Method for preparing high silicon steel through one-step molten salt electrolysis
Through the one-step molten salt electrolysis method, the barium salt, fluorine and chloride salt systems are used to control the diffusion of silicon ions at high temperatures, and high silicon steel is directly prepared, solving the problems of complex processes and high cost in the existing technology, achieving high efficiency and uniformity The preparation of high-silicon steel reduces production costs and improves the uniformity of silicon content.
Patent Information
- Application Number
- CN202410943331.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the preparation process of high-silicon steel is complex, has high cost, and has problems such as difficulty in processing and low production efficiency. Especially when increasing the silicon content to 6.5 wt%, additional annealing treatment is required, which increases the complexity and production cost.
By using one-step molten salt electrolysis method, the current density, time and temperature are controlled by adding barium salt, fluorine and chloride salt to the electrolyte, the current density, time and temperature are achieved, and the silicon ion diffusion in the range of 1000℃ to 1200℃ is directly prepared to avoid the An additional diffusion annealing process was performed.
The preparation process is simplified, production costs are reduced, production efficiency is improved, and the uniformity and density of high silicon steel are ensured. The Si content reaches more than 6.3%, the current efficiency is as high as more than 80%, and the product has few holes and seamless gaps, and the density is high.
Smart Images

Figure CN118910679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high silicon steel material, in particular to a method for preparing the high silicon steel by utilizing one-step molten salt electrolysis, and belongs to the technical field of metallurgical materials. Background Art
[0002] Fe-Si alloy, commonly known as silicon steel, is a key magnetic material for manufacturing generators, motors, transformers, mutual inductors, and relays, and is widely used in the power and electronics industries. Silicon steel is one of the most produced and used materials in the field of magnetic materials, and plays a vital role in storing and converting energy. In the prior art, silicon steel with a silicon content of 6.5wt% has excellent soft magnetic properties, including high magnetic permeability, low coercivity, and low iron loss, and is therefore widely regarded as an ideal core material for achieving high efficiency and energy saving. However, with the increase of silicon content, the elongation of silicon steel deteriorates sharply, which makes it challenging in processing and forming, thereby limiting its industrial production and wide application.
[0003] When preparing high silicon steel strip by rapid solidification, a very high cooling rate is required. Therefore, the thickness of high silicon steel strip prepared by rapid solidification is generally between 0.02mm and 0.06mm. There are large restrictions on the size, which seriously restricts the scope of use of high silicon steel strip. The CVD method is to first roll in a low silicon state, and then add silicon to the silicon steel to increase the silicon content. Through a continuous CVD furnace, a layer of Fe 3 Si material, and then increase the temperature to promote the diffusion of silicon into silicon steel, and finally prepare Fe-6.5wt%Si alloy strip. However, the CVD process has poor stability, high cost and great environmental pollution, which limits the large-scale production of 6.5wt% silicon steel. Therefore, it is urgent to develop a new green and scalable production process.
[0004] The Chinese invention patent with announcement number CN115874231B discloses a method for preparing high silicon steel by molten salt electrolysis, with low silicon steel as the substrate, and the Si content in the substrate is 3.0-4.5wt%. The substrate is used as the cathode, and single crystal / polycrystalline Si is used as the anode, and constant current electrolysis is performed in fluoride molten salt. The present invention can produce high silicon steel strips with consistent Si content on the surface and in the center by regulating parameters such as current density, electrolysis temperature, time and silicon ion concentration in the molten salt, thereby realizing green recycling of molten salt and electrolyte, avoiding the problem of brittle cracking of high silicon steel during rolling, and having a high product yield. The entire process can achieve continuous production.
[0005] The Chinese invention patent application with publication number CN107338460A discloses a method for preparing gradient silicon steel, which specifically comprises: using NaCl, KCl, NaF and SiO 2As raw materials, NaCl, KCl and NaF were mixed in a molar ratio of 1:1:2, and then SiO 2 , preparation of NaCl-KCl-NaF-SiO 2 Molten salt; 1.2% Si low silicon steel sheet as cathode, high purity graphite sheet as anode, put into the above molten salt for electrodeposition; after the deposition, place the cathode in an annealing furnace for diffusion annealing. The present invention uses a cheap and stable molten salt system and a molten salt electrochemical method to prepare an alloy strip with a surface silicon content of 6.5%. The entire preparation process does not involve pressure processing or other plastic deformation processes, which fundamentally avoids any processing difficulties caused by the low plasticity of the Fe-6.5% Si alloy strip.
[0006] However, the above-mentioned existing technologies all require annealing to obtain high-silicon steel, which greatly increases the complexity of preparation, product quality risks and production costs, and reduces production efficiency. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a preparation method for a high-silicon steel sheet using a silicon steel sheet with ≤3wt% Si or pure iron as a matrix through one-step deposition and diffusion, aiming to reduce the complexity of the production process, avoid damage to the original structure of the matrix, reduce costs and improve production efficiency.
[0008] The present invention provides a method for preparing high silicon steel by one-step molten salt electrolysis, comprising the following steps:
[0009] 1) Place the electrolyte in an electrolytic container, then immerse the cathode and anode in the electrolyte, heat the electrolytic container to 1000-1200°C in an inert gas atmosphere, connect the electrodes to a power source and charge at a current density of 5-20 mA cm -2 The electrodes are supplied with a constant current for 60-120 min, wherein the electrolyte comprises a mixture of at least one of silicon dioxide and fluorosilicate (referred to as electrolyte A), an alkali metal salt and a barium salt, and the fluorosilicate comprises Na 2 SiF 6 , K 2 SiF 6 , Li 2 SiF 6 At least one of the following, the barium salt comprising BaF 2 、BaCl 2 At least one of the alkali metal salts includes at least one of KF, KCl, LiF, LiCl, NaCl, and NaF, and based on the total mass of the mixture, the barium salt accounts for 10%-40%, the alkali metal salt accounts for 40-60%, and the electrolyte A accounts for 10-40%;
[0010] 2) After the electrolysis is completed, the cathode is removed, cleaned and dried to obtain high silicon steel.
[0011] Furthermore, the method also includes: a pretreatment step of heating the electrolyte to remove moisture, the heating temperature is 200-300° C., and the insulation time is not less than 12 hours.
[0012] Furthermore, in the step 2), the electrolytic container is heated to 1000-1200° C. and then kept warm for 20-30 minutes.
[0013] Furthermore, the cathode in step 1) is low silicon steel or pure iron with Si content ≤ 3wt%.
[0014] Furthermore, the anode in step 1) is single crystal silicon or polycrystalline silicon.
[0015] Furthermore, in step 1), the thickness of the cathode is 0.1 to 0.65 mm.
[0016] Furthermore, in step 1), the electrolysis container comprises a crucible and a vertical resistance furnace, and placing the electrolyte in the electrolysis container specifically comprises: placing the electrolyte in the crucible, and then placing the crucible in the constant temperature area of the vertical resistance furnace.
[0017] Furthermore, the crucible includes an iron crucible, a quartz crucible, a corundum crucible, a graphite crucible or a nickel crucible.
[0018] Furthermore, the inert gas atmosphere is an atmosphere of argon or nitrogen with a purity of ≥99%.
[0019] The present invention creatively proposes that adding barium salt to the electrolytic molten salt can increase the melting temperature of the molten salt, so that the reaction temperature reaches the temperature of Si diffusion, eliminating the additional diffusion annealing process and realizing the one-step preparation of high silicon steel. In addition, by introducing high melting point barium salt and stabilizing the volatility of Si (IV) compounds based on fluorine and chloride, an excellent diffusion silicide coating can be produced, and the stable fluorine and chloride ion complexes help to reduce the diffusion control effect, thereby inhibiting the increase of interface roughness and the generation of porous and dendrite powder growth.
[0020] In the molten salt system of the present invention in which fluorine and chloride salts of barium are mixed, the deposition and diffusion of Si are affected by current density, time and temperature. Specifically, at a temperature of 1000°C to 1200°C, the reduction reaction of silicon ions in a fluoride salt or chloride salt and an oxide or fluorosilicate molten salt system is a one-step irreversible process controlled by diffusion. Therefore, controlling the temperature within the above range is particularly beneficial for the system of the present invention to generate uniform high-silicon steel. Based on this, electrolysis under the above problem can be effectively achieved by adjusting the composition of the molten salt. During the electrolysis process, if the current density is too large, the deposition rate of Si will be too fast, resulting in the generation of pores. If the current density is too small, the deposition rate of Si will be small, and it will be difficult to deposit on the substrate. Therefore, in order to obtain a suitable deposition rate, based on the reaction system and electrolysis parameters of the present invention, the current density should be controlled to 5-20 mA cm -2 In addition, if the electrolysis time is too long, the diffusion layer formed by Si diffusion will be too thick, and if the electrolysis time is too short, the diffusion layer formed by Si diffusion will be too thin, both of which are not conducive to the formation of uniform high-silicon steel. Therefore, in order to obtain uniformly distributed high-silicon steel, based on the system and electrolysis parameters of the present invention, the time should be controlled to 60-120min, which is more suitable.
[0021] The fluorine-alkali salts and chlorine-alkali salts selected in the present invention have the characteristics of low vapor pressure, low viscosity, wide electrochemical window, high ionic conductivity (and low electronic conductivity) and large decomposition potential range (>3V), and can effectively dissolve reaction products such as oxygen ions, silicates or carbon dioxide during the electrolysis process.
[0022] The present invention eliminates the need for an additional diffusion annealing process to achieve a one-step preparation of high silicon steel. In the prior art, the additional annealing process requires that the Si content of low silicon steel be between 3-4.5%, and the Si content deposited in the ferrosilicon alloy layer be controlled to reach 13wt% (thus requiring a strong current or long-term electrolytic deposition) to achieve a Si content of 6.5% after annealing. At the same time, the deposited Fe x The Si alloy layer needs to be seamlessly connected to the substrate without gaps. The low silicon steel selected in the present invention has a Si content of ≤3% or pure iron. By controlling the electrolysis parameters and electrolyte components, at a temperature of 1000°C to 1200°C, the reduction reaction of silicon ions in the fluoride salt or chloride salt and oxide or fluorosilicate molten salt system is a one-step irreversible process controlled by diffusion. During the electrolysis process, deposition and diffusion are carried out simultaneously to promote the uniform distribution of Si in the entire substrate, and silicon steel with 6.5wt% Si is prepared to achieve one-step molten salt electrolysis.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention adopts a one-step method to prepare high silicon steel, which has a simple preparation process and high efficiency. Compared with the additional annealing process, it effectively avoids the generation of phase change and component segregation, has a simple process, and has little effect on the original structure of the matrix;
[0025] 2. The Si content in the high silicon steel prepared by the present invention can reach more than 6.3%, the current efficiency can reach more than 80%, and the deviation between the maximum and minimum Si content obtained by randomly selecting 20 points for detection can be controlled within 0.25%. The product has few holes, no obvious gaps are observed, and the density is high;
[0026] 3. The medicine used in the present invention is cheap, easy to obtain, and has low consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Electrolysis device used in the present invention
[0028] Figure 2 Scanning electron microscope image of the electrolysis product of Example 1 of the present invention
[0029] Among them, 1-furnace tube, 2-anode, 3-cathode, 4-molten salt, 5-crucible, 6-carbon block, 7-air inlet, 8-air outlet DETAILED DESCRIPTION
[0030] Example 1
[0031] Weigh 10g of BaF with a purity of 99% 2 , 50g KF with a purity of 99.9%, 40g SiO with a purity of 99.5% 2 , mixed at 500r / min for 30min in a planetary high-energy ball mill, taken out, put into an iron crucible wiped dry with alcohol, put the crucible into a horizontal furnace, pass high-purity Ar, heat to 200℃ and keep warm for 12h to remove free water and bound water in the mixed salt.
[0032] A single crystal Si rod with a diameter of 10 mm and a length of 50 mm was used as the anode, and a 0.65 mm thick low-silicon steel sheet was used as the cathode. The chemical composition and mass percentage of the low-silicon steel sheet were: Si: 1.0%, C: 0.0022%, Als: 0.56%, Mn: 0.32%, O: 0.0058%, P: 0.012%, S: 0.0017%, N: 0.0019%, Ti: 0.0018%, V: 0.0012%, Nb: 0.0017%, B: 0.0053%, Sn: 0.101%, and the rest were Fe elements. The surface of the motor was cleaned with deionized water and anhydrous ethanol in turn, and then placed in a 70°C oven to dry for use.
[0033] Use crucible tongs to place the iron crucible containing salt in the constant temperature area of the vertical resistance furnace, keep the crucible horizontal, fix the low-silicon steel sheet cathode on one end of the stainless steel rod, and insert it into the middle of the furnace tube through the pipe opening of the furnace cover of the resistance furnace. The same operation is performed on the Si rod anode. After checking that the airtightness of the resistance furnace is good, introduce high-purity Ar gas and circulating water to raise the temperature of the resistance furnace to 1100℃. After reaching the target temperature, keep it warm for 30 minutes to completely melt the mixed salt.
[0034] Use a multimeter to connect the top of the two electrodes to determine the position of the molten salt and the depth of the electrodes immersed in the molten salt. Both the anode and cathode are immersed in 1.5cm. After fixing the electrode position, connect the electrodes to the power supply and set the constant current to 48.6mA (15mA / cm 2 ), electrolysis time 60min.
[0035] After the electrolysis is finished, the electrode is slowly lifted up and cooled to room temperature at a rate of 5°C / min. The electrode sheet is taken out of the furnace, cleaned and placed in a 70°C oven to dry. Figure 1 The electrolysis product can be seen by scanning electron microscopy. Figure 2 .
[0036] The final Si content of the high silicon steel obtained by the method of this embodiment is 6.5%, and the iron loss P is 10 / 50 =0.48W·kg -1 , P 10 / 400 =8.7W·kg -1 , B 8 =1.34T. The current efficiency of this embodiment is 80.3%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.23wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0037] Example 2
[0038] In the preparation method of this embodiment, 40g of BaCl with a purity of 99% was weighed. 2 , 50g KCl with a purity of 99.9%, 10g SiO with a purity of 99.5% 2 , other steps and parameters are the same as those in Example 1. After measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.4%, and the iron loss P 10 / 50 =0.53W·kg -1 , P 10 / 400 =9.0W·kg -1 , B 8 =1.35T. The current efficiency of this embodiment is 88.7%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.24wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0039] Example 3
[0040] In the preparation method of this embodiment, 30 g of BaF with a purity of 99% was weighed. 2 , 60g of 99.9% pure NaF, 10g of 99.5% pure Na 2 SiF 6 , other steps and parameters are the same as those in Example 1. After measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.4%, and the iron loss P 10 / 50 =0.52W·kg -1 , P 10 / 400 =9.0W·kg -1 , B 8 =1.31T. The current efficiency of this embodiment is 86%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.23wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0041] Example 4
[0042] In the preparation method of this embodiment, 30 g of BaF with a purity of 99% was weighed. 2 , 60g of 99.9% pure LiF, 10g of 99.5% pure K 2 SiF 6 , other steps and parameters are the same as those in Example 1. After measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.4%, and the iron loss P 10 / 50 =0.49W·kg -1 , P 10 / 400 =8.9W·kg -1 , B 8 =1.34T. The current efficiency of this embodiment is 85.6%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.25wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0043] Example 5
[0044] In the preparation method of this embodiment, the constant current is set to 32.4 mA (10 mA / cm 2 ), electrolysis time 75min, other steps, parameters are the same as those in Example 1, after measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.3%, the iron loss P 10 / 50 =0.52W·kg -1 , P 10 / 400 =9.2W·kg -1 , B 8=1.35T. The current efficiency of this embodiment is 84.6%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.21wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0045] Example 6
[0046] In the preparation method of this embodiment, the constant current is set to 16.2 mA (5 mA / cm 2 ), electrolysis time 100min, other steps, parameters are the same as those in Example 1, after measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.3%, the iron loss P 10 / 50 =0.49W·kg -1 , P 10 / 400 =9.1W·kg -1 , B 8 =1.33T. The current efficiency of this embodiment is 86.9%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.22wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0047] Example 7
[0048] In the preparation method of this embodiment, pure iron is selected for the cathode, and the other steps and parameters are the same as those in Example 1. After measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.3%, and the iron loss P 10 / 50 =0.48W·kg -1 , P 10 / 400 =9.1W·kg -1 , B 8 =1.32T. The current efficiency of this embodiment is 87.8%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.23wt%, which is within the error range. The product has few pores, no obvious gaps are observed, and the density is high.
[0049] Comparative Example 1
[0050] The preparation method of this comparative example is the same as that of Example 1, except that the constant current is set to 97.2 mA (30 mA / cm 2 ). According to the measurement, the final Si content of the high silicon steel obtained in this embodiment is 6.4%, and the iron loss P 10 / 50 =0.48W·kg -1 , P 10 / 400 =8.9W·kg -1 , B 8=1.29T. The current efficiency of this embodiment is 70.3%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.22wt%, which is within the error range. However, the product has many micropores, and gaps of tens of microns are observed, and the density is poor.
[0051] Comparative Example 2
[0052] The preparation method of this comparative example is the same as that of Example 1, except that the electrolysis time is 30 minutes. The final Si content of the high silicon steel obtained in this example is 4.7%, and the iron loss P is 10 / 50 =0.89W·kg -1 , P 10 / 400 =16W·kg -1 , B 8 =1.28T. The current efficiency of this embodiment is 45.6%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.22wt%, which is within the error range. However, the product has many micropores, and gaps of tens of microns are observed, and the density is poor.
[0053] Comparative Example 3
[0054] The preparation method of this comparative example is the same as that of Example 2, except that the constant current is set to 9.72 mA (3 mA / cm 2 ). According to the measurement, the final Si content of the high silicon steel obtained in this embodiment is 4.5%, and the iron loss P 10 / 50 =0.87W·kg -1 , P 10 / 400 =15.7W·kg -1 , B 8 =1.31T. The current efficiency of this embodiment is 50.5%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 1.3wt%, which exceeds the allowable error. However, the product has few cavities and no obvious gaps are observed.
[0055] Comparative Example 4
[0056] The preparation method of this comparative example is the same as that of Example 2, except that the electrolysis time is set to 180 min. The final Si content of the high silicon steel obtained in this example is 6.2%, and the iron loss P is 10 / 50 =0.46W·kg -1 , P 10 / 400 =9.3W·kg -1 , B 8=1.28T. The current efficiency of this embodiment is 75.6%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.23wt%, which is within the error range. However, the product has many micropores, and gaps of tens of microns are observed, and the density is poor.
[0057] Comparative Example 5
[0058] The preparation method of this comparative example is the same as that of Example 1, except that the electrolysis temperature is set to 900°C. After measurement, the final Si content of the high silicon steel obtained in this embodiment is 4.8%, and the iron loss P is 10 / 50 =0.86W·kg -1 , P 10 / 400 =15.6W·kg -1 , B 8 =1.34T. The current efficiency of this embodiment is 53.4%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 1.3wt%, which exceeds the allowable error. However, the product has few voids and no obvious gaps are observed.
[0059] Comparative Example 6
[0060] The preparation method of this embodiment is the same as that of embodiment 1, except that the electrolysis temperature is 1300°C. According to the measurement, the final Si content of the high silicon steel obtained in this embodiment is 8.4%, and the iron loss P is 10 / 50 =0.45W·kg -1 , P 10 / 400 =8.8W·kg -1 , B 8 =1.39T. The current efficiency of this embodiment is 81.3%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.22wt%, which is within the error range. However, the silicon content is high, and the product has more micropores, and gaps of tens of microns are observed, and the density is poor.
[0061] Comparative Example 7
[0062] Weigh 30g of 99.5% pure LiF, 60g of 99.9% pure KF, and 10g of 99.5% pure NaSiF 4 , mixed at 500r / min for 30min in a planetary high-energy ball mill, taken out, put into an iron crucible wiped dry with alcohol, put the crucible into a horizontal furnace, pass high-purity Ar, heat to 200℃ and keep warm for 12h to remove free water and bound water in the mixed salt.
[0063] A single crystal Si rod with a diameter of 10 mm and a length of 50 mm was used as the anode, and a 0.65 mm thick low-silicon steel sheet was used as the cathode. The chemical composition of the low-silicon steel sheet included (mass percentage): Si: 1.0%, C: 0.0022%, Als: 0.56%, Mn: 0.32%, O: 0.0058%, P: 0.012%, S: 0.0017%, N: 0.0019%, Ti: 0.0018%, V: 0.0012%, Nb: 0.0017%, B: 0.0053%, Sn: 0.101%, and the rest was Fe element. The surface of the motor was cleaned with deionized water and anhydrous ethanol in turn, and then placed in a 70°C oven to dry for use.
[0064] Use crucible tongs to place the iron crucible containing salt in the constant temperature area of the vertical resistance furnace, keep the crucible horizontal, fix the low-silicon steel sheet cathode on one end of the stainless steel rod, and insert it into the middle of the furnace tube through the pipe opening of the furnace cover of the resistance furnace. The same operation is performed on the Si rod anode. After checking that the airtightness of the resistance furnace is good, introduce high-purity Ar gas and circulating water to raise the temperature of the resistance furnace to 600°C. After reaching the target temperature, keep it warm for 30 minutes to completely melt the mixed salt.
[0065] Use a multimeter to connect the top of the two electrodes to determine the position of the molten salt and the depth of the electrodes immersed in the molten salt. Both the anode and cathode are immersed in 1.5cm. After fixing the electrode position, connect the electrodes to the power supply and set the constant current to 48.6mA (15mA / cm 2 ), electrolysis time 60min.
[0066] After the electrolysis is finished, the electrode is slowly lifted up and cooled to room temperature at a cooling rate of 5°C / min. The electrode sheet is taken out of the furnace, cleaned, and then placed in a 70°C oven for drying.
[0067] The electrolysis product was placed in the constant temperature area of the annealing furnace. After checking the airtightness, the annealing furnace was purged three times with high-purity Ar. Then, the temperature was increased to 1100°C at a heating rate of 5°C / min in an Ar atmosphere and kept at that temperature for 60 minutes. After heat treatment, the sample was cooled to room temperature at a cooling rate of 5°C / min.
[0068] The final Si content of the high silicon steel obtained by the comparative method is 4.2%, and the iron loss P is 10 / 50 =0.88W·kg -1 , P 10 / 400 =15W·kg -1 , B 8 =1.28T. The current efficiency of this embodiment is 48.6%. Among the 20 points randomly detected on the cross section of the sample, the difference between the highest and lowest values of Si content is 0.65wt%, which exceeds the allowable error. The product has many micropores, and gaps of more than ten to several tens of microns are observed, and the density is poor.
[0069] It should be noted that, according to the above embodiments of the present invention, those skilled in the art can fully realize the full scope of the independent claims and dependent rights of the present invention, and the implementation process and method are the same as the above embodiments; and the part not described in detail in the present invention belongs to the well-known technology in the field. However, the protection scope of the present invention is not limited to this, and any changes or substitutions that can be easily thought of by any person familiar with the field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing high silicon steel by one-step molten salt electrolysis, characterized in that: The steps include: 1) Place the electrolyte in an electrolytic container, then immerse the cathode and anode in the electrolyte, heat the electrolytic container to 1000-1200°C in an inert gas atmosphere, connect the electrodes to a power source and charge at a current density of 5-20 mA cm -2 The electrodes are supplied with a constant current for 60-120 min, wherein the electrolyte comprises a mixture of electrolyte A, an alkali metal salt and a barium salt, wherein the electrolyte A comprises at least one of silicon dioxide and a fluorosilicate, wherein the fluorosilicate comprises at least one of Na2SiF6, K2SiF6, and Li2SiF6, wherein the alkali metal salt comprises at least one of KF, KCl, LiF, LiCl, NaCl, and NaF, and wherein the barium salt comprises at least one of BaF2 and BaCl2; 2) After the electrolysis is completed, the cathode is removed, cleaned and dried to obtain high silicon steel.
2. The method according to claim 1, characterized in that Based on the total mass of the electrolyte mixture, the barium salt accounts for 10%-40%, the alkali metal salt accounts for 40-60%, and the electrolyte A accounts for 10-40%.
3. The method according to claim 1 or 2, characterized in that The method further comprises: a pretreatment step of heating the electrolyte to remove moisture, wherein the heating temperature is 200-300° C. and the heat preservation time is not less than 12 hours.
4. The method according to claim 1 or 2, characterized in that: In the step 2), the electrolysis container is heated to 1000-1200° C. and then kept warm for 20-30 minutes.
5. The method according to claim 1 or 2, characterized in that: The cathode in step 1) is low silicon steel or pure iron with Si content ≤ 3wt%.
6. The method according to claim 1 or 2, characterized in that: The anode in step 1) is single crystal silicon or polycrystalline silicon.
7. The method according to claim 1 or 2, characterized in that: In the step 1), the thickness of the cathode is 0.1 to 0.65 mm.
8. The method according to claim 1 or 2, characterized in that: In step 1), the electrolysis container includes a crucible and a vertical resistance furnace, and placing the electrolyte in the electrolysis container specifically includes: placing the electrolyte in the crucible, and then placing the crucible in the constant temperature area of the vertical resistance furnace.
9. The method according to claim 1 or 2, characterized in that: The crucible includes an iron crucible, a quartz crucible, a corundum crucible, a graphite crucible or a nickel crucible.
10. The method according to claim 1 or 2, characterized in that: The inert gas atmosphere is an atmosphere of argon or nitrogen with a purity of ≥99%.