Ester group-containing cured epoxy material and degradation method of composite material thereof

By using low-carbon fatty amine compounds and epoxy resins to perform amine decomposition reaction at low temperatures, the problem of difficulty in recycling and high-temperature degradation of epoxy resin materials is solved, and low-energy-consuming epoxy curing is achieved decomposition and recycling of matter.

CN118909305APending Publication Date: 2024-11-08SWANCOR INNOVATION & INCUBATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310509088.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing epoxy resin materials are difficult to recycle and reuse after being discarded, and the high-temperature degradation process consumes high energy, making it difficult to achieve a low-energy-consuming degradation method.

Method used

The degradation of the ester-containing epoxy cured substance is achieved by mixing it with an ester-containing epoxy cured substance and performing an amine-degraded substance at a low temperature of 10°C to 50°C.

Benefits of technology

Without the need for a high temperature environment, the decomposition of the ester-containing epoxy cured substance is achieved, which reduces energy consumption and provides a low-energy recycling and treatment method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909305A_ABST
    Figure CN118909305A_ABST
Patent Text Reader

Abstract

The invention provides a degradation method of an ester group-containing cured epoxy material and a composite material thereof. The degradation method of the ester group-containing epoxy cured product comprises a mixing step and a degradation step. In the mixing step, the ester group-containing cured epoxy material and aliphatic amines are mixed to form a degradation system, and in the degradation step, the degradation system is placed at a degradation temperature to degrade the ester group-containing cured epoxy material. Therefore, the aliphatic amine compound with low carbon number is used as the degradation liquid to decompose the ester group-containing epoxy cured product at low temperature, so that the purpose of degradation without energy consumption is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a degradation method of an ester-containing epoxy cured product and a composite material thereof, in particular to a degradation method of an ester-containing epoxy cured product and a composite material thereof which can be implemented at low temperature. Background Art

[0002] Epoxy resin materials have the advantages of low viscosity and good operability before curing, and excellent thermal stability, mechanical strength and chemical resistance after curing. They are widely used in various fields and are often used in fiber composite materials with high strength and lightweight requirements. However, due to the chemical cross-linking characteristics of thermosetting materials, they are non-reprocessable, making it difficult to recycle and reuse thermosetting materials after they are discarded. With the rise of environmental awareness in recent years, the issue of waste disposal has gradually been taken seriously and has become the primary issue in the development of composite materials today.

[0003] In addition, after curing, epoxy resin will form a stable covalent network bond, which is difficult to decompose and recycle through chemical degradation. Therefore, in order to achieve the purpose of easy recycling after the product is retired, introducing easily destructible bonds into the epoxy structure is the main research direction of academia and industry.

[0004] At present, a research team has introduced a carbonate structure into the main chain of epoxy resin, and found that the derivative cured product of the epoxy resin after curing can be completely degraded by hexylamine at high temperature (125°C); another research team derived and synthesized active ester hardeners from waste polycarbonate, which still has the property of being degraded by hexylamine at high temperature after curing with epoxy resin. Therefore, the introduction of ester groups into epoxy cured products can be degraded and recovered by aminolysis, but degradation at high temperature has the disadvantage of energy consumption.

[0005] In view of this, how to find a suitable amine degradation liquid so that the epoxy curing material containing ester groups can be degraded without heating, thereby achieving the advantage of not consuming energy, has become the goal of relevant industries. Summary of the invention

[0006] An object of the present invention is to provide a method for degrading an ester-containing epoxy cured product and a composite material thereof, wherein a low-carbon aliphatic amine compound is used as a degradation liquid to decompose the ester-containing epoxy cured product at low temperature.

[0007] One embodiment of the present invention provides a method for degrading an ester-containing epoxy cured product, comprising a mixing step and a degradation step. The mixing step is to mix the ester-containing epoxy cured product with aliphatic amines to form a degradation system, and the degradation step is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured product.

[0008] According to the method for degrading an ester-containing epoxy cured product described in the preceding paragraph, the aliphatic amine may be a diamine or pentylamine having 2 to 5 carbon atoms.

[0009] According to the method for degrading an ester-containing epoxy cured product as described in the preceding paragraph, the ester group in the ester-containing epoxy cured product may refer to an ester group, a carbonate group or an urethane group.

[0010] According to the degradation method of the epoxy cured product containing ester group as described in the previous paragraph, the epoxy cured product containing ester group can be obtained by curing the epoxy compound containing ester structure with a hardener.

[0011] According to the degradation method of the epoxy cured product containing an ester group as described in the preceding paragraph, the ester group in the epoxy compound containing an ester group structure may refer to an ester group, a carbonate group or an urethane group.

[0012] According to the degradation method of the ester-containing epoxy curing material described in the previous paragraph, the hardener can be one of an amine hardener, a phenol hardener, an acid anhydride hardener, and an ester hardener, or a mixture of more than one of them.

[0013] According to the degradation method of the epoxy cured product containing ester groups described in the previous paragraph, the epoxy cured product containing ester groups can be obtained by curing an epoxy compound with an acid anhydride hardener or an ester hardener.

[0014] According to the degradation method of the ester-containing epoxy cured product described in the previous paragraph, the ester-containing epoxy cured product can be obtained by catalyzing an epoxy compound containing an ester structure with an acid-base catalyst and then subjecting it to epoxy self-curing.

[0015] According to the degradation method of the ester-containing epoxy cured product described in the preceding paragraph, the degradation temperature may be 10°C to 50°C.

[0016] Another embodiment of the present invention provides a method for degrading an ester-containing epoxy cured material composite material, comprising a mixing step and a degradation step. The mixing step is to mix the ester-containing epoxy cured material composite material with aliphatic amines to form a degradation system, and the degradation step is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured material composite material and filter and separate the polyol oligomer and the fiber.

[0017] According to the degradation method of the ester-containing epoxy cured material composite material described in the previous paragraph, the aliphatic amine can be a diamine or pentylamine having 2 to 5 carbon atoms.

[0018] According to the degradation method of the epoxy cured material composite material containing ester groups as described in the preceding paragraph, the ester group in the epoxy cured material composite material containing ester groups may refer to an ester group, a carbonate group or an urethane group.

[0019] According to the degradation method of the ester-containing epoxy cured material composite material described in the previous paragraph, the degradation temperature can be 10°C to 50°C.

[0020] Thus, the present invention mainly selects amine compounds with low carbon number, and immerses the epoxy cured product containing ester group in the amine compounds, so that the aminolysis reaction can be carried out without high temperature environment, thereby achieving the purpose of decomposing the epoxy cured product containing ester group. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to make the above and other objects, features, advantages and embodiments of the present invention more clearly understood, the following are the descriptions of the accompanying drawings:

[0022] Figure 1 FIG. 4 is a flow chart showing the steps of a method for degrading an ester-containing epoxy cured product according to one embodiment of the present invention.

[0023] Figure 2 FIG. 4 is a flow chart showing the steps of a method for degrading an ester-containing epoxy cured material composite material according to another embodiment of the present invention.

[0024]

Main component symbol description

[0025] 100: Degradation method of epoxy curing materials containing ester groups

[0026] 200: Degradation method of composite materials containing ester-based epoxy curing materials

[0027] 110,120,210,220: Steps DETAILED DESCRIPTION

[0028] The following will discuss various embodiments of the present invention in more detail. However, this embodiment can be an application of various inventive concepts and can be specifically implemented in various specific scopes. The specific embodiments are for illustrative purposes only and are not limited to the scope of the disclosure.

[0029] <Degradation Method of Ester-containing Epoxy Cured Material>

[0030] See also Figure 1 , which is a flow chart showing the steps of a method 100 for degrading an ester-containing epoxy cured product according to one embodiment of the present invention. Figure 1 In the present invention, the degradation method 100 of the epoxy cured product containing an ester group includes steps 110 and 120.

[0031] Step 110 is a mixing step, which is to mix the ester group-containing epoxy curing material with aliphatic amines to form a degradation system, and the aliphatic amines can be diamines with carbon numbers of 2 to 5 or amylamines, and diamines with carbon numbers of 2 to 5 are such as ethylenediamine, propylenediamine, butanediamine (1,4-butanediamine) or pentanediamine (1,5-pentanediamine). Specifically, the ester group in the ester group-containing epoxy curing material can refer to an ester group, a carbonate group or a urethane group.

[0032] Specifically, the ester-containing epoxy cured product can be obtained by curing an epoxy compound containing an ester structure with a hardener, wherein the ester group in the epoxy compound containing an ester structure can refer to an ester group, a carbonate group or an urethane group, and the hardener can be one or a mixture of more than one of an amine hardener, a phenol hardener, an acid anhydride hardener, and an ester hardener; or, the ester-containing epoxy cured product can be obtained by curing an epoxy compound with an acid anhydride hardener or an ester hardener, wherein the epoxy compound is a general epoxy resin, such as bisphenol A epoxy resin (DGEBA), bisphenol F epoxy resin (DGEBF), phenolic epoxy resin (PNE), cresol novolac epoxy (CNE), dicyclopentadiene-phenol epoxy resin (DNE), naphthalene-containing epoxy resin (Naphthalene-containing epoxy), phosphorus epoxy resin or a mixture thereof; or, the ester-containing epoxy cured product can also be obtained by catalyzing an ester-containing epoxy compound with an acid-base catalyst and then subjecting the epoxy compound to epoxy self-curing.

[0033] Step 120 is a degradation step, which is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy curing material, wherein the degradation temperature can be 10°C to 50°C, preferably 20°C to 40°C, so as to maintain the ester-containing epoxy curing material at a low temperature to degrade it.

[0034] <Degradation Method of Ester-containing Epoxy Cured Composite Material>

[0035] See also Figure 2 , which is a flow chart showing the steps of a method 200 for degrading an ester-containing epoxy cured material composite material according to another embodiment of the present invention. Figure 2 In the present invention, the degradation method 200 of the composite material containing ester-based epoxy cured material includes step 210 and step 220.

[0036] Step 210 is a mixing step, which is to mix the ester group-containing epoxy cured material composite material with aliphatic amines to form a degradation system, and the aliphatic amines can be diamines or pentylamines having carbon numbers of 2 to 5. Specifically, the ester group in the ester group-containing epoxy cured material composite material can refer to an ester group, a carbonate group, or a urethane group.

[0037] In detail, the ester-containing epoxy cured material composite material can be obtained by molding an ester-containing epoxy resin composition and fibers through a composite process at room temperature or high temperature, wherein the composite process includes a pultrusion process, a vacuum infusion process, a compression molding process or a prepreg molding process, but is not limited thereto; and the fibers can be glass fibers, carbon fibers, flax fibers, polyamide fibers or a mixture thereof, but is not limited thereto.

[0038] Step 220 is a degradation step, which is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured material composite material, and filter and separate the polyol oligomers and fibers. The degradation temperature can be 10°C to 50°C, preferably 20°C to 40°C, so as to maintain the ester-containing epoxy cured material composite material at a low temperature to degrade, and realize a recycling mechanism for separating fibers and organic matter.

[0039] Thus, the present invention uses a low-carbon aliphatic amine monomer as a degradation liquid, so that the ester-containing epoxy cured product is immersed in the degradation liquid and can be degraded at room temperature. The purpose of decomposing the ester-containing epoxy cured product can be achieved in a non-high temperature environment or even without energy-consuming heating, thereby solving the issues of epoxy waste recycling and energy saving and carbon reduction.

[0040] The present invention is further illustrated by the following specific embodiments, which are used to facilitate those skilled in the art to which the present invention belongs, so that they can fully utilize and practice the present invention without excessive interpretation. These embodiments should not be regarded as limiting the scope of the present invention, but are used to illustrate how to implement the materials and methods of the present invention.

[0041] <Synthesis example>

[0042] Synthesis Example 1: 2 grams of epoxy resin DPCEP2 containing an ester structure (epoxy equivalent is 483 g / eq) and 0.26 grams of hardener Jeffamine D230 (purchased from Huntsman, active hydrogen equivalent is 62 g / eq) are put into an aluminum pan and mixed evenly, and then placed in a 70°C oven for curing for 6 hours to obtain the ester-containing epoxy cured product of Synthesis Example 1.

[0043] Synthesis Example 2: Take 2 grams of epoxy resin DPCEP2 containing an ester structure (epoxy equivalent is 483g / eq), 0.69 grams of methyltetrahydrophthalic anhydride (MTHPA, purchased from Zhonghou Chemical, reaction equivalent is 166.2g / eq) and 0.004 grams (0.2wt% of epoxy resin) of 2-methylimidazole and put them into an aluminum pan and mix them evenly. Then put them in an oven at 120°C for half an hour and in an oven at 150°C for 1 hour to obtain the ester-containing epoxy cured product of Synthesis Example 2.

[0044] Synthesis Example 3: 2 grams of bisphenol A epoxy resin (from Changchun Man-Made Resins, product code BE188, epoxy equivalent of 185 g / eq), 1.80 grams of methyltetrahydrophthalic anhydride (MTHPA, purchased from Zhonghou Chemical, reaction equivalent of 166.2 g / eq) and 0.004 grams (0.2 wt% of epoxy resin) of 2-methylimidazole were put into an aluminum pan and mixed evenly, and then placed in a 120°C oven for curing for half an hour and 150°C oven for curing for 1 hour to obtain the ester-containing epoxy cured product of Synthesis Example 3.

[0045] Synthesis Example 4: 2 grams of bisphenol A epoxy resin (from Changchun Man-Made Resins, product code BE188, epoxy equivalent of 185 g / eq), 1.37 grams of polycarbonate (from Chi Mei Industrial, product code PC-122, reaction equivalent of 127 g / eq) and 0.004 grams (0.2 wt% of epoxy resin) of 2-methylimidazole were put into an aluminum pan for melt mixing, and then placed in a 175° C. oven for curing for half an hour to obtain the ester-containing epoxy cured product of Synthesis Example 4.

[0046] Synthesis Example 5: 2 grams of bisphenol A epoxy resin (from Changchun Artificial Resin, product code BE188, epoxy equivalent of 185 g / eq) and 0.67 grams of hardener Jeffamine D230 (from Huntsman, active hydrogen equivalent of 62 g / eq) were placed in an aluminum pan and mixed evenly, and then placed in a 70°C oven for curing for 6 hours to obtain the epoxy cured product of Synthesis Example 5.

[0047] Synthesis Example 6: Take 2 grams of epoxy resin DPCEP2 containing an ester structure (epoxy equivalent is 483g / eq) and 0.004 grams (0.2wt% of epoxy resin) of 2-methylimidazole and put them into an aluminum pan and mix them evenly. Then put them in an oven at 120°C for half an hour and in an oven at 150°C for 1 hour to obtain the ester-containing epoxy cured product of Synthesis Example 6.

[0048] In addition, according to different process operation requirements, the epoxy resin composition in the above-mentioned Synthesis Examples 1 to 6 can be adjusted to an appropriate gelation time for room temperature fiber impregnation molding, and then a baking process is performed according to the curing conditions described in each synthesis example to obtain an ester-containing epoxy cured material composite material containing fibers.

[0049] <Example / Comparative Example>

[0050] Examples 1 to 5: 1 gram of the ester-containing epoxy cured products of Synthesis Examples 1 to 4 and Synthesis Example 6 were taken and immersed in 10 mL of pentamethylenediamine respectively, and the degradation conditions were observed at room temperature.

[0051] Comparative Example 1: 1 gram of the epoxy cured product of Synthesis Example 5 was taken and immersed in 10 mL of pentamethylenediamine, and the degradation condition was observed at room temperature.

[0052] Comparative Example 2: 1 gram of the ester-containing epoxy curing material of Synthesis Example 1 and 10 grams of hexamethylenediamine were taken. However, hexamethylenediamine solidified at room temperature and could not be mixed smoothly. Therefore, they were placed in an oven at 60°C to melt the hexamethylenediamine, and then immersed at 60°C to observe the degradation status.

[0053] Comparative Example 3: 1 gram of the ester-containing epoxy cured product of Synthesis Example 1 was taken and immersed in 10 mL of hexylamine, and the degradation condition was observed at room temperature.

[0054] Comparative Example 4: 1 gram of the ester-containing epoxy cured product of Synthesis Example 1 was taken and immersed in 10 mL of triethylenetetramine, and the degradation condition was observed at room temperature.

[0055] Comparative Example 5: 1 gram of the ester-containing epoxy cured product of Synthesis Example 1 was taken and immersed in 10 mL of triethylenetetramine, and the degradation condition was observed at 135°C.

[0056] <Degradation Status Assessment>

[0057] The degradation temperatures, degradation times and residual weights of Examples 1 to 5 and Comparative Examples 1 to 5 are listed in Table 1 below.

[0058]

[0059] From the results in Table 1 above, it can be seen that Examples 1 to 5 can all be completely degraded by pentamethylenediamine at room temperature of 25°C, and it can be found that Examples 2 and 5, which have a higher proportion of ester groups in the epoxy cured product, have the best degradation efficiency, while Comparative Example 1, which has no ester groups in the epoxy cured product, has no significant change after being immersed in pentamethylenediamine at room temperature for 7 days.

[0060] Comparative Example 2 replaces pentamethylenediamine with hexamethylenediamine, which changes from liquid to solid at room temperature, so it is difficult to implement room temperature degradation. Therefore, after heating Comparative Example 2 to 60°C to melt it into a liquid state, it can be found that although Comparative Example 2 is immersed in a state higher than room temperature, the effect obtained by immersion for 3 days is still much inferior to that of Example 1 immersed at room temperature. In addition, Comparative Example 3 replaces hexamethylenediamine with hexamethylenediamine, which is liquid at room temperature. The degradation effect after immersion at room temperature for 7 days is not obvious, which shows that when the carbon number of the amine compound is further increased, there is a negative impact on the overall low-temperature degradation effect.

[0061] Comparative Example 4 replaces pentamethylenediamine with multifunctional triethylenetetramine. It can be found that there is no obvious breakthrough in the degradation effect at room temperature, and the result obtained after immersion for 7 days is not ideal. Comparative Example 5 is heated to 135°C, and it can be found that its degradation effect is excellent, and it can be completely degraded in about 12 hours. It is consistent with the existing technology that amine compounds have the characteristics of ester aminolysis at high temperatures, but the reactivity at low temperatures is extremely low. Even if multifunctional amines with higher alkalinity are used, it is difficult to achieve the effect of low-temperature degradation. It can be explained that the alkalinity of the amines used is not an indicator of whether it can be degraded at room temperature.

[0062] In summary, when the present invention uses a low-carbon fatty amine compound as a degradation liquid, it helps the degradation liquid to penetrate into the ester-containing epoxy cured product to a certain extent, so that the ester-containing epoxy cured product can achieve the purpose of decomposition under low temperature conditions, overcoming the technical prejudice of the prior art that a high-temperature process (>100° C.) is required for degradation, and the problem that the prior art has long wanted to solve is solved, providing a low-energy consumption recycling and reuse method for the ester-containing epoxy cured product.

[0063] Although the present invention has been disclosed in the above embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the claims.

Claims

1. A method for degrading an ester-containing epoxy cured product, characterized in that: Include: performing a mixing step of mixing the ester group-containing epoxy curing material with aliphatic amines to form a degradation system; and The degradation step is carried out by placing the degradation system at a degradation temperature to degrade the ester-containing epoxy cured product.

2. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The aliphatic amine is a diamine having 2 to 5 carbon atoms or pentylamine.

3. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester group in the ester group-containing epoxy cured product refers to an ester group, a carbonate group or a urethane group.

4. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester-containing epoxy cured product is obtained by curing an epoxy compound containing an ester structure with a hardener.

5. The method for degrading an ester group-containing epoxy cured product according to claim 4, wherein: The ester group in the epoxy compound containing an ester structure refers to an ester group, a carbonate group or a urethane group.

6. The method for degrading an ester group-containing epoxy cured product according to claim 4 or 5, characterized in that: The hardener is one of an amine hardener, a phenol hardener, an acid anhydride hardener, and an ester hardener, or a mixture of more than one of the above.

7. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester-containing epoxy cured product is obtained by curing an epoxy compound with an acid anhydride curing agent or an ester curing agent.

8. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester-containing epoxy cured product is obtained by epoxy self-curing after the epoxy compound containing the ester structure is catalyzed by an acid-base catalyst.

9. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The degradation temperature is between 10°C and 50°C.

10. A method for degrading a composite material containing an ester group epoxy cured product, characterized in that: Include: A mixing step is performed, which is to mix the ester group-containing epoxy cured material composite material with aliphatic amines to form a degradation system; as well as The degradation step is carried out, which is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured material composite material, and filter and separate the polyol oligomer and the fiber.

11. The method for degrading the composite material containing ester group epoxy cured material according to claim 10, characterized in that: The aliphatic amine is a diamine having 2 to 5 carbon atoms or pentylamine.

12. The method for degrading the composite material containing ester group epoxy cured material according to claim 10, characterized in that: The ester group in the ester group-containing epoxy cured material composite material refers to an ester group, a carbonate group or an urethane group.

13. The method for degrading the composite material containing ester group epoxy cured material according to claim 10, characterized in that: The degradation temperature is between 10°C and 50°C.