduced pressure rotary evaporation to obtain compound 1.
[0018] Step S2, adding 50 parts by mass of solvent acetone and 1 part by mass of sulfonated polyphenylimidazole powder into a reactor, dissolving them at 80°C, adding 1 part by mass of catalyst potassium carbonate, and continuing to stir at 90°C for 1h under a nitrogen atmosphere, thoroughly mixing 0.3 parts by mass of compound 1 with 10 parts by mass of solvent acetone, pouring them into a reactor and reacting for 24h, after the reaction is completed, pouring the solution into deionized water for precipitation, then washing with deionized water and solvent acetone, and drying in an oven at 80°C for 8h to obtain polymer 1.
[0019] Step S3, adding 10 parts by mass of solvent acetone and 0.3 parts by mass of polymer 1 into a reactor, dissolving them at 25°C, adding 0.3 parts by mass of catalyst potassium carbonate, heating to 90°C under a nitrogen atmosphere, stirring and reacting for 1 hour, then mixing 0.6 parts by mass of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane with 2 parts by mass of solvent acetone, pouring into a reactor and reacting for 24 hours, after the reaction is completed, pouring the reaction solution into deionized water for precipitation, then washing with deionized water and solvent acetone, and drying in an oven at 80°C for 8 hours to obtain polymer 2.
[0020] Step S4, dissolving 0.1 parts by mass of polymer 2 in 10 parts by mass of solvent acetone at 80°C, casting it in a clean glass tank, coating it with a scraper, irradiating it under 365nm ultraviolet light for 1 hour for photocrosslinking reaction, and then placing it in an oven at 80°C for 18 hours to obtain a cross-linked sulfonated polyphenylimidazole composite membrane with a thickness of 50 μm.
[0021] like Figure 1 As shown, cross-linked sulfonated polyphenylimidazole can be photo-cross-linked by 365 nm ultraviolet light. Figure 2 As shown, the infrared spectra of polymer 2 and cross-linked sulfonated polyphenylimidazole are at 3078 and 2886 cm −1 The stretching vibration peak is shown at 1116 cm −1 The stretching vibration peak of COC can be observed at the sulfonated polyphenylimidazole main chain and the two grafted side chains. The above results show that PBI has successfully grafted compound 1 and 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane and cross-linking has occurred successfully.
[0022] Example 2
[0023] A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, dissolving 3 parts by mass of anthrone, 15 parts by mass of 1,6-dibromohexane and 20 parts by mass of catalyst 4-dimethylaminopyridine in 130 parts by mass of solvent dimethyl sulfoxide, heating to reflux for 14 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by reduced pressure rotary evaporation to obtain compound 1.
[0024] Step S2, add 70 parts by mass of solvent dimethyl sulfoxide and 1.2 parts by mass of sulfonated polyphenylimidazole powder into the reactor, dissolve them at 80°C, add 1.2 parts by mass of catalyst 4-dimethylaminopyridine, continue stirring at 95°C for 1.4h under a nitrogen atmosphere, fully mix 0.4 parts by mass of compound 1 with 13 parts by mass of solvent dimethyl sulfoxide, pour into the reactor and react for 26h, after the reaction is completed, pour the solution into deionized water for precipitation, then wash with deionized water and solvent acetone, put into an oven at 80°C and dry for 10h to obtain polymer 1.
[0025] Step S3, add 13 parts by mass of solvent dimethyl sulfoxide and 0.4 parts by mass of polymer 1 into the reactor, dissolve them at 25°C, add 0.4 parts by mass of catalyst 4-dimethylaminopyridine, heat to 94°C under a nitrogen atmosphere, stir and react for 1.4 hours, then mix 0.8 parts by mass of 2-(2-bromoethoxy)ethyl-trimethylammonium with 3 parts by mass of solvent dimethyl sulfoxide, pour into the reactor and react for 26 hours. After the reaction is completed, pour the reaction solution into deionized water for precipitation, then wash with deionized water and solvent acetone, and dry in an oven at 80°C for 10 hours to obtain polymer 2.
[0026] Step S4, dissolving 0.14 parts by mass of polymer 2 in 13 parts by mass of solvent dimethyl sulfoxide at 80°C, casting it in a clean glass tank, coating it with a scraper, irradiating it under 365nm ultraviolet light for 1.5 hours for photocrosslinking reaction, and then placing it in an oven at 80°C for drying for 20 hours to obtain a cross-linked sulfonated polyphenylimidazole composite membrane with a thickness of 40 μm.
[0027] Example 3
[0028] A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, dissolving 4 parts by mass of anthrone, 18 parts by mass of 1,7-dibromoheptane and 25 parts by mass of catalyst ammonium formate in 140 parts by mass of solvent N,N-dimethylacetamide, heating to reflux for 16 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by reduced pressure rotary evaporation to obtain compound 1.
[0029] Step S2, add 80 parts by mass of solvent N,N-dimethylacetamide and 1.5 parts by mass of sulfonated polyphenylimidazole powder into the reactor, dissolve them at 80°C, add 1.5 parts by mass of catalyst ammonium formate, continue stirring at 100°C for 1.7h under a nitrogen atmosphere, fully mix 0.5 parts by mass of compound 1 and 17 parts by mass of solvent N,N-dimethylacetamide, pour into the reactor and react for 30h, after the reaction is completed, pour the solution into deionized water for precipitation, then wash with deionized water and solvent acetone, put into an oven at 80°C and dry for 10h to obtain polymer 1.
[0030] Step S3, add 17 parts by mass of solvent N,N-dimethylacetamide and 0.5 parts by mass of polymer 1 into the reactor, dissolve them at 25°C, add 0.5 parts by mass of catalyst ammonium formate, heat to 96°C under a nitrogen atmosphere, stir and react for 1.7 hours, then mix 1.2 parts by mass of 2-(2-bromoethoxy)ethanol with 3 parts by mass of solvent N,N-dimethylacetamide, pour into the reactor and react for 30 hours. After the reaction is completed, pour the reaction solution into deionized water for precipitation, then wash with deionized water and solvent acetone, and dry in an oven at 80°C for 10 hours to obtain polymer 2.
[0031] Step S4, dissolving 0.16 parts by mass of polymer 2 in 17 parts by mass of solvent N,N-dimethylacetamide at 80°C, casting it in a clean glass tank, coating it with a scraper, irradiating it under 365nm ultraviolet light for 1.8 hours for photocrosslinking reaction, and then placing it in an oven at 80°C for drying for 22 hours to obtain a cross-linked sulfonated polyphenylimidazole composite membrane with a thickness of 45 μm.
[0032] Example 4
[0033] A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, dissolving 5 parts by mass of anthrone, 20 parts by mass of 1,10-dibromodecane and 30 parts by mass of catalyst sodium hydride in 150 parts by mass of solvent N,N-dimethylformamide, heating to reflux for 18 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by reduced pressure rotary evaporation to obtain compound 1.
[0034] Step S2, adding 100 parts by mass of solvent N,N-dimethylformamide and 2 parts by mass of sulfonated polyphenylimidazole powder into a reactor, dissolving them at 80°C, adding 2 parts by mass of catalyst sodium hydride, and continuing to stir at 100°C for 2h under a nitrogen atmosphere, thoroughly mixing 0.6 parts by mass of compound 1 with 20 parts by mass of solvent N,N-dimethylformamide, pouring into a reactor and reacting for 36h, after the reaction is completed, pouring the solution into deionized water for precipitation, then washing with deionized water and solvent acetone, and drying in an oven at 80°C for 12h to obtain polymer 1.
[0035] Step S3, adding 20 parts by mass of solvent N,N-dimethylformamide and 0.6 parts by mass of polymer 1 into a reactor, dissolving them at 25°C, adding 0.6 parts by mass of catalyst sodium hydride, heating to 100°C under a nitrogen atmosphere, stirring and reacting for 2 hours, then mixing 0.8 parts by mass of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane with 4 parts by mass of solvent N,N-dimethylformamide, pouring into a reactor and reacting for 36 hours, after the reaction is completed, pouring the reaction solution into deionized water for precipitation, then washing with deionized water and solvent acetone, and drying in an oven at 80°C for 12 hours to obtain polymer 2.
[0036] Step S4, dissolving 0.2 parts by mass of polymer 2 in 20 parts by mass of solvent N,N-dimethylformamide at 80°C, casting it in a clean glass tank, coating it with a scraper, irradiating it under 365nm ultraviolet light for 2h for photocrosslinking reaction, and then placing it in an oven at 80°C for drying for 24h to obtain a cross-linked sulfonated polyphenylimidazole composite membrane with a thickness of 60μm.
[0037] Example 5
[0038] A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for a vanadium battery comprises the following steps: Step S1, dissolving 3 parts by mass of anthrone, 12 parts by mass of 1,12-dibromododecane and 18 parts by mass of catalyst potassium carbonate in 130 parts by mass of solvent acetone, heating to reflux for 14 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by reduced pressure rotary evaporation to obtain compound 1.
[0039] Step S2, add 60 parts by mass of solvent acetone and 1.3 parts by mass of sulfonated polyphenylimidazole powder into the reactor, dissolve them at 80°C, add 1.4 parts by mass of catalyst potassium carbonate, continue stirring at 95°C for 1.5h under a nitrogen atmosphere, fully mix 0.4 parts by mass of compound 1 with 15 parts by mass of solvent acetone, pour into the reactor and react for 30h, after the reaction is completed, pour the solution into deionized water for precipitation, then wash with deionized water and solvent acetone, put into an oven at 80°C and dry for 10h to obtain polymer 1.
[0040] Step S3, adding 15 parts by mass of solvent acetone and 0.4 parts by mass of polymer 1 into a reactor, dissolving them at 25° C., adding 0.5 parts by mass of catalyst potassium carbonate, heating to 96° C. under a nitrogen atmosphere, stirring and reacting for 1.5 hours, then mixing 1.0 parts by mass of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane with 3 parts by mass of solvent acetone, pouring into a reactor and reacting for 30 hours, after the reaction is completed, pouring the reaction solution into deionized water for precipitation, then washing with deionized water and solvent acetone, and drying in an oven at 80° C. for 10 hours to obtain polymer 2.
[0041] Step S4, dissolving 0.15 parts by mass of polymer 2 in 15 parts by mass of solvent acetone at 80°C, casting it in a clean glass tank, coating it with a scraper, irradiating it with 365nm ultraviolet light for 1.4 hours for photocrosslinking reaction, and then placing it in an oven at 80°C for drying for 20 hours to obtain a cross-linked sulfonated polyphenylimidazole composite membrane with a thickness of 55 μm.
[0042] Comparative Example 1 Step S1, add 10 parts by mass of solvent acetone and 0.3 parts by mass of polymer sulfonated polybenzimidazole into a reactor, dissolve them at 25°C, add 0.3 parts by mass of catalyst potassium carbonate, heat to 90°C under a nitrogen atmosphere, stir and react for 1 hour, then mix 0.6 parts by mass of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane with 2 parts by mass of solvent acetone, pour into a reactor and react for 24 hours. After the reaction is completed, pour the reaction solution into deionized water for precipitation, then wash with deionized water and solvent acetone, and dry in an oven at 80°C for 8 hours to obtain polymer 2.
[0043] Step S2, dissolving 0.1 parts by mass of polymer 2 in 10 parts by mass of solvent acetone at 80°C, casting it in a clean glass tank, coating it with a scraper, and then placing it in an oven at 80°C to dry for 18 hours to obtain a grafted modified sulfonated polyphenylimidazole composite membrane with a thickness of 50 μm.
[0044] Comparative Example 2 Blank sulfonated polyphenylimidazole membrane, membrane thickness is 50 μm.
[0045] 1. Mechanical properties test The mechanical properties of the films of the examples and comparative examples were measured using a SHIMADZUAG-I1KN universal testing machine. The film samples to be tested were cut into 5 mm×50 mm specifications and stretched at a stretching speed of 100 mm / min for mechanical property testing.
[0046] 2. The membrane is assembled into a stack for efficiency testing The embodiment and comparative example membranes were assembled into a stack for testing, and the coulombic efficiency, voltage efficiency and energy efficiency were tested and recorded under the same test conditions. The test results are shown in the following table: Table 1: Performance test table of membrane modules using examples and comparative examples
[0047] It can be seen that Examples 1-5 have higher tensile strengths than Comparative Examples 1 and 2, because the cross-linked sulfonated polyphenylimidazole composite membrane of the present invention has an anthracene photocrosslinking structure, which can improve the tensile strength of the membrane, thereby improving the mechanical stability of the membrane. Comparative Example 1 has higher voltage efficiency and lower tensile strength and coulomb efficiency than Comparative Example 2, because the hydrophilic side chain introduced into the sulfonated polyphenylimidazole improves the ion conductivity of the polybenzimidazole membrane, thereby making the vanadium battery have a higher voltage efficiency, but the swelling becomes larger, which damages the mechanical strength and compactness of the membrane, thereby reducing the coulomb efficiency of the vanadium battery. Examples 1-5 have higher voltage efficiency than Comparative Examples 1 and 2, because the cross-linked sulfonated polyphenylimidazole composite membrane of the present invention has an anthracene photocrosslinking structure, and the large volume and butterfly-shaped rigid structure of the dimer hinder the close stacking of the polymer, so that the membrane obtains a higher water and acid absorption level, thereby improving the proton conductivity of the membrane, thereby improving the voltage efficiency of the vanadium battery. In addition, the cross-linked sulfonated polyphenylimidazole composite membrane of the present invention has an anthracene photo-cross-linked structure, which limits the swelling of the membrane, so that it maintains excellent vanadium resistance and inhibits the penetration of vanadium ions, thereby improving the coulombic efficiency of the vanadium battery.
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries, characterized in that: The following steps are involved: Step S1, dissolving 2-5 parts by mass of anthrone, 9-20 parts by mass of dibromoalkane and 14-30 parts by mass of a catalyst in 120-150 parts by mass of a solvent, heating under reflux for 12-18 hours under a nitrogen atmosphere, cooling to room temperature, passing through a column and removing the solvent by vacuum rotary evaporation to obtain compound 1; Step S2, adding 50-100 parts by mass of solvent and 1-2 parts by mass of sulfonated polyphenylimidazole powder into a reactor, dissolving them at 80° C., adding 1-2 parts by mass of a catalyst, stirring at 90-100° C. for 1-2 hours under a nitrogen atmosphere, fully mixing 0.3-0.6 parts by mass of compound 1 with 10-20 parts by mass of solvent, pouring into a reactor to react for 24-36 hours, and after the reaction is completed, pouring the solution into deionized water for precipitation, then washing with deionized water and acetone, and drying in an oven at 80° C. for 8-12 hours to obtain a polymer 1; Step S3, adding 10-20 parts by mass of solvent and 0.3-0.6 parts by mass of polymer 1 to a reactor, dissolving them at 25°C, adding 0.3-0.6 parts by mass of catalyst, heating to 90-100°C under a nitrogen atmosphere, stirring and reacting for 1-2h, then mixing 0.6-1.2 parts by mass of compound 2 with 2-4 parts by mass of solvent, pouring into a reactor and reacting for 24-36h, after the reaction is completed, pouring the reaction solution into deionized water for precipitation, then washing with deionized water and acetone, and drying in an oven at 80°C for 8-12h to obtain polymer 2; Step S4, dissolving 0.1-0.2 parts by mass of polymer 2 in 10-20 parts by mass of solvent at 80°C, casting it in a clean glass tank, coating it with a scraper, performing photocrosslinking reaction under ultraviolet light, and then placing it in an oven at 80°C to dry for 18-24 hours to obtain a cross-linked sulfonated polyphenylimidazole composite membrane.
2. The method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: The dibromoalkane in step S1 is any one of 1,4-dibromobutane, 1,6-dibromohexane, 1,7-dibromoheptane, 1,10-dibromodecane and 1,12-dibromododecane.
3. The method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: The catalyst in step S1, step S2 and step S3 is any one of potassium carbonate, 4-dimethylaminopyridine, ammonium formate and sodium hydride.
4. The method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: In step S1, step S2, step S3 and step S4, the solvent is any one of dimethyl sulfoxide, acetone, N,N-dimethylacetamide and N,N-dimethylformamide.
5. The method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: In step S3, compound 2 is any one of 1-(2-bromoethoxy)-2-(2-methoxyethoxy)ethane, 2-(2-bromoethoxy)ethyl-trimethylammonium, and 2-(2-bromoethoxy)ethanol.
6. The method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: The photo-crosslinking reaction condition in step S4 is irradiation under 365 nm ultraviolet light for 1-2 h.
7. The method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries according to claim 1, characterized in that: The thickness of the cross-linked sulfonated polyphenylimidazole composite membrane in step S4 is 40-60 μm.
8. A cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries, characterized in that: The composite membrane is prepared by the method for preparing a cross-linked sulfonated polyphenylimidazole composite membrane for vanadium batteries as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Polyhydroxy functionalized polybenzimidazole ion exchange membrane and preparation method
CN110078961A
SCOF sulfonated polybenzimidazole ion exchange composite membrane and preparation method thereof