Large low-segregation ultralow-carbon stainless steel ingot and preparation method thereof

Through the electric furnace smelting and vacuum pouring process, the manufacturing problem of low-segregation ultra-low-carbon stainless steel ingots above 100 tons is solved, and low-segregation and high-quality steel forgings are achieved to meet the needs of components of large hydropower units.

CN118910513APending Publication Date: 2024-11-08CHINA ERZHONG GRP DEYANG HEAVY IND
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410707158.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing technology is difficult to manufacture low-segment ultra-low-carbon stainless steel ingots above 100 tons, resulting in poor uniformity of forgings and serious defects in UT heart detection, which cannot meet the key components of large hydroelectric units.

Method used

The process flow of electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace microalloy smelting → vacuum combined pouring is adopted. Through multiple electric furnace smelting and ladle smelting, the liquid molten steel composition and temperature are controlled. Perform multiple vacuum treatments and alloying to ensure low segregation and high quality of the ingot.

Benefits of technology

It has successfully manufactured low-segregation ultra-low-carbon stainless steel ingots above 100 tons, with C segregation ≤13% and Cr segregation ≤4%, solving equipment bottlenecks and metallurgical difficulties and meeting the engineering application of steel forgings above 200t.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a large low-segregation ultralow-carbon stainless steel ingot and a preparation method thereof, and belongs to the technical field of stainless steel. The large low-segregation ultralow-carbon stainless steel ingot comprises the following components in percentage by mass: less than or equal to 0.04% of C, less than or equal to 0.40% of Si, 12.50-13.50% of Cr, 4.40-5.00% of Ni, 0.40-0.80% of Mo, 0.0150-0.0800% of N, less than or equal to 0.010% of Al, less than or equal to 20ppm of O, less than or equal to 0.05% of V, less than or equal to 0.010% of P, less than or equal to 0.002% of S and the balance of iron and inevitable impurities. According to the low segregation, the segregation of C is smaller than or equal to 13%, and the segregation of Cr is smaller than or equal to 4%. The segregation of C is less than or equal to 13%, and the segregation of Cr is less than or equal to 4%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a large low-segregation ultra-low carbon stainless steel ingot and a preparation method thereof, belonging to the technical field of stainless steel. Background Art

[0002] Ultra-low carbon stainless steel represented by 0Cr13Ni4Mo and 0Cr13Ni5Mo is widely used in hydropower, nuclear power and other fields due to its excellent properties. However, due to its high alloy content, large solidification shrinkage ratio and large segregation tendency, it has long remained in the preparation of steel ingots and corresponding forgings below 100t level, but still has problems such as large segregation, poor performance uniformity and serious internal defects of UT detection.

[0003] With the rapid development of major equipment manufacturing technology, the demand for such large stainless steel forgings is becoming increasingly obvious. There is an urgent need to manufacture large-scale low-segregation ultra-low carbon stainless steel ingots and corresponding forgings above 100 tons or even above 200t, which can be used to manufacture key components of large hydropower units and solve the bottleneck of forging supply.

[0004] CN105908101A discloses an ultra-low carbon nitrogen steel and a preparation method thereof, wherein the total amount of ultra-low carbon nitrogen steel is calculated as follows: C≤0.030, Si≤0.75, Mn≤2.00, P≤0.045, S≤0.030, Cr 18.00-20.00, Ni 8.00-12.00, N≤0.10, and the rest is Fe, and the unit of measurement is weight%. The process flow is blast furnace molten iron → converter smelting → continuous casting, and the carbon and nitrogen content in the steel is low, the method is simple, easy to operate, and the cost is low. However, due to the limitations of the residual element control level, the size specifications of the continuous casting billet, etc., it is not suitable for the manufacture of steel ingots above 100 tons and corresponding forgings. Summary of the invention

[0005] The first object of the present invention is to provide a large-scale low-segregation ultra-low carbon stainless steel ingot.

[0006] To achieve the purpose of the present invention, the composition of the large-scale low-segregation ultra-low carbon stainless steel ingot is calculated by mass percentage as follows: C≤0.04%, Si≤0.40%, Cr: 12.50-13.50%, Ni: 4.40-5.00%, Mo: 0.40-0.80%, N: 0.0150-0.0800%, Al≤0.010%, O≤20ppm, V≤0.05%, P≤0.010%, S≤0.002%, and the rest are iron and unavoidable impurities; the low segregation is C segregation ≤13%, Cr segregation ≤4%.

[0007] In a specific embodiment, the steel ingot is above 100 tons, preferably above 120 tons, and more preferably above 200 tons; preferably, the segregation of C is ≤11.7%, and the segregation of Cr is ≤3.5%.

[0008] In a specific embodiment, the preparation method of the steel ingot includes: electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace microalloying smelting → vacuum casting. Vacuum casting is to cast qualified casting molten steel smelted by multiple ladles into the same steel ingot.

[0009] In a specific embodiment, the number of furnaces for electric furnace smelting is ≥2, the steel output of each furnace for electric furnace smelting is 71% to 76% of the finished molten steel, the finished molten steel volume is ≥200t, the finished molten steel is molten steel that has been micro-alloyed and smelted in a ladle refining furnace, vacuum treated, and whose chemical composition meets the process requirements, the number of ladles is ≥2, and the amount of molten steel in each ladle furnace is 65t to 160t; preferably, there is one VOD station, each ladle performs VOD operation in turn, and qualified molten steel is vacuum cast in turn;

[0010] Preferably, the ladle diameter of the ladle refining furnace is ≥2800 mm, and the ladle height is ≥2800 mm;

[0011] In the electric furnace smelting, P in the molten steel is controlled below 0.0025%, C is controlled below 0.06%, S is controlled below 0.020%, and V is controlled below 0.005%. Preferably, the electric furnace smelting is carried out by strong oxygen blowing and carbon injection operation to produce high-basicity and strong oxidizing slag for deep removal of P and C.

[0012] In a specific embodiment, the ladle refining furnace slag is smelted, and the slag-making P content is controlled below 0.0015%; preferably, lime and fluorite are used for slag making, the lime dosage is 2-4t, the fluorite dosage is 0.7-1.5t, the slag layer thickness is 150-250m, and the slag basicity is 4-6;

[0013] The ladle refining furnace slag smelting preferably adopts bottom blowing argon to stir the molten steel;

[0014] The ladle refining furnace slag smelting preferably also includes:

[0015] A. Select aluminum blocks and add them at 1-3 kg / t steel to precipitate and deoxidize the molten steel, and control the Al2O3 content in the slag to 8-15%;

[0016] B. Use low P and low V ferrochrome to alloy Cr, where P≤0.028% and V≤0.20% in ferrochrome, and control the P content of Cr alloying to less than 0.006% and the V content to less than 0.045%;

[0017] C. Perform alloying operation to adjust the Cr content to Cr: 8.75-12.15%; the Ni content to Ni: 3.74-5.00%; and the Mo content to Mo: 0.36-0.80%;

[0018] D. When the temperature is ≥1650℃, perform ladle inversion to remove the slag; after ladle inversion, the space from the liquid level in the ladle to the edge of the ladle is preferably greater than 800mm;

[0019] Preferably, the VOD operation is performed when the temperature of the molten steel after the ladle is between 1560 and 1630° C. If the temperature of the molten steel after the ladle is not within the range of 1560 to 1630° C., it is necessary to increase or decrease the temperature to 1560 to 1630° C. before performing the VOD operation.

[0020] After the composition of the second batch of molten steel in the electric furnace is qualified, the molten steel is injected into the second ladle to carry out the slag smelting stage of the ladle refining furnace of the second batch of molten steel, and the operation steps are the same as above.

[0021] If the molten steel in the first or second furnace of the ladle refining furnace, or in both furnaces, is insufficient, the electric furnace can smelt the third or fourth furnace until the molten steel in the ladle refining furnace meets the requirements.

[0022] In a specific embodiment, the VOD includes transferring the ladle after smelting the slag in the ladle refining furnace to the VOD station and performing the VOD operation. The VOD operation includes sequentially performing vacuuming. When the vacuum degree in the furnace is ≤15kpa, the oxygen gun is opened for top oxygen blowing operation, argon is blown at the bottom, and vacuuming is continued. The oxygen blowing parameters are adjusted according to the oxygen potential curve. After the oxygen potential drops, the oxygen is blown for 5 to 20 minutes, the oxygen blowing is stopped, the first vacuum treatment is maintained for 10 to 30 minutes, and then the VCD operation is entered; preferably, the oxygen pressure in the oxygen gun is 0.4 to 1.5Mpa, and the flow rate is controlled at 50 to 1500m 3 / h, first small and then large, dynamically adjust the oxygen flow rate according to the oxygen potential diagram, the oxygen potential and oxygen flow rate are inversely proportional; the flow rate of VOD bottom blowing argon is preferably 80-180L / min. Continue vacuuming for the first vacuum treatment.

[0023] Overblowing is determined based on the actual parameters of endpoint C content requirements, molten steel volume, free space height, oxygen flow rate and pressure, combined with the oxygen potential curve.

[0024] In a specific embodiment, the ladle refining furnace VOD smelting includes, in sequence, releasing vacuum, adding ferrosilicon at 3-8 kg / t steel, adding Si at a content of Si≤0.40%, adding Al blocks according to the degree of peroxidation and the residual Al content in the molten steel after VOD deoxidation not exceeding 0.01%, preferably adding Al blocks at 3-8 kg / t steel in the ladle refining furnace VCD smelting; adding lime by controlling the amount of slag according to the thickness of the slag layer of 80-150 mm; if the temperature is ≥1650°C, adding 1-4 t of alloy, if the temperature is <1650°C, no alloy is added; performing a second vacuum treatment, and after the treatment, performing micro-alloying smelting in the ladle refining furnace;

[0025] The parameters of the second vacuum treatment are preferably: vacuum degree ≤ 1000pa, bottom blowing argon gas flow rate controlled at 80-180L / min, vacuum holding time 10-30min;

[0026] The ladle refining furnace microalloying smelting includes sampling for chemical analysis, temperature adjustment, deoxidation, microalloying, and steel tapping operations; the N content adjustment principle of the microalloying is: adjusting the N content according to 100% of the lower limit of the internal control range to 150% of the upper limit of the internal control range;

[0027] The first ladle’s steel composition control: C = the upper limit of the internal control range ± 0.005%, Cr = the upper limit of the internal control range -0.20% ~ the upper limit of the internal control range ± 0.10%; the second ladle’s steel composition control: C = the lower limit of the internal control range ± 0.005%, Cr = the lower limit of the internal control range ± 0.20% ~ the middle limit of the internal control range; the remaining components are controlled according to the middle limit of the internal control range;

[0028] The first batch of molten steel reaches 80 to 120°C above the melting point for steel tapping, and the second batch of molten steel reaches 60 to 100°C above the melting point for steel tapping.

[0029] The internal control range mentioned in the present invention refers to a smaller composition range required by customers within the composition range of the large low-segregation ultra-low carbon stainless steel ingot of the present invention.

[0030] The micro-alloying is to adjust the content of alloying elements according to the difference between the internal control component requirements and the actual chemical analysis results.

[0031] After all the molten steel heats have completed the VOD operation, the subsequent temperature adjustment, deoxidation and micro-alloying operations can be carried out in different furnaces according to the capacity and number of ladle furnaces, or they can be carried out alternately in the same furnace.

[0032] In a specific embodiment, the pouring temperature of the vacuum casting is 40-80°C above the melting point, the pouring speed is 5-9t / min, the vacuum degree is ≤1000pa, and the nitrogen removal rate of the vacuum casting is controlled at 5-50%. The vacuum dripping degassing is promoted.

[0033] The second object of the present invention is to provide a method for preparing the above-mentioned large low-segregation ultra-low carbon stainless steel ingot.

[0034] To achieve the second object of the present invention, the preparation method of the steel ingot comprises: electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace microalloying smelting → vacuum casting;

[0035] The number of furnaces for electric furnace smelting is ≥2, the steel output of each furnace is 71% to 76% of the finished molten steel, the finished molten steel is ≥200t, the finished molten steel is molten steel after microalloying in a ladle refining furnace, vacuum treated, and the chemical composition meets the process requirements, the number of ladles is ≥2, and the amount of molten steel in each ladle furnace is 65t to 160t; preferably, there is one VOD station, each ladle performs VOD operation in turn, and qualified molten steel is vacuum cast in turn;

[0036] Preferably, the ladle diameter of the ladle refining furnace is ≥2800 mm, and the ladle height is ≥2800 mm;

[0037] In the electric furnace smelting, P in the molten steel is controlled below 0.0025%, C is controlled below 0.06%, S is controlled below 0.020%, and V is controlled below 0.005%. Preferably, the electric furnace smelting is carried out by strong oxygen blowing and carbon injection operation to produce high-basicity and strong oxidizing slag for deep removal of P and C.

[0038] In a specific embodiment, the ladle refining furnace slag is smelted, and the slag-making P content is controlled below 0.0015%; preferably, lime and fluorite are used for slag making, the lime dosage is 2-4t, the fluorite dosage is 0.7-1.5t, the slag layer thickness is 150-250m, and the slag basicity is 4-6;

[0039] The ladle refining furnace slag smelting preferably adopts bottom blowing argon to stir the molten steel;

[0040] The ladle refining furnace slag smelting preferably also includes:

[0041] A. Select aluminum blocks and add them at 1-3 kg / t steel to precipitate and deoxidize the molten steel, and control the Al2O3 content in the slag to 8-15%;

[0042] B. Use low P and low V ferrochrome to alloy Cr, where P≤0.028% and V≤0.20% in ferrochrome, and control the P content of Cr alloying to less than 0.006% and the V content to less than 0.045%;

[0043] C. Perform alloying operation to adjust the Cr content to Cr: 8.75-12.15%; the Ni content to Ni: 3.74-5.00%; and the Mo content to Mo: 0.36-0.80%;

[0044] D. When the temperature is ≥1650℃, perform ladle inversion to remove the slag; after ladle inversion, the space from the liquid level in the ladle to the edge of the ladle is preferably greater than 800mm;

[0045] Preferably, the VOD operation is performed when the temperature of the molten steel after the ladle is 1560-1630°C;

[0046] The VOD includes transferring the ladle after smelting the slag in the ladle refining furnace to the VOD station and performing the VOD operation. The VOD operation includes sequentially performing vacuuming. When the vacuum degree in the furnace is ≤15kpa, the oxygen gun is opened to perform top oxygen blowing operation, bottom argon blowing, and continuous vacuuming. The oxygen blowing parameters are adjusted according to the oxygen potential curve. After the oxygen potential drops, oxygen is overblown for 5 to 20 minutes, oxygen blowing is stopped, and the first vacuum treatment is maintained for 10 to 30 minutes before entering the VCD operation. Preferably, the oxygen pressure in the oxygen gun is 0.4 to 1.5Mpa, and the flow rate is controlled at 50 to 1500m 3 / h, first small and then large, dynamically adjust the oxygen flow rate according to the oxygen potential diagram, the oxygen potential and oxygen flow rate are inversely proportional; the flow rate of VOD bottom blowing argon is preferably 80-180L / min;

[0047] The VCD smelting in the ladle refining furnace includes, in sequence, releasing vacuum, adding ferrosilicon at 3-8 kg / t steel, adding Si at a content of Si≤0.40%, adding Al blocks at a residual Al content in the deoxidized molten steel not exceeding 0.01%, preferably, adding Al blocks at 3-8 kg / t steel in the VCD smelting in the ladle refining furnace; adding lime by controlling the amount of slag according to the thickness of the slag layer of 80-150 mm; adding 1-4 t alloy if the temperature is ≥1650°C, and adding no alloy if the temperature is <1650°C; performing a second vacuum treatment, and performing microalloying smelting in the ladle refining furnace after the treatment is completed;

[0048] The parameters of the second vacuum treatment are preferably: vacuum degree ≤ 1000pa, argon gas flow rate controlled at 80-180L / min, and vacuum holding time 10-30min;

[0049] The ladle refining furnace microalloying smelting includes sampling for chemical analysis, temperature adjustment, deoxidation, microalloying, and steel tapping operations;

[0050] The principle of adjusting the N content of the microalloying is: adjusting the N content by 100% of the lower limit of the internal control range to 150% of the upper limit of the internal control range;

[0051] The first ladle’s steel composition control: C = the upper limit of the internal control range ± 0.005%, Cr = the upper limit of the internal control range -0.20% ~ the upper limit of the internal control range ± 0.10%; the second ladle’s steel composition control: C = the lower limit of the internal control range ± 0.005%, Cr = the lower limit of the internal control range ± 0.20% ~ the middle limit of the internal control range; the remaining components are controlled according to the middle limit of the internal control range;

[0052] The first ladle of molten steel is tapped when its temperature reaches 80-120℃ above the melting point, and the second ladle of molten steel is tapped when its temperature reaches 60-100℃ above the melting point;

[0053] The pouring temperature of the vacuum casting is 40-80°C above the melting point, the pouring speed is 5-9t / min, the vacuum degree is ≤1000pa, and the nitrogen removal rate of the vacuum casting is controlled at 5-50%. The vacuum dripping degassing is promoted.

[0054] Beneficial effects:

[0055] The segregation of C in the steel ingot of 100-ton level or above of the present invention is ≤13%, and the segregation of Cr is ≤4%.

[0056] The present invention not only solves the equipment bottleneck, but also overcomes the metallurgical difficulties of ultra-low carbon stainless steel. It can use a single VOD device to produce two or more furnaces of qualified molten steel, meet the casting requirements of steel ingots above 200t level, and obtain low segregation forgings to meet engineering applications. DETAILED DESCRIPTION

[0057] To achieve the purpose of the present invention, the composition of the large-scale low-segregation ultra-low carbon stainless steel ingot is calculated by mass percentage as follows: C≤0.04%, Si≤0.40%, Cr: 12.50-13.50%, Ni: 4.40-5.00%, Mo: 0.40-0.80%, N: 0.0150-0.0800%, Al≤0.010%, O≤20ppm, V≤0.05%, P≤0.010%, S≤0.002%, and the rest are iron and unavoidable impurities; the low segregation is C segregation ≤13%, Cr segregation ≤4%.

[0058] In a specific embodiment, the steel ingot is above 100 tons, preferably above 120 tons, and more preferably above 200 tons; preferably, the segregation of C is ≤11.7%, and the segregation of Cr is ≤3.5%.

[0059] In a specific embodiment, the preparation method of the steel ingot includes: electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace microalloying smelting → vacuum casting. Vacuum casting is to cast qualified casting molten steel smelted by multiple ladles into the same steel ingot.

[0060] In a specific embodiment, the number of furnaces for electric furnace smelting is ≥2, the steel output of each furnace for electric furnace smelting is 71% to 76% of the finished molten steel, the finished molten steel volume is ≥200t, the finished molten steel is molten steel that has been micro-alloyed and smelted in a ladle refining furnace, vacuum treated, and whose chemical composition meets the process requirements, the number of ladles is ≥2, and the amount of molten steel in each ladle furnace is 65t to 160t; preferably, there is one VOD station, each ladle performs VOD operation in turn, and qualified molten steel is vacuum cast in turn;

[0061] Preferably, the ladle diameter of the ladle refining furnace is ≥2800 mm, and the ladle height is ≥2800 mm;

[0062] In the electric furnace smelting, P in the molten steel is controlled below 0.0025%, C is controlled below 0.06%, S is controlled below 0.020%, and V is controlled below 0.005%. Preferably, the electric furnace smelting is carried out by strong oxygen blowing and carbon injection operation to produce high-basicity and strong oxidizing slag for deep removal of P and C.

[0063] In a specific embodiment, the ladle refining furnace slag is smelted, and the slag-making P content is controlled below 0.0015%; preferably, lime and fluorite are used for slag making, the lime dosage is 2-4t, the fluorite dosage is 0.7-1.5t, the slag layer thickness is 150-250m, and the slag basicity is 4-6;

[0064] The ladle refining furnace slag smelting preferably adopts bottom blowing argon to stir the molten steel;

[0065] The ladle refining furnace slag smelting preferably also includes:

[0066] A. Select aluminum blocks and add them at 1-3 kg / t steel to precipitate and deoxidize the molten steel, and control the Al2O3 content in the slag to 8-15%;

[0067] B. Use low P and low V ferrochrome to alloy Cr, where P≤0.028% and V≤0.20% in ferrochrome, and control the P content of Cr alloying to less than 0.006% and the V content to less than 0.045%;

[0068] C. Perform alloying operation to adjust the Cr content to Cr: 8.75-12.15%; the Ni content to Ni: 3.74-5.00%; and the Mo content to Mo: 0.36-0.80%;

[0069] D. When the temperature is ≥1650℃, perform ladle inversion to remove the slag; after ladle inversion, the space from the liquid level in the ladle to the edge of the ladle is preferably greater than 800mm;

[0070] Preferably, the VOD operation is performed when the temperature of the molten steel after the ladle is between 1560 and 1630° C. If the temperature of the molten steel after the ladle is not within the range of 1560 to 1630° C., it is necessary to increase or decrease the temperature to 1560 to 1630° C. before performing the VOD operation.

[0071] After the composition of the second batch of molten steel in the electric furnace is qualified, the molten steel is injected into the second ladle to carry out the slag smelting stage of the ladle refining furnace of the second batch of molten steel, and the operation steps are the same as above.

[0072] If the molten steel in the first or second furnace of the ladle refining furnace, or in both furnaces, is insufficient, the electric furnace can smelt the third or fourth furnace until the molten steel in the ladle refining furnace meets the requirements.

[0073] In a specific embodiment, the VOD includes transferring the ladle after smelting the slag in the ladle refining furnace to the VOD station and performing the VOD operation. The VOD operation includes sequentially performing vacuuming. When the vacuum degree in the furnace is ≤15kpa, the oxygen gun is opened for top oxygen blowing operation, argon is blown at the bottom, and vacuuming is continued. The oxygen blowing parameters are adjusted according to the oxygen potential curve. After the oxygen potential drops, the oxygen is blown for 5 to 20 minutes, the oxygen blowing is stopped, the first vacuum treatment is maintained for 10 to 30 minutes, and then the VCD operation is entered; preferably, the oxygen pressure in the oxygen gun is 0.4 to 1.5Mpa, and the flow rate is controlled at 50 to 1500m 3 / h, first small and then large, dynamically adjust the oxygen flow rate according to the oxygen potential diagram, the oxygen potential and oxygen flow rate are inversely proportional; the flow rate of VOD bottom blowing argon is preferably 80-180L / min. Continue vacuuming for the first vacuum treatment.

[0074] Overblowing is determined based on the actual parameters of endpoint C content requirements, molten steel volume, free space height, oxygen flow rate and pressure, combined with the oxygen potential curve.

[0075] In a specific embodiment, the ladle refining furnace VOD smelting includes, in sequence, releasing vacuum, adding ferrosilicon at 3-8 kg / t steel, adding Si at a content of Si≤0.40%, adding Al blocks according to the degree of peroxidation and the residual Al content in the molten steel after VOD deoxidation not exceeding 0.01%, preferably adding Al blocks at 3-8 kg / t steel in the ladle refining furnace VCD smelting; adding lime by controlling the amount of slag according to the thickness of the slag layer of 80-150 mm; if the temperature is ≥1650°C, adding 1-4 t of alloy, if the temperature is <1650°C, no alloy is added; performing a second vacuum treatment, and after the treatment, performing micro-alloying smelting in the ladle refining furnace;

[0076] The parameters of the second vacuum treatment are preferably: vacuum degree ≤ 1000pa, bottom blowing argon gas flow rate controlled at 80-180L / min, vacuum holding time 10-30min;

[0077] The ladle refining furnace microalloying smelting includes sampling for chemical analysis, temperature adjustment, deoxidation, microalloying, and steel tapping operations; the N content adjustment principle of the microalloying is: adjusting the N content according to 100% of the lower limit of the internal control range to 150% of the upper limit of the internal control range;

[0078] The first ladle’s steel composition control: C = the upper limit of the internal control range ± 0.005%, Cr = the upper limit of the internal control range -0.20% ~ the upper limit of the internal control range ± 0.10%; the second ladle’s steel composition control: C = the lower limit of the internal control range ± 0.005%, Cr = the lower limit of the internal control range ± 0.20% ~ the middle limit of the internal control range; the remaining components are controlled according to the middle limit of the internal control range;

[0079] The first batch of molten steel reaches 80 to 120°C above the melting point for steel tapping, and the second batch of molten steel reaches 60 to 100°C above the melting point for steel tapping.

[0080] The micro-alloying is to adjust the content of alloying elements according to the difference between the internal control component requirements and the actual chemical analysis results.

[0081] After all the molten steel heats have completed the VOD operation, the subsequent temperature adjustment, deoxidation and micro-alloying operations can be carried out in different furnaces according to the capacity and number of ladle furnaces, or they can be carried out alternately in the same furnace.

[0082] In a specific embodiment, the pouring temperature of the vacuum casting is 40-80°C above the melting point, the pouring speed is 5-9t / min, the vacuum degree is ≤1000pa, and the nitrogen removal rate of the vacuum casting is controlled at 5-50%. The vacuum dripping degassing is promoted.

[0083] To achieve the second object of the present invention, the preparation method of the steel ingot comprises: electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace microalloying smelting → vacuum casting;

[0084] The number of furnaces for electric furnace smelting is ≥2, the steel output of each furnace is 71% to 76% of the finished molten steel, the finished molten steel is ≥200t, the finished molten steel is molten steel after microalloying in a ladle refining furnace, vacuum treated, and the chemical composition meets the process requirements, the number of ladles is ≥2, and the amount of molten steel in each ladle furnace is 65t to 160t; preferably, there is one VOD station, each ladle performs VOD operation in turn, and qualified molten steel is vacuum cast in turn;

[0085] Preferably, the ladle diameter of the ladle refining furnace is ≥2800 mm, and the ladle height is ≥2800 mm;

[0086] In the electric furnace smelting, P in the molten steel is controlled below 0.0025%, C is controlled below 0.06%, S is controlled below 0.020%, and V is controlled below 0.005%. Preferably, the electric furnace smelting is carried out by strong oxygen blowing and carbon injection operation to produce high-basicity and strong oxidizing slag for deep removal of P and C.

[0087] In a specific embodiment, the ladle refining furnace slag is smelted, and the slag-making P content is controlled below 0.0015%; preferably, lime and fluorite are used for slag making, the lime dosage is 2-4t, the fluorite dosage is 0.7-1.5t, the slag layer thickness is 150-250m, and the slag basicity is 4-6;

[0088] The ladle refining furnace slag smelting preferably adopts bottom blowing argon to stir the molten steel;

[0089] The ladle refining furnace slag smelting preferably also includes:

[0090] A. Select aluminum blocks and add them at 1-3 kg / t steel to precipitate and deoxidize the molten steel, and control the Al2O3 content in the slag to 8-15%;

[0091] B. Use low P and low V ferrochrome to alloy Cr, where P≤0.028% and V≤0.20% in ferrochrome, and control the P content of Cr alloying to less than 0.006% and the V content to less than 0.045%;

[0092] C. Perform alloying operation to adjust the Cr content to Cr: 8.75-12.15%; the Ni content to Ni: 3.74-5.00%; and the Mo content to Mo: 0.36-0.80%;

[0093] D. When the temperature is ≥1650℃, perform ladle inversion to remove the slag; after ladle inversion, the space from the liquid level in the ladle to the edge of the ladle is preferably greater than 800mm;

[0094] Preferably, the VOD operation is performed when the temperature of the molten steel after the ladle is 1560-1630°C;

[0095] The VOD includes transferring the ladle after smelting the slag in the ladle refining furnace to the VOD station and performing the VOD operation. The VOD operation includes sequentially performing vacuuming. When the vacuum degree in the furnace is ≤15kpa, the oxygen gun is opened to perform top oxygen blowing operation, bottom argon blowing, and continuous vacuuming. The oxygen blowing parameters are adjusted according to the oxygen potential curve. After the oxygen potential drops, oxygen is overblown for 5 to 20 minutes, oxygen blowing is stopped, and the first vacuum treatment is maintained for 10 to 30 minutes before entering the VCD operation. Preferably, the oxygen pressure in the oxygen gun is 0.4 to 1.5Mpa, and the flow rate is controlled at 50 to 1500m 3 / h, first small and then large, dynamically adjust the oxygen flow rate according to the oxygen potential diagram, the oxygen potential and oxygen flow rate are inversely proportional; the flow rate of VOD bottom blowing argon is preferably 80-180L / min;

[0096] The VCD smelting in the ladle refining furnace includes, in sequence, releasing vacuum, adding ferrosilicon at 3-8 kg / t steel, adding Si at a content of Si≤0.40%, adding Al blocks at a residual Al content in the deoxidized molten steel not exceeding 0.01%, preferably, adding Al blocks at 3-8 kg / t steel in the VCD smelting in the ladle refining furnace; adding lime by controlling the amount of slag according to the thickness of the slag layer of 80-150 mm; adding 1-4 t alloy if the temperature is ≥1650°C, and adding no alloy if the temperature is <1650°C; performing a second vacuum treatment, and performing microalloying smelting in the ladle refining furnace after the treatment is completed;

[0097] The parameters of the second vacuum treatment are preferably: vacuum degree ≤ 1000pa, argon gas flow rate controlled at 80-180L / min, and vacuum holding time 10-30min;

[0098] The ladle refining furnace microalloying smelting includes sampling for chemical analysis, temperature adjustment, deoxidation, microalloying, and steel tapping operations;

[0099] The principle of adjusting the N content of the microalloying is: adjusting the N content by 100% of the lower limit of the internal control range to 150% of the upper limit of the internal control range;

[0100] The first ladle’s steel composition control: C = the upper limit of the internal control range ± 0.005%, Cr = the upper limit of the internal control range -0.20% ~ the upper limit of the internal control range ± 0.10%; the second ladle’s steel composition control: C = the lower limit of the internal control range ± 0.005%, Cr = the lower limit of the internal control range ± 0.20% ~ the middle limit of the internal control range; the remaining components are controlled according to the middle limit of the internal control range;

[0101] The first ladle of molten steel is tapped when its temperature reaches 80-120℃ above the melting point, and the second ladle of molten steel is tapped when its temperature reaches 60-100℃ above the melting point;

[0102] The pouring temperature of the vacuum casting is 40-80°C above the melting point, the pouring speed is 5-9t / min, the vacuum degree is ≤1000pa, and the nitrogen removal rate of the vacuum casting is controlled at 5-50%. The vacuum dripping degassing is promoted.

[0103] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0104] Example 1

[0105] 1. Produce a 240t grade large stainless steel ingot with standard composition of C≤0.04%, Si≤0.40%, Cr:12.50-13.50%, Ni:4.40-5.00%, Mo:0.40-0.80%, N:0.0150-0.0800%, Al≤0.010%, O≤20ppm, V≤0.05%, P≤0.010%, S≤0.002%. The internal control composition range is C: 0.02-0.04%, Si: 0.20-0.40%, Cr: 12.60-13.20%, Ni: 4.40-4.80%, Mo: 0.40-0.60%, N: 0.0150-0.0400%, Al≤0.010%, O≤20ppm, V≤0.05%, P≤0.010%, S≤0.002%.

[0106] 2. The process flow for smelting ultra-low carbon stainless steel is electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace micro-alloying smelting → vacuum casting. The amount of smelted finished molten steel is about 250t, the number of ladles is 2, and the VOD station is 1. The 2 ladles are operated in turn for VOD, and the qualified molten steel is vacuum cast in turn. Each molten steel is about 125t.

[0107] 3. In the electric furnace smelting process, through strong oxygen blowing and carbon injection operation, high basicity and strong oxidizing slag is produced, and deep P and C are removed. The P in the molten steel is controlled at 0.0018%, C is controlled at 0.05%, S is controlled at 0.018%, and V is controlled at 0.003%.

[0108] 4. In the smelting process of the ladle refining furnace, the ladle diameter is about 3000mm, the ladle height is 4000mm, and bottom blowing argon is used to stir the molten steel.

[0109] 5. In the slag smelting process of the ladle refining furnace, lime and fluorite are used for slag making, with 2t of lime and 1.2t of fluorite, 180m of slag layer thickness, and 4-5 slag basicity. High-quality lime and fluorite are selected, and the amount of phosphorus added in slag making is controlled below 0.0012%.

[0110] 6. Aluminum blocks are used as pre-deoxidizers, and 2.5 kg / t of steel is added to precipitate and deoxidize the molten steel to control the Al2O3 content in the slag to about 14%.

[0111] 7. In ferrochrome, P=0.025%, V=0.18%. By alloying Cr, the amount of P increases to 0.0056%, and the amount of V increases to 0.04%.

[0112] 8. After alloying of two steel batches, the first batch of steel has the following composition: C = 0.28%, Si = 0.35%, Cr = 11.2%, Ni = 4.60%, Mo = 0.75%, N = 0.025%, Al = 0.007%, V = 0.045%, P = 0.0093%, S = 0.002%. The second batch of steel has the following composition: C = 0.25%, Si = 0.31%, Cr = 11.5%, Ni = 4.62%, Mo = 0.72%, N = 0.023%, Al = 0.008%, V = 0.044%, P = 0.0091%, S = 0.002%.

[0113] 9. After the temperature of the first furnace steel liquid is ≥1650℃, the ladle is reversed to remove the slag. After the ladle is reversed, the temperature of the steel liquid is 1610℃, and the free space from the liquid level in the ladle to the edge of the ladle is 1200mm. The ladle is moved into the VOD station for VOD operation.

[0114] 10. During VOD, first pump in the vacuum pump in turn. When the vacuum degree in the furnace is ≤15kpa, gradually lower the oxygen gun, adjust the gun height, and open the oxygen gun to blow oxygen. The oxygen pressure is 0.4~1.5Mpa, and the flow rate is controlled at 50~1500m 3 / h, first small and then large; the argon flow rate at the bottom of the bag is 80-180L / min, and the vacuum is continuously drawn. Observe the oxygen potential and tail gas temperature, and adjust the oxygen blowing pressure and flow according to the oxygen potential and tail gas temperature values.

[0115] 11. When the oxygen potential reaches an inflection point, continue blowing oxygen for 12 minutes, stop blowing oxygen, and continue vacuuming, i.e. the first vacuum treatment, and maintain for 20 minutes.

[0116] 12. After the vacuum is maintained, release the vacuum, measure the temperature, and take samples. The actual temperature is 1720°C. Add ferrosilicon at 5kg / t steel. The Si content is 0.35% of the smelted product Si content. Add Al blocks at 5kg / t steel. The residual Al content is 0.009%. Control the slag amount according to the slag layer thickness of 140mm, add lime, add 1t of ferrochrome, and carry out the second vacuum treatment.

[0117] 13. Second vacuum treatment parameters: vacuum degree ≤1000pa, holding time about 20min, argon flow rate controlled at 80~180L / min.

[0118] 14. After the second vacuum is completed, the first furnace returns to the heating station for deoxidation, temperature adjustment and micro-alloying operations.

[0119] 15. Repeat the above VOD operation process for the second batch of molten steel.

[0120] 16. After the VOD operation is completed for both furnaces of molten steel, nitriding alloy is added according to N=0.030%. When N=0.0200-0.0300%, the tapping condition of N is met.

[0121] 17. The first ladle of molten steel is controlled to have the following composition: C = 0.040%, Cr = 13.20%; the second ladle of molten steel is controlled to have the following composition: C = 0.021%, Cr = 12.80%; the remaining composition is controlled within the internal control range. The first ladle of molten steel is tapped when the temperature reaches the melting point + 90°C, and the second ladle of molten steel is tapped when the temperature reaches the melting point + 70°C.

[0122] 18. Two bags of molten steel are vacuum poured in sequence, the pouring temperature is melting point + 50 ° C, the pouring speed is 6.7t / min, the vacuum degree is ≤800pa, the vacuum pouring nitrogen removal rate is controlled at 20-30%, and the diffusion during the pouring process is good.

[0123] 19. After the water riser was cut off, the steel ingot was forged into the hub of a large impact wheel. The water riser end was tested and the water riser end showed C = 0.030%, Cr = 12.92%, N = 0.0180%, Ni = 4.52%, Mo = 0.45%, Al = 0.007%, O = 17ppm, V = 0.047%, P = 0.0092%, and S = 0.002%.

[0124] At the riser end, C=0.034%, Cr=13.45%, N=0.0195%, Ni=4.51%, Mo=0.46%, Al=0.005%, O=14ppm, V=0.047%, P=0.0091%, S=0.002%. The maximum segregation of C is 11.7%, and the maximum segregation of Cr is 3.5%. The segregation control of C and Cr reaches the expected target.

Claims

1. Large low segregation ultra-low carbon stainless steel ingot, characterized by: The composition of the steel ingot is calculated by mass percentage as follows: C≤0.04%, Si≤0.40%, Cr: 12.50-13.50%, Ni: 4.40-5.00%, Mo: 0.40-0.80%, N: 0.0150-0.0800%, Al≤0.010%, O≤20ppm, V≤0.05%, P≤0.010%, S≤0.002%, and the rest are iron and unavoidable impurities; the low segregation is C segregation ≤13%, and Cr segregation ≤4%.

2. The large low-segregation ultra-low carbon stainless steel ingot according to claim 1, characterized in that: The steel ingot is above 100 tons, preferably above 120 tons, and more preferably above 200 tons; preferably, the segregation of C is ≤11.7%, and the segregation of Cr is ≤3.5%.

3. The large low-segregation ultra-low carbon stainless steel ingot according to claim 1 or 2, characterized in that: The preparation method of the steel ingot comprises: electric furnace smelting→ ladle refining furnace slag smelting→VOD→ ladle refining furnace VCD smelting→ ladle refining furnace microalloying smelting→vacuum casting.

4. The large low-segregation ultra-low carbon stainless steel ingot according to claim 3, characterized in that: The number of furnaces for electric furnace smelting is ≥2, and the amount of finished molten steel is ≥200t. The finished molten steel is molten steel that has been micro-alloyed in a ladle refining furnace, vacuum treated, and has chemical composition that meets the process requirements. The number of ladles is ≥2, and the amount of molten steel in each ladle furnace is 65t-160t. Preferably, there is one VOD station, and each ladle performs VOD operation in turn, and qualified molten steel is vacuum cast in turn. Preferably, the ladle diameter of the ladle refining furnace is ≥2800 mm, and the ladle height is ≥2800 mm; In the electric furnace smelting, P in the molten steel is controlled below 0.0025%, C is controlled below 0.06%, S is controlled below 0.020%, and V is controlled below 0.005%. Preferably, the electric furnace smelting is carried out by strong oxygen blowing and carbon injection operation to produce high-basicity and strong oxidizing slag for deep removal of P and C.

5. The large low-segregation ultra-low carbon stainless steel ingot according to claim 3, characterized in that: The ladle refining furnace slag smelting, slag adding P content is controlled below 0.0015%; preferably lime and fluorite are used for slag making, the lime dosage is 2-4t, the fluorite dosage is 0.7-1.5t, the slag layer thickness is 150-250m, and the slag basicity is 4-6; The ladle refining furnace slag smelting preferably adopts bottom blowing argon to stir the molten steel; The ladle refining furnace slag smelting preferably also includes: A. Select aluminum blocks and add them at 1-3 kg / t steel to precipitate and deoxidize the molten steel, and control the Al2O3 content in the slag to 8-15%; B. Use low P and low V ferrochrome to alloy Cr, where P≤0.028% and V≤0.20% in ferrochrome, and control the P content of Cr alloying to less than 0.006% and the V content to less than 0.045%; C. Perform alloying operation to adjust the Cr content to Cr: 8.75-12.15%; the Ni content to Ni: 3.74-5.00%; and the Mo content to Mo: 0.36-0.80%; D. When the temperature is ≥1650℃, perform ladle inversion to remove the slag; after ladle inversion, the space from the liquid level in the ladle to the edge of the ladle is preferably greater than 800mm; Preferably, the VOD operation is performed when the temperature of the molten steel after the ladle is between 1560 and 1630°C.

6. The large low-segregation ultra-low carbon stainless steel ingot according to claim 4, characterized in that: The VOD includes transferring the ladle after smelting the slag in the ladle refining furnace to the VOD station and performing the VOD operation. The VOD operation includes sequentially performing vacuuming. When the vacuum degree in the furnace is ≤15kpa, the oxygen gun is opened to perform top oxygen blowing operation, bottom argon blowing, and continuous vacuuming. The oxygen blowing parameters are adjusted according to the oxygen potential curve. After the oxygen potential drops, the oxygen is blown for 5 to 20 minutes, the oxygen blowing is stopped, the first vacuum treatment is maintained for 10 to 30 minutes, and then the VCD operation is entered. Preferably, the oxygen pressure in the oxygen gun is 0.4 to 1.5Mpa, and the flow rate is controlled at 50 to 1500m 3 / h, first small and then large, dynamically adjust the oxygen flow rate according to the oxygen potential diagram, the oxygen potential and the oxygen flow rate are inversely proportional; the flow rate of VOD bottom blowing argon is preferably 80-180L / min.

7. The large low-segregation ultra-low carbon stainless steel ingot according to claim 6, characterized in that: The ladle refining furnace VOD smelting includes, in sequence, releasing vacuum, adding ferrosilicon at 3-8kg / t steel, adding Si at a content of Si≤0.40%, adding Al blocks at a residual Al content of no more than 0.01% in the molten steel after VOD deoxidation in combination with the degree of overoxidation, preferably adding Al blocks at 3-8kg / t steel in the ladle refining furnace VCD smelting; controlling the amount of slag and adding lime at a slag layer thickness of 80-150mm; adding 1-4t alloy if the temperature is ≥1650°C, and adding no alloy if the temperature is <1650°C; performing a second vacuum treatment, and performing microalloying smelting in the ladle refining furnace after the treatment is completed; The parameters of the second vacuum treatment are preferably: vacuum degree ≤ 1000pa, bottom blowing argon gas flow rate controlled at 80-180L / min, vacuum holding time 10-30min; The ladle refining furnace microalloying smelting includes sampling for chemical analysis, temperature adjustment, deoxidation, microalloying, and steel tapping operations; the N content adjustment principle of the microalloying is: adjusting the N content according to 100% of the lower limit of the internal control range to 150% of the upper limit of the internal control range; The first ladle’s steel composition control: C = the upper limit of the internal control range ± 0.005%, Cr = the upper limit of the internal control range -0.20% ~ the upper limit of the internal control range ± 0.10%; the second ladle’s steel composition control: C = the lower limit of the internal control range ± 0.005%, Cr = the lower limit of the internal control range ± 0.20% ~ the middle limit of the internal control range; the remaining components are controlled according to the middle limit of the internal control range; The first batch of molten steel reaches 80 to 120°C above the melting point for steel tapping, and the second batch of molten steel reaches 60 to 100°C above the melting point for steel tapping.

8. The large low-segregation ultra-low carbon stainless steel ingot according to claim 3, characterized in that: The pouring temperature of the vacuum casting is 40-80°C above the melting point, the pouring speed is 5-9t / min, the vacuum degree is ≤1000pa, and the nitrogen removal rate of the vacuum casting is controlled at 5-50%.

9. The method for preparing a large low-segregation ultra-low carbon stainless steel ingot according to any one of claims 1 to 8, characterized in that: The preparation method of the steel ingot comprises: electric furnace smelting → ladle refining furnace slag smelting → VOD → ladle refining furnace VCD smelting → ladle refining furnace microalloying smelting → vacuum casting; The number of furnaces for electric furnace smelting is ≥2, and the amount of finished molten steel is ≥200t. The finished molten steel is molten steel after microalloying in a ladle refining furnace, vacuum treated, and the chemical composition meets the process requirements. The number of ladles is ≥2, and the amount of molten steel in each ladle furnace is 65t-160t. Preferably, there is one VOD station, and each ladle performs VOD operation in turn, and qualified molten steel is vacuum cast in turn. Preferably, the ladle diameter of the ladle refining furnace is ≥2800 mm, and the ladle height is ≥2800 mm; In the electric furnace smelting, P in the molten steel is controlled below 0.0025%, C is controlled below 0.06%, S is controlled below 0.020%, and V is controlled below 0.005%. Preferably, the electric furnace smelting is carried out by strong oxygen blowing and carbon injection operation to produce high-basicity and strong oxidizing slag for deep removal of P and C.

10. The method for preparing a large low-segregation ultra-low carbon stainless steel ingot according to claim 9, characterized in that: The ladle refining furnace slag smelting, slag adding P content is controlled below 0.0015%; preferably lime and fluorite are used for slag making, the lime dosage is 2-4t, the fluorite dosage is 0.7-1.5t, the slag layer thickness is 150-250m, and the slag basicity is 4-6; The ladle refining furnace slag smelting preferably adopts bottom blowing argon to stir the molten steel; The ladle refining furnace slag smelting preferably also includes: A. Select aluminum blocks and add them at 1-3 kg / t steel to precipitate and deoxidize the molten steel, and control the Al2O3 content in the slag to 8-15%; B. Use low P and low V ferrochrome to alloy Cr, where P≤0.028% and V≤0.20% in ferrochrome, and control the P content of Cr alloying to less than 0.006% and the V content to less than 0.045%; C. Perform alloying operation to adjust the Cr content to Cr: 8.75-12.15%; the Ni content to Ni: 3.74-5.00%; and the Mo content to Mo: 0.36-0.80%; D. When the temperature is ≥1650℃, perform ladle inversion to remove the slag; after ladle inversion, the space from the liquid level in the ladle to the edge of the ladle is preferably greater than 800mm; Preferably, the VOD operation is performed when the temperature of the molten steel after the ladle is 1560-1630°C; The VOD includes transferring the ladle after smelting the slag in the ladle refining furnace to the VOD station and performing the VOD operation. The VOD operation includes sequentially performing vacuuming. When the vacuum degree in the furnace is ≤15kpa, the oxygen gun is opened to perform top oxygen blowing operation, bottom argon blowing, and continuous vacuuming. The oxygen blowing parameters are adjusted according to the oxygen potential curve. After the oxygen potential drops, oxygen is overblown for 5 to 20 minutes, oxygen blowing is stopped, and the first vacuum treatment is maintained for 10 to 30 minutes before entering the VCD operation. Preferably, the oxygen pressure in the oxygen gun is 0.4 to 1.5Mpa, and the flow rate is controlled at 50 to 1500m 3 / h, first small and then large, dynamically adjust the oxygen flow rate according to the oxygen potential diagram, the oxygen potential and oxygen flow rate are inversely proportional; the flow rate of VOD bottom blowing argon is preferably 80-180L / min; The VCD smelting in the ladle refining furnace includes, in sequence, releasing vacuum, adding ferrosilicon at 3-8 kg / t steel, adding Si at a content of Si≤0.40%, adding Al blocks at a residual Al content in the deoxidized molten steel not exceeding 0.01%, preferably, adding Al blocks at 3-8 kg / t steel in the VCD smelting in the ladle refining furnace; adding lime by controlling the amount of slag according to the thickness of the slag layer of 80-150 mm; adding 1-4 t alloy if the temperature is ≥1650°C, and adding no alloy if the temperature is <1650°C; performing a second vacuum treatment, and performing microalloying smelting in the ladle refining furnace after the treatment is completed; The parameters of the second vacuum treatment are preferably: vacuum degree ≤ 1000pa, argon gas flow rate controlled at 80-180L / min, and vacuum holding time 10-30min; The ladle refining furnace microalloying smelting includes sampling for chemical analysis, temperature adjustment, deoxidation, microalloying, and steel tapping operations; The principle of adjusting the N content of the microalloying is: adjusting the N content by 100% of the lower limit of the internal control range to 150% of the upper limit of the internal control range; The first ladle’s steel composition control: C = the upper limit of the internal control range ± 0.005%, Cr = the upper limit of the internal control range -0.20% ~ the upper limit of the internal control range ± 0.10%; the second ladle’s steel composition control: C = the lower limit of the internal control range ± 0.005%, Cr = the lower limit of the internal control range ± 0.20% ~ the middle limit of the internal control range; the remaining components are controlled according to the middle limit of the internal control range; The first ladle of molten steel is tapped when its temperature reaches 80-120℃ above the melting point, and the second ladle of molten steel is tapped when its temperature reaches 60-100℃ above the melting point; The pouring temperature of the vacuum casting is 40-80°C above the melting point, the pouring speed is 5-9t / min, the vacuum degree is ≤1000pa, and the nitrogen removal rate of the vacuum casting is controlled at 5-50%.

Citation Information

Patent Citations

  • Ultra-low carbon and nitrogen steel and preparing method

    CN105908101A