Polyimide aerogel / phase change material temperature control composite material as well as preparation method and application thereof
By using polyimide aerogel carrier and fatty alcohol conductive particles in PTC materials, the porous structure is formed, which solves the problems of collapse and leakage and temperature control during heating, and achieves excellent temperature control performance under low temperature environments and stable conductive network, suitable for the application of precision electronic components.
Patent Information
- Application Number
- CN202411154649.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-22
AI Technical Summary
During the heating process, the expansion volume of the existing PTC materials has large changes in the skeleton support material, which is difficult to support solid-liquid phase transformation, prone to collapse and leakage, and requires the control circuit to complete the temperature control needs, which cannot meet the temperature control needs in low temperature environments.
Polyimide aerogel as a carrier, loading fatty alcohols and conductive particles, and prepare polyimide aerogel/phase change material temperature-controlled composite materials by polymerization, freeze-drying and thermal imidation, and use vacuum and ultrasound to perform Adsorption, a porous structure is formed to suppress collapse and leakage, and adaptive temperature regulation is achieved through Joule heating.
Provide excellent temperature control performance in low temperature environments, prevent collapse and leakage, and maintain the stability of the conductive network. It is suitable for low-temperature thermal management of precision electronic components, and the preparation method is simple and easy to industrialize.
Smart Images

Figure CN118909437A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of temperature control composite materials, and in particular to a polyimide aerogel / phase change material temperature control composite material and a preparation method and application thereof. Background Art
[0002] In recent years, with the rapid development of aerospace, automobile transportation, household appliances and other fields, various large-scale integrated circuits have been widely used in various types of precision electronic equipment, and small size and high integration have become the development direction of various electronic components. However, the thermal expansion and thermal contraction coefficients of different device materials vary greatly. When the temperature difference between the device and the external environment is too large, it will produce large thermal stress, reduce the working performance and reliability of the device, and thus affect the working efficiency and service life of the device. In order to prevent electronic equipment components from failing in high or low temperature environments for a long time, general precision electronic equipment is required to work within the range of -15 to 50°C. Temperature control issues have gradually become the main problem restricting the development of electronic components.
[0003] PTC (Positive Temperature Coefficient) materials have broad prospects in temperature control systems in the fields of aerospace, automobile transportation, and household appliances because they can achieve adaptive temperature control without the help of control circuits. The Curie temperature of the polymer-based PTC materials currently developed is generally high (50-300°C), which is difficult to meet the temperature control requirements of electronic components in the room temperature range, and the materials are prone to problems such as decreased stability during long-term use. At present, some researchers have prepared a series of low Curie temperature polymer-based PTC materials by directly and simply blending eutectic skeleton support materials with low Curie point phase change materials such as paraffin and organic acid crystals. However, during the heating process of these materials, the eutectic skeleton support materials have the problem of large expansion volume changes. At the same time, the heated soft skeleton support material is not enough to support the phase change material undergoing solid-liquid phase change, and it is prone to collapse and leakage. Summary of the invention
[0004] The present invention provides a polyimide aerogel / phase change material temperature control composite material and a preparation method and application thereof, so as to overcome the technical problems that the existing PTC material has a large expansion volume change in the skeleton support material during the heating process and is insufficient to support the solid-liquid phase change, and is prone to collapse and leakage, and the existing Joule heating material needs to rely on a control circuit to complete temperature control in application.
[0005] In order to achieve the above object, the technical solution of the embodiment of the present invention is:
[0006] The first aspect of the present invention provides a polyimide aerogel / phase change material temperature control composite material, comprising:
[0007] A polyimide aerogel carrier, and a load loaded on the polyimide aerogel carrier, wherein the load includes a fatty alcohol and conductive particles;
[0008] The conductive particles include carbon black with a particle size of 30 nm and nickel powder with a particle size of 3 μm;
[0009] The mass ratio of the nickel powder to the carbon black is 1:0.6-1.8.
[0010] In combination with the first aspect, preferably, the polyimide aerogel carrier is prepared by polymerization, freeze-drying and thermal imidization of aromatic diamine and aromatic dianhydride.
[0011] In combination with the first aspect, preferably, the aromatic diamine is one or more of p-phenylenediamine, 3,5-diaminobenzoic acid, 2-(3-aminophenyl)-5-aminobenzimidazole, 4,4'-diaminodiphenyl ether, and 2-(4-aminophenyl)-5-aminobenzimidazole;
[0012] And / or, the aromatic dianhydride is one or more of pyromellitic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, and 4,4'-diaminodiphenyl sulfone.
[0013] In combination with the first aspect, preferably, the fatty alcohol is one or more of dodecanol, tridecanol, tetradecanol and pentadecanol.
[0014] The second aspect of the present invention provides a method for preparing the polyimide aerogel / phase change material temperature control composite material according to the first aspect, comprising:
[0015] After dissolving aromatic diamine in a polar solvent, adding aromatic dianhydride, performing heating polymerization, purifying, and collecting polyamic acid powder;
[0016] The polyamic acid powder, tertiary amine and water are mixed to obtain a polyamic acid aqueous solution, which is then freeze-dried and thermally imidized to obtain a polyimide aerogel;
[0017] The fatty alcohol and the conductive particles are heated and melted to obtain a mixture, and the polyimide aerogel is impregnated in the mixture, and adsorption is performed in a vacuum environment and under ultrasound to collect the polyimide aerogel / phase change material temperature control composite material.
[0018] In combination with the second aspect, preferably, the molar ratio of the aromatic diamine to the aromatic dianhydride is 1:1;
[0019] And / or, the mass ratio of the mixed material to the polyimide aerogel is 60-30:1.
[0020] In combination with the second aspect, preferably, the polar solvent is dimethylacetamide, and the tertiary amine is triethylamine;
[0021] And / or, the solid content of the polyamic acid aqueous solution is 1.2 wt %.
[0022] In combination with the second aspect, preferably, when the aromatic diamine is dissolved in the polar solvent, the dissolution time is 20 to 50 minutes; when the heating polymerization is performed, the polymerization time is 5 to 15 hours;
[0023] And / or, when freeze drying is performed, the freeze drying time is 48 to 96 hours;
[0024] And / or, the thermal imidization comprises: first drying at 80° C., 100° C., and 120° C. for 1 hour, and then imidizing at 200° C., 300° C., and 400° C. for 2 hours to obtain the polyimide aerogel.
[0025] In combination with the second aspect, preferably, the heating and melting time is 1 to 2 hours; the temperature of the vacuum environment is 90° C.; the ultrasonic time is 1 to 2 hours;
[0026] And / or, when the vacuum adsorption is performed, the adsorption time is 12 to 24 hours.
[0027] The third aspect of the present invention provides an application of the single polyimide aerogel / phase change material temperature control composite material described in the first aspect or the polyimide aerogel / phase change material temperature control composite material prepared by the method described in the second aspect in the preparation of low-temperature thermal management materials for precision electronic components.
[0028] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present invention include at least:
[0029] The polyimide aerogel / phase change material temperature control composite material provided by the present invention uses polyimide aerogel as a carrier, uses fatty alcohol as a phase change material and is loaded in the porous structure of the polyimide aerogel, and the fatty alcohol contains uniformly distributed carbon black and nickel powder; on the one hand, the polyimide aerogel serves as a supporting matrix of the PTC composite material, which can meet the requirements of application in harsh environments such as low temperature; on the other hand, under the action of capillary force, surface tension and hydrogen bond, the polyimide aerogel with a high surface area can effectively suppress the collapse and leakage problem caused by the phase change of the phase change material during the heating process of the PTC; thirdly, after the fatty alcohol melts and destroys the conductive network, the flow of the molten state can be suppressed, and the conductive network can be prevented from reforming and generating the NTC phenomenon; fourthly, it has the advantages of low low-temperature resistivity, stable performance and high repetition rate given by composite conductive particles of different particle sizes.
[0030] The preparation method provided by the present invention comprises the following steps: subjecting aromatic diamine and aromatic dianhydride to polymerization reaction under the condition of dissolution in a polar solvent, and then subjecting them to purification treatment to obtain polyamic acid powder; then, mixing the polyamic acid powder and a tertiary amine in water to obtain a polyamic acid solution, and then subjecting the polyamic acid solution to freeze-drying and thermal imidization to obtain a polyimide aerogel; then, heating and melting fatty alcohol and conductive particles to obtain a mixture, and impregnating the polyimide aerogel into the mixture, and subjecting the mixture to adsorption under vacuum and ultrasound so that the mixture can be fully adsorbed into the three-dimensional porous structure of the polyimide aerogel, and collecting the polyimide aerogel / phase change material temperature control composite material. On the one hand, polyimide aerogel, as the supporting matrix of PTC composite materials, can meet the application requirements in harsh environments such as low temperature; on the other hand, under the action of capillary force, surface tension and hydrogen bond, polyimide aerogel with a high surface area can effectively suppress the collapse and leakage problem caused by the phase change of phase change materials during the heating process of PTC; thirdly, after the fatty alcohol melts and destroys the conductive network, it can suppress the flow of the molten state, and prevent the conductive network from reforming and producing the NTC phenomenon; fourthly, it also has the lower low-temperature resistivity, stable performance and high repetition rate given by composite conductive particles of different particle sizes; fifthly, compared with the traditional single vacuum negative pressure adsorption, ultrasonic adsorption can prevent the high-viscosity mixture particles from aggregating and blocking the aerogel pores to affect the adsorption efficiency. The mechanical vibration of the ultrasonic wave can effectively disperse the particles and increase the adsorption effect through the acoustic cavitation effect and tunnel effect, making the overall structure tighter.
[0031] The polyimide aerogel / phase change material temperature control composite material provided by the present invention has, on the one hand, excellent temperature control performance under vacuum and low temperature conditions, and is expected to be used as a low-temperature thermal management material for precision electronic components; on the other hand, its preparation method is simple, the raw materials are readily available, and it is easy to carry out large-scale industrial production.
[0032] In addition, on the one hand, most of the existing low Curie temperature polymer-based PTC temperature control materials are prepared by blending low Curie temperature phase change materials with polymer-based skeleton support materials, and packaging strategies combined with porous materials have not yet been considered. On the other hand, unlike the temperature control materials of porous materials adsorbing phase change core materials, which complete passive temperature regulation by absorbing or releasing latent heat during the phase change process of the phase change core materials, the polyimide aerogel / phase change material temperature control composite material of the present invention achieves active self-control temperature regulation through adaptive Joule heating. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a microscopic morphology of the polyimide aerogel / phase change material temperature control composite material prepared in Example 5;
[0034] Figure 2 This is the thermal analysis spectrum of the polyimide aerogel / phase change material temperature control composite material prepared in Example 1;
[0035] Figure 3 The temperature-resistivity diagram of the polyimide aerogel / phase change material temperature control composite material prepared in Example 5;
[0036] Figure 4 This is a temperature-resistivity cycle diagram of the polyimide aerogel / phase change material temperature control composite material prepared in Example 5;
[0037] Figure 5 This is a temperature control diagram of the polyimide aerogel / phase change material temperature control composite material prepared in Example 5 under a vacuum environment. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings. The described embodiments should not be regarded as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0039] In the following description, reference is made to "some embodiments", which describe a subset of all possible embodiments, but it is understood that "some embodiments" may be the same subset or different subsets of all possible embodiments, and may be combined with each other without conflict. Unless otherwise defined, all technical and scientific terms used in the embodiments of the present invention have the same meaning as those commonly understood by those skilled in the art to which the embodiments of the present invention pertain. The terms used in the embodiments of the present invention are only for the purpose of describing the embodiments of the present invention and are not intended to limit the present invention.
[0040] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0041] It should be noted that all raw materials / reagents in the embodiments of the present invention can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; the term "and / or" in the embodiments of the present invention is only used to describe the association relationship between associated objects, indicating that three relationships may exist, for example, A and / or B means the existence of A alone, B alone, and A and B at the same time, wherein A and B can be singular or plural, and the character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0042] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0043] Those skilled in the art should understand that in the following description of the embodiments of the present invention, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.
[0044] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "an" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0045] It will be appreciated by those skilled in the art that the numerical ranges in the embodiments of the present invention are to be understood as also specifically disclosing each intermediate value between the upper and lower limits of the range. Each smaller range between the intermediate values in any stated value and stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0046] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the embodiments or test cases of the present invention. All documents mentioned in this specification are generally incorporated by reference to disclose and describe methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of the present invention shall prevail.
[0047] It should be noted that all raw materials and / or reagents in the examples of the present invention are purchased on the market or prepared according to conventional methods well known to those skilled in the art.
[0048] In a first aspect, an embodiment of the present invention provides a polyimide aerogel / phase change material temperature control composite material, comprising:
[0049] A polyimide aerogel carrier, and a load loaded on the polyimide aerogel carrier, wherein the load includes a fatty alcohol and conductive particles;
[0050] The conductive particles include carbon black with a particle size of 30 nm and nickel powder with a particle size of 3 μm;
[0051] The mass ratio of the nickel powder to the carbon black is 1:0.6-1.8.
[0052] It should be noted that the fatty alcohol contains uniformly distributed conductive particles.
[0053] The polyimide aerogel / phase change material temperature control composite material provided by the present invention uses polyimide aerogel as a carrier, uses fatty alcohol as a phase change material and is loaded in the porous structure of the polyimide aerogel, and the fatty alcohol contains uniformly distributed carbon black and nickel powder; on the one hand, the polyimide aerogel is used as a supporting matrix of the PTC composite material, which can meet the requirements of application in harsh environments such as low temperature; on the other hand, under the action of capillary force, surface tension and hydrogen bonding, the polyimide aerogel with a high surface area can effectively suppress the collapse and leakage problem caused by the phase change of the phase change material during the heating process of the PTC; Thirdly, after the fatty alcohol melts and destroys the conductive network, it can inhibit the flow of the molten state, prevent the conductive network from reforming and producing the NTC phenomenon; fourthly, it also has the lower low-temperature resistivity, stable performance and high repetition rate given by the composite conductive particles of different particle sizes; fifthly, compared with the traditional single vacuum negative pressure adsorption, ultrasonic adsorption can prevent the high-viscosity mixture particles from aggregating and blocking the aerogel pores to affect the adsorption efficiency. The mechanical vibration of the ultrasonic wave can effectively disperse the particles and increase the adsorption effect through the acoustic cavitation effect and tunnel effect, and the overall structure is tighter.
[0054] In practical applications, polyimide aerogel has become one of the most popular materials in the field of special engineering polymers due to its excellent mechanical properties, high temperature resistance, extremely low temperature resistance, corrosion resistance and high porosity.
[0055] In the present invention, polyimide aerogel can provide a skeleton with high supporting strength for the PTC material, and its high and low temperature resistance and corrosion resistance can also give the PTC material extremely high environmental adaptability. The high porosity can provide more surface area for adsorbing phase change materials and conductive particles, providing more capillary force, surface tension and hydrogen bonding force for the phase change material.
[0056] In a specific embodiment, the polyimide aerogel carrier in the embodiment of the present invention is preferably prepared by polymerization, freeze drying and thermal imidization of aromatic diamine and aromatic dianhydride.
[0057] In a specific embodiment, the aromatic diamine in the embodiment of the present invention is preferably one of p-phenylenediamine, 3,5-diaminobenzoic acid, 2-(3-aminophenyl)-5-aminobenzimidazole, 4,4'-diaminodiphenyl ether, and 2-(4-aminophenyl)-5-aminobenzimidazole.
[0058] In a specific embodiment, the aromatic dianhydride in the embodiment of the present invention is preferably one of pyromellitic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, and 4,4'-diaminodiphenyl sulfone.
[0059] In a specific embodiment, the fatty alcohol in the embodiment of the present invention is preferably one of dodecanol, tridecanol, tetradecanol, and pentadecanol; further, tetradecanol is more preferred. In the present application, the fatty alcohol plays the role of a phase change material.
[0060] In a second aspect, an embodiment of the present invention provides a method for preparing a polyimide aerogel / phase change material temperature control composite material, comprising:
[0061] S10: After dissolving aromatic diamine in a polar solvent, aromatic dianhydride is added, and heating polymerization and purification are performed, and then polyamic acid powder is collected.
[0062] S20: After the polyamic acid powder, tertiary amine and water are mixed, a polyamic acid aqueous solution is obtained, and then freeze-dried and thermally imidized to obtain a polyimide aerogel.
[0063] S30: heating and melting the fatty alcohol and the conductive particles to obtain a mixture, impregnating the polyimide aerogel into the mixture, adsorbing the mixture under vacuum and ultrasound, and collecting the polyimide aerogel / phase change material temperature control composite material.
[0064] In step S1 of the preparation method provided by the present invention, there is no limitation on the specific implementation method of dissolving, for example, the dissolving can be carried out under heating conditions or under stirring conditions, as long as the aromatic diamine and the polar solvent are dissolved uniformly. There is no particular limitation on stirring in the present invention, for example, mechanical stirring can be used, and generally, preferably, in order to make the reaction more complete, the stirring reaction is continued for a period of time after the addition is completed.
[0065] In step S1 of the preparation method provided by the present invention, there is no limitation on the specific implementation method of the polymerization. For example, the polymerization can be carried out under heating conditions or at room temperature, as long as the aromatic diamine and the aromatic dianhydride can be polymerized to obtain polyamic acid.
[0066] In step S1 of the preparation method provided by the present invention, there is no limitation on the specific implementation method of purification. For example, the reaction product of the aromatic diamine and the aromatic dianhydride may be subjected to multiple washing, centrifugation, drying and other treatments. The reaction product may be washed with deionized water, ethanol, methanol and other solvents; the drying may be performed at high temperature or in a frozen environment.
[0067] The present invention preferably mixes and dissolves the polar solvent and aromatic diamine under stirring at room temperature, then adds aromatic dianhydride, heats in a water bath and stirs to polymerize to obtain a solution to make the reaction more uniform, drips the solution dropwise into deionized water, grinds, washes and dries the precipitated powder to obtain polyamic acid powder.
[0068] The preparation method provided by the present invention comprises the following steps: compounding aromatic diamine and aromatic dianhydride under the condition of dissolving in a polar solvent, subjecting the aromatic diamine and aromatic dianhydride to polymerization reaction and purification treatment to obtain polyamic acid powder; then, mixing the polyamic acid powder and tertiary amine in water to obtain a polyamic acid solution, freeze-drying and thermal imidization to obtain a polyimide aerogel; then, heating and melting fatty alcohol and conductive particles to obtain a mixture, impregnating the polyimide aerogel in the mixture, adsorbing under vacuum and ultrasound so that the mixture can be fully adsorbed into the three-dimensional porous structure of the polyimide aerogel, and collecting the polyimide aerogel / phase change material temperature control composite material. On the one hand, polyimide aerogel, as the supporting matrix of PTC composite materials, can meet the application requirements in harsh environments such as low temperature; on the other hand, under the action of capillary force, surface tension and hydrogen bond, polyimide aerogel with a high surface area can effectively suppress the collapse and leakage caused by the phase change of phase change materials during the heating process of PTC; thirdly, after the fatty alcohol melts and destroys the conductive network, it can suppress the flow of the molten state, which can prevent the conductive network from reforming and producing the NTC phenomenon; fourthly, it also has the lower low-temperature resistivity, stable performance and high repetition rate given by composite conductive particles of different particle sizes; fifthly, compared with the traditional single vacuum negative pressure adsorption, ultrasonic adsorption can prevent the high-viscosity mixture particles from aggregating and blocking the aerogel pores to affect the adsorption efficiency. The mechanical vibration of the ultrasonic wave can effectively disperse the particles and increase the adsorption effect through the acoustic cavitation effect and tunnel effect, and the overall structure is tighter.
[0069] In a specific embodiment, the molar ratio of the aromatic diamine to the aromatic dianhydride in the embodiment of the present invention is preferably 1:1.
[0070] In a specific embodiment, the mass ratio of the mixed material to the polyimide aerogel in the embodiment of the present invention is preferably 60-30:1.
[0071] In a specific embodiment, the polar solvent in the embodiment of the present invention is preferably dimethylacetamide, and the tertiary amine is preferably triethylamine.
[0072] In a specific embodiment, the solid content of the polyamic acid aqueous solution in the embodiment of the present invention is preferably 1.2 wt %.
[0073] In a specific embodiment, when the aromatic diamine is dissolved in a polar solvent, the dissolution time is preferably 20 to 50 minutes; when the heating polymerization is performed, the polymerization time is preferably 5 to 15 hours.
[0074] In a specific embodiment, when freeze drying is performed in the embodiment of the present invention, the freeze drying time is preferably 48 to 96 hours.
[0075] In a specific embodiment, the thermal imidization in the embodiment of the present invention includes: first drying at 80°C, 100°C, and 120°C for 1 hour, and then imidizing at 200°C, 300°C, and 400°C for 2 hours to obtain a polyimide aerogel.
[0076] In a specific embodiment, the heating and melting time in the embodiment of the present invention is preferably 1 to 2 hours; the temperature of the vacuum environment is preferably 90° C.; and the ultrasonic time is preferably 1 to 2 hours.
[0077] In a specific embodiment, when vacuum adsorption is performed in the embodiment of the present invention, the adsorption time is preferably 12 to 24 hours.
[0078] In a third aspect, an embodiment of the present invention provides an application of the polyimide aerogel / phase change material temperature control composite material described in the first aspect or the polyimide aerogel / phase change material temperature control composite material prepared by the method described in the second aspect in the preparation of low-temperature thermal management materials for precision electronic components.
[0079] The polyimide aerogel / phase change material temperature control composite material provided by the present invention has, on the one hand, excellent temperature control performance under vacuum and low temperature conditions, and can be expected to be used as a low-temperature thermal management material for precision electronic components; on the other hand, its preparation method is simple, the raw materials are easily available, and it is easy to carry out large-scale industrial production.
[0080] The technical method of the present invention will be further described below in conjunction with specific embodiments.
[0081] Examples 1-8
[0082] This embodiment provides a method for preparing a polyimide aerogel / phase change material temperature control composite material 1-8, and the specific steps are as follows:
[0083] (1) After dissolving aromatic diamine in a polar solvent, adding aromatic dianhydride, polymerizing and purifying, and collecting polyamic acid powder:
[0084] 22.43g (0.1mol) of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 724g of N,N-dimethylacetamide solution at room temperature and stirred at 400rpm for 30min. Next, 29.42g (0.1mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was dissolved in the solution and stirred for 10h under nitrogen atmosphere and room temperature to obtain a polyamic acid solution. The polyamic acid solution was dripped dropwise in deionized water, the precipitated powder was ground and washed three times in deionized water and ethanol and dried at 80°C for 12h to obtain a polyamic acid powder.
[0085] (2) After the polyamic acid powder, tertiary amine and water are mixed, a polyamic acid aqueous solution is obtained, followed by freeze drying and thermal imidization to obtain a polyimide aerogel:
[0086] The polyamic acid powder was dissolved in an aqueous solution of triethylamine to obtain a polyamic acid salt solution with a solid content of 1.2%. The prepared polyamic acid salt was injected into a mold, the temperature was set to -50°C and the sample was frozen for 30 minutes. After the mold was inverted, the sample was placed in a vacuum freeze dryer and kept at -30°C and a pressure of less than 10Pa for 72 hours. Next, the sample was placed in a vacuum oven and imidized at 200°C, 300°C and 400°C for 2 hours each to obtain a polyimide aerogel.
[0087] (3) After the fatty alcohol and the conductive particles are heated and melted, a mixture is obtained, and the polyimide aerogel is impregnated in the mixture, and adsorption is performed under vacuum and ultrasound to collect the polyimide aerogel / phase change material temperature control composite material:
[0088] 20g of fatty alcohol was heated and melted at 70°C, 2.4-3.6g of carbon black and 2.0-4.0g of nickel were slowly added, and mechanical stirring was performed at 300rpm for 1h to obtain a mixture. Subsequently, the polyimide aerogel was immersed in the molten mixture, adsorbed in a vacuum oven at 90°C for 12h, and adsorbed in ultrasound at 70°C for 2h. The mixture was fully adsorbed into the three-dimensional pores of the aerogel, and cooled to room temperature to obtain a polyimide aerogel / phase change material temperature control composite material.
[0089] The polyimide aerogel / phase change material temperature control composite materials of Examples 1-8 were prepared in the same manner as above, as shown in Table 1. Table 1 shows the component conditions, low temperature resistivity, Curie temperature, PTC strength (P = Lg (ρ max / ρ min ), ρ max is the maximum resistivity of the material, ρ minis the minimum resistivity of the material) and whether there is collapse and leakage (80℃, PTC is in good condition, no collapse and leakage is √; collapse and leakage is ×).
[0090] Table 1
[0091]
[0092]
[0093] Comparative Examples 1-3
[0094] This comparative example 1-3 provides a method for preparing a single conductive particle carbon black system polyimide aerogel / tetradecanol temperature control composite material, and the specific steps are as follows:
[0095] (1) After dissolving aromatic diamine in a polar solvent, adding aromatic dianhydride, polymerizing and purifying, and collecting polyamic acid powder:
[0096] 22.43g (0.1mol) of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 724g of N,N-dimethylacetamide solution at room temperature and stirred at 400rpm for 30min. Next, 29.42g (0.1mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was dissolved in the solution and stirred for 10h under nitrogen atmosphere and room temperature to obtain a polyamic acid solution. The polyamic acid solution was dripped dropwise in deionized water, the precipitated powder was ground and washed three times in deionized water and ethanol and dried at 80°C for 12h to obtain a polyamic acid powder.
[0097] (2) After the polyamic acid powder, tertiary amine and water are mixed, a polyamic acid aqueous solution is obtained, followed by freeze drying and thermal imidization to obtain a polyimide aerogel:
[0098] The polyamic acid powder was dissolved in an aqueous solution of triethylamine to obtain a polyamic acid salt solution with a solid content of 1.2%. The prepared polyamic acid salt was injected into a mold, the temperature was set to -50°C and the sample was frozen for 30 minutes. After the mold was inverted, the sample was placed in a vacuum freeze dryer and kept at -30°C and a pressure of less than 10Pa for 72 hours. Next, the sample was placed in a vacuum oven and imidized at 200°C, 300°C and 400°C for 2 hours each to obtain a polyimide aerogel.
[0099] (3) Preparation of polyimide aerogel / phase change material temperature control composite materials with single conductive particle carbon black system:
[0100] 20g of tetradecanol was heated and melted at 70°C, 2.4-3.6g of carbon black was slowly added, and mechanical stirring was performed at 300rpm for 1h to obtain a mixture. Subsequently, the aerogel was immersed in the molten mixture, adsorbed in a vacuum oven at 90°C for 12h, and adsorbed in ultrasound at 70°C for 2h. The mixture was fully adsorbed into the three-dimensional pores of the aerogel. When it was cooled to room temperature, a single conductive particle carbon black system polyimide aerogel / tetradecanol temperature-controlled composite material was obtained.
[0101] Table 2 is a comparison table of the component conditions, low-temperature resistivity, Curie temperature, PTC strength and collapse and leakage of the single conductive particle carbon black system polyimide aerogel / tetradecanol temperature control composite materials of comparative examples 1-3.
[0102] Table 2
[0103]
[0104] Comparative Examples 4-6
[0105] Comparative Examples 4-6 provide a method for preparing a single conductive particle nickel powder system polyimide aerogel / tetradecanol temperature control composite material, and the specific steps are as follows:
[0106] (1) After dissolving aromatic diamine in a polar solvent, adding aromatic dianhydride, polymerizing and purifying, and collecting polyamic acid powder:
[0107] 22.43g (0.1mol) of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 724g of N,N-dimethylacetamide solution at room temperature and stirred at 400rpm for 30min. Next, 29.42g (0.1mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was dissolved in the solution and stirred for 10h under nitrogen atmosphere and room temperature to obtain a polyamic acid solution. The polyamic acid solution was dripped dropwise in deionized water, the precipitated powder was ground and washed three times in deionized water and ethanol and dried at 80°C for 12h to obtain a polyamic acid powder.
[0108] (2) After the polyamic acid powder, tertiary amine and water are mixed, a polyamic acid aqueous solution is obtained, followed by freeze drying and thermal imidization to obtain a polyimide aerogel:
[0109] The polyamic acid powder was dissolved in an aqueous solution of triethylamine to obtain a polyamic acid salt solution with a solid content of 1.2%. The prepared polyamic acid salt was injected into a mold, the temperature was set to -50°C and the sample was frozen for 30 minutes. After the mold was inverted, the sample was placed in a vacuum freeze dryer and kept at -30°C and a pressure of less than 10Pa for 72 hours. Next, the sample was placed in a vacuum oven and imidized at 200°C, 300°C and 400°C for 2 hours each to obtain a polyimide aerogel.
[0110] (3) Preparation of polyimide aerogel / tetradecanol temperature control composite materials with single conductive particle nickel powder system:
[0111] 20g of tetradecanol was heated and melted at 70°C, 5-20g of nickel powder was slowly added, and mechanical stirring was performed at 300rpm for 1h to obtain a mixture. Subsequently, the aerogel was immersed in the molten mixture, adsorbed in a vacuum oven at 90°C for 12h, and adsorbed in ultrasound at 70°C for 2h. The mixture was fully adsorbed into the three-dimensional pores of the aerogel. When it was cooled to room temperature, a single conductive particle nickel powder system polyimide aerogel / tetradecanol temperature-controlled composite material was obtained.
[0112] Table 3 is a comparison table of the component conditions, low-temperature resistivity, Curie temperature, PTC strength and collapse and leakage of the single conductive particle nickel powder system polyimide aerogel / tetradecanol temperature control composite material of comparative examples 4-6.
[0113] Table 3
[0114]
[0115] Comparative Examples 7-9
[0116] This comparative example 7-9 provides a method for preparing a single conductive particle carbon black system polyimide aerogel / paraffin temperature control composite material, and the specific steps are as follows:
[0117] (1) After dissolving aromatic diamine in a polar solvent, adding aromatic dianhydride, polymerizing and purifying, and collecting polyamic acid powder:
[0118] 22.43g (0.1mol) of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 724g of N,N-dimethylacetamide solution at room temperature and stirred at 400rpm for 30min. Next, 29.42g (0.1mol) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was dissolved in the solution and stirred for 10h under nitrogen atmosphere and room temperature to obtain a polyamic acid solution. The polyamic acid solution was dripped dropwise in deionized water, the precipitated powder was ground and washed three times in deionized water and ethanol and dried at 80°C for 12h to obtain a polyamic acid powder.
[0119] (2) After the polyamic acid powder, tertiary amine and water are mixed, a polyamic acid aqueous solution is obtained, followed by freeze drying and thermal imidization to obtain a polyimide aerogel:
[0120] The polyamic acid powder was dissolved in an aqueous solution of triethylamine to obtain a polyamic acid salt solution with a solid content of 1.2%. The prepared polyamic acid salt was injected into a mold, the temperature was set to -50°C and the sample was frozen for 30 minutes. After the mold was inverted, the sample was placed in a vacuum freeze dryer and kept at -30°C and a pressure of less than 10Pa for 72 hours. Next, the sample was placed in a vacuum oven and imidized at 200°C, 300°C and 400°C for 2 hours each to obtain a polyimide aerogel.
[0121] (3) Preparation of polyimide aerogel / paraffin temperature control composite materials with single conductive particle carbon black system:
[0122] 20g paraffin was heated and melted at 70°C, 2.4-3.6g carbon black was slowly added, and mechanical stirring was performed at 300rpm for 1h to obtain a mixture. Subsequently, the aerogel was immersed in the molten mixture, and adsorbed in a vacuum oven at 90°C for 12h, and adsorbed in ultrasound at 70°C for 2h. The mixture was fully adsorbed into the three-dimensional pores of the aerogel. When it was cooled to room temperature, a single conductive particle carbon black system polyimide aerogel / paraffin temperature control composite material was obtained.
[0123] Table 4 is a comparison table of the component conditions, low-temperature resistivity, Curie temperature, PTC strength and collapse and leakage of the single conductive particle carbon black system polyimide aerogel / paraffin temperature control composite materials of Comparative Examples 7-9.
[0124] Table 4
[0125]
[0126] Comparative Examples 10-12
[0127] Comparative Examples 10-12 provide a composite material that is not encapsulated with polyimide aerogel, and the specific steps are as follows:
[0128] 20 g of fatty alcohol was heated and melted at 70° C., 2.4-3.6 g of carbon black was slowly added, and mechanically stirred at 300 rpm for 1 hour to obtain a mixture, which was poured into a mold and cooled to room temperature to obtain a composite material without polyimide aerogel encapsulation.
[0129] Table 5 provides a comparison table of component conditions, low temperature resistivity, Curie temperature, PTC strength and collapse and leakage of composite materials not encapsulated with polyimide aerogel for comparative examples 10-12.
[0130] Table 5
[0131]
[0132] As can be seen from Table 1 above, Examples 1-5 verify that when the fatty alcohol is tetradecanol, the optimal comprehensive performance of the low-temperature resistivity, Curie temperature, and PTC strength of the polyimide aerogel / phase change material temperature control composite material is optimal, and the optimal mass ratio of carbon black and nickel powder is 1:1.8. The mass fraction of carbon black in fatty alcohol is 12%, 15%, and 18%, and the mass fraction of nickel powder in fatty alcohol is 10% and 20%. Among them, the carbon black with a mass fraction of 18% fatty alcohol and the nickel powder with a mass fraction of 20% fatty alcohol are difficult to fully adsorb due to the excessive viscosity of the system. At the optimal mass ratio of 1:1.8, the low-temperature resistivity of the polyimide aerogel / phase change material temperature control composite material is optimally 0.77Ω*m, the Curie temperature is optimally 34°C, and the PTC strength is optimally 3.41. When the mass ratio of carbon black and nickel powder is 1:1.8, the comprehensive performance of the polyimide aerogel / phase change material temperature control composite material with fatty alcohols being dodecanol, tridecanol, and pentadecanol is verified. It can be seen that when the fatty alcohol is tetradecanol, the effect is the best. The reason is that the conductive filler has the best compatibility with tetradecanol and the interface interaction is the strongest.
[0133] As can be seen from Table 2, Comparative Examples 1-3 verify the component conditions, low-temperature resistivity, Curie temperature, and PTC strength of the single conductive particle carbon black system polyimide aerogel / tetradecanol temperature control composite material. When the carbon black is 3.6g, the comprehensive effect is optimal, the low-temperature resistivity is optimal at 1.42Ω*m, the Curie temperature is optimal at 34°C, and the PTC strength is optimal at 3.07. Comparative Example 5 has an optimal mass ratio of carbon black and nickel powder of 1:1.8, with a low-temperature resistivity of 0.77Ω*m and a PTC strength of 3.41. Its low-temperature resistivity is higher and its PTC strength is lower. This shows that the introduction of composite conductive particles of different particle sizes adds new conductive network connection points. At the same time, the conductive network is more easily destroyed during the phase change process. The composite material has a lower low-temperature resistivity and a higher PTC strength.
[0134] As can be seen from Table 3, Comparative Examples 4-6 verify the component conditions, low-temperature resistivity, Curie temperature, and PTC strength of the single conductive particle nickel powder system polyimide aerogel / tetradecanol temperature control composite material. When the nickel powder is 10g, the comprehensive effect is optimal, the low-temperature resistivity is optimal at 3.90Ω*m, the Curie temperature is optimal at 34°C, and the PTC strength is optimal at 2.32. Compared with the low-temperature resistivity of 0.77Ω*m and the PTC strength of 3.41 of the optimal mass ratio of carbon black and nickel powder of 1:1.8 in Example 5, its low-temperature resistivity is high and the PTC strength is low. This once again verifies that the introduction of composite conductive particles of different particle sizes adds new conductive network connection points, and the conductive network is more easily destroyed during the phase change process. The composite material has a lower low-temperature resistivity and a higher PTC strength.
[0135] As can be seen from Table 4, Comparative Examples 7-9 verify that when the phase change material is paraffin, the overall effect is optimal when the carbon black is 3.6g, the optimal low-temperature resistivity is 3.27Ω*m, the optimal Curie temperature is 47°C, and the optimal PTC strength is 1.97. Compared with the fatty alcohol system, the effect is poor. The composite material whose phase change material is a fatty alcohol system has a lower low-temperature resistivity and a higher PTC strength. This is because the conductive filler has better wettability in tetradecanol and is more evenly dispersed than in paraffin, so it has a better initial conductivity. At the same time, tetradecanol has a higher phase change resistance, and the phase change has a greater degree of damage to the tetradecanol crystallization, and the conductive network is more easily destroyed. The tetradecanol system has a higher PTC strength.
[0136] As can be seen from Table 5, Comparative Examples 10-12 verify that the composite material without polyimide aerogel encapsulation has collapsed. Under the action of capillary force, surface tension and hydrogen bonding, polyimide aerogel with a high surface area can effectively suppress the collapse and leakage caused by the softening of the PTC matrix and the phase change of the phase change material during heating.
[0137] As shown in Tables 1-4 above, compared with Comparative Examples 1-6, the introduction of compound conductive particles in Examples 1-8 makes the composite material have lower low-temperature resistivity and higher PTC strength. Compared with Comparative Examples 7-9, Comparative Examples 1-3 show that the composite material in which the phase change material is a paraffin system has lower low-temperature resistivity and higher PTC strength than the system in which the phase change material is a fatty alcohol system. Compared with Comparative Examples 10-11, under the action of capillary force, surface tension and hydrogen bonding, polyimide aerogel with a high surface area can effectively inhibit the collapse and leakage caused by the softening of the PTC matrix and the phase change of the phase change material during heating.
[0138] In order to verify the technical effect of the present application, the performance of the polyimide aerogel / phase change material temperature control composite material of the embodiment was analyzed. The results are as follows Figure 1-5 shown. Figure 1This is a microscopic morphology of the polyimide aerogel / phase change material temperature control composite material of Example 5. Figure 2 This is the DSC graph of the polyimide aerogel / phase change material temperature control composite material of Example 1. Figure 3 This is the temperature-resistivity diagram of the polyimide aerogel / phase change material temperature control composite material of Example 5. Figure 4 This is the temperature-resistivity cycle diagram of the polyimide aerogel / phase change material temperature control composite material of Example 5. Figure 5 This is a temperature control diagram of the polyimide aerogel / phase change material temperature control composite material in Example 5 under a vacuum environment.
[0139] according to Figure 1 It can be seen that the morphology and structure of the prepared polyimide aerogel / phase change material temperature control composite material. The polyimide aerogel exhibits a three-dimensional structure with tubular pores, which is caused by the unidirectional freezing method. The fatty alcohol and conductive particles fill the pores of the aerogel, showing the characteristics of complete adsorption. No obvious interface between the aerogel and the phase change material is observed, indicating that the high surface area polyimide aerogel and the phase change material have good compatibility, which is due to the capillary force, surface tension and hydrogen bonding force between them.
[0140] according to Figure 2 It can be seen that when the sample is heated from -20℃ to 80℃ at a heating rate of 5℃ / min, the horizontal coordinates of several main characteristic points such as the change trend, starting point and peak temperature point of the two curves are almost equal, which shows that the phase change temperature and phase change range of the PTC composite material depend on the phase change material used to prepare the PTC composite material. The Curie temperature of tetradecanol is about 34℃ and the melting point is 39.4℃, while the Curie temperature of the PTC composite material is about 34℃ and the melting point is 38.9℃.
[0141] according to Figure 3 It can be seen that in a programmable constant temperature and humidity test box, a temperature rise and fall experiment is carried out. During the temperature rise process, when the sample temperature is near the Curie temperature, the resistivity increases sharply and reaches a peak. This characteristic is due to the fact that the fourteen alcohol phase change matrix of the PTC composite material absorbs heat and rises to the Curie temperature to undergo a phase change, destroying the conductive network of the material. Embodiments 1-9 have lower low-temperature resistivity, low Curie temperature and high PTC strength. During the cooling process, there is a deviation between the curve and the heating curve, the phase change material is overcold, and there is a difference between the crystallization temperature and the melting temperature. Before cooling to the crystallization temperature, the phase change material is still in a molten state. When the crystallization temperature is reached, the fourteen alcohol solidifies and crystallizes, and the conductive network begins to recover to the initial resistance value.
[0142] according to Figure 4It can be seen that in 50 cycles of heating and cooling, the low-temperature resistivity of the prepared polyimide aerogel / phase change material temperature control composite material was maintained between 1.50-1.61Ω*m, and the PTC strength decreased from 3.53 to 3.25, with excellent cycle stability. This is attributed to the capillary force, surface tension and hydrogen bonding force between the aerogel and tetradecanol. In the molten state, tetradecanol will not flow, its position will not change, and it has stability.
[0143] according to Figure 5 It can be seen that the homemade vacuum box is placed in a programmable constant temperature and humidity test chamber at -20℃ to simulate the working environment of spacecraft electronic components, and a 5mm thick aluminum block is loaded on the PTC surface for device temperature control test. In a non-adiabatic environment where only thermal radiation is considered, in the first few minutes of power-on, the heat generation is greater than the heat dissipation (thermal radiation), and the temperature of the composite material rises rapidly. After heating for a period of time, it reaches the Curie temperature of tetradecanol. At this time, the internal conductive network is destroyed, the short circuit is formed, and heat generation cannot continue. The heat generation is equivalent to the heat dissipation, and the thermal equilibrium state is reached. As the applied voltage increases, the temperature at which the composite material reaches the thermal equilibrium state gradually increases, but it is still below 34℃, which fully demonstrates the application potential of PTC composite materials in the field of temperature control of spacecraft electronic components.
[0144] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A polyimide aerogel / phase change material temperature control composite material, It is characterized in that include: A polyimide aerogel carrier, and a load loaded on the polyimide aerogel carrier, wherein the load includes a fatty alcohol and conductive particles; The conductive particles include carbon black with a particle size of 30 nm and nickel powder with a particle size of 3 μm; The mass ratio of the nickel powder to the carbon black is 1:0.6-1.
8.
2. The polyimide aerogel / phase change material temperature control composite material according to claim 1, It is characterized in that The polyimide aerogel carrier is prepared by polymerization, freeze drying and thermal imidization of aromatic diamine and aromatic dianhydride.
3. The polyimide aerogel / phase change material temperature control composite material according to claim 2, It is characterized in that The aromatic diamine is one or more of p-phenylenediamine, 3,5-diaminobenzoic acid, 2-(3-aminophenyl)-5-aminobenzimidazole, 4,4'-diaminodiphenyl ether, and 2-(4-aminophenyl)-5-aminobenzimidazole; And / or, the aromatic dianhydride is one or more of pyromellitic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, and 4,4'-diaminodiphenyl sulfone.
4. The polyimide aerogel / phase change material temperature control composite material according to claim 1, It is characterized in that The fatty alcohols are one or more of dodecanol, tridecanol, tetradecanol and pentadecanol.
5. A method for preparing the polyimide aerogel / phase change material temperature control composite material according to any one of claims 1 to 4, It is characterized in that include: After dissolving aromatic diamine in a polar solvent, adding aromatic dianhydride, polymerizing and purifying, collecting polyamic acid powder; The polyamic acid powder, tertiary amine and water are mixed to obtain a polyamic acid aqueous solution, which is then freeze-dried and thermally imidized to obtain a polyimide aerogel; The fatty alcohol and the conductive particles are heated and melted to obtain a mixture, and the polyimide aerogel is impregnated in the mixture, and adsorption is performed in a vacuum environment and under ultrasound to collect the polyimide aerogel / phase change material temperature control composite material.
6. The polyimide aerogel / phase change material temperature control composite material according to claim 5, It is characterized in that The molar ratio of the aromatic diamine to the aromatic dianhydride is 1:1; And / or, the mass ratio of the mixed material to the polyimide aerogel is 60-30:
1.
7. The method for preparing the polyimide aerogel / phase change material temperature control composite material according to claim 5, It is characterized in that The polar solvent is dimethylacetamide, and the tertiary amine is triethylamine; And / or, the solid content of the polyamic acid aqueous solution is 1.2 wt %.
8. The method for preparing the polyimide aerogel / phase change material temperature control composite material according to claim 5, It is characterized in that When the aromatic diamine is dissolved in the polar solvent, the dissolution time is 20 to 50 minutes; when the heating polymerization is performed, the polymerization time is 5 to 15 hours; And / or, when freeze drying is performed, the freeze drying time is 48 to 96 hours; And / or, the thermal imidization comprises: first drying at 80° C., 100° C., and 120° C. for 1 hour, and then imidizing at 200° C., 300° C., and 400° C. for 2 hours to obtain the polyimide aerogel.
9. The method for preparing the polyimide aerogel / phase change material temperature control composite material according to claim 5, It is characterized in that The heating and melting time is 1 to 2 hours; the temperature of the vacuum environment is 90° C.; the ultrasonic time is 1 to 2 hours; And / or, when the vacuum adsorption is performed, the adsorption time is 12 to 24 hours.
10. Use of a polyimide aerogel / phase change material temperature control composite material according to any one of claims 1 to 4 or a polyimide aerogel / phase change material temperature control composite material prepared by the method according to any one of claims 5 to 9 in the preparation of low-temperature thermal management materials for precision electronic components.
Citation Information
Patent Citations
Assembly and system for managing thermal runaway issues in electric vehicle batteries
CN115023342A
Composite thermal insulation material
CN116834402A
Polyimide aerogel composite diaphragm with thermal closing function as well as preparation method and application of polyimide aerogel composite diaphragm
CN118173972A
Systems, structures and materials for electrochemical device thermal management
US20160226114A1
Aerogel-foam composites
WO2007146945A2
Cited By
Heat insulation-heat conduction integrated phase change composite material and preparation method thereof
CN119978538A
Temperature-regulating chemical fiber, and preparation method therefor and use thereof