Raw material for single crystal growth of samarium-doped lead magnesium niobate and lead titanate and preparation method thereof

In the preparation process of the raw materials for single crystal growth of samarium-doped lead niobium magnesium titanate, the problem of uneven component distribution is solved, significantly improving the The piezoelectric properties and mass of the crystal are reduced, and abnormal deviations in piezoelectric properties are reduced.

CN118910739APending Publication Date: 2024-11-08BEIJING SINOMA SYNTHETIC CRYSTALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410987487.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

Smart Images

  • Figure BDA0004957861760000091
    Figure BDA0004957861760000091
  • Figure BDA0004957861760000101
    Figure BDA0004957861760000101
  • Figure BDA0004957861760000102
    Figure BDA0004957861760000102
Patent Text Reader

Abstract

The invention provides a raw material for growth of a samarium-doped lead magnesium niobate and lead titanate single crystal, a preparation method of the raw material and the single crystal. Wherein the chemical composition of the raw material for growth of the samarium-doped lead magnesium niobate and lead titanate (Sm-PMNT) single crystal is Sm < x > Pb (1-1.5 x) [(Mg < 1 / 3 > Nb < 2 / 3 >) < 0.70 > Ti < 0.30 >] O3, and x is more than or equal to 0.005 and less than or equal to 0.02. According to the preparation method provided by the invention, millimeter-scale Sm2O3 grinding medium balls are prepared, the Sm2O3 grinding medium balls are adopted for ball milling, ball milling parameters are regulated and controlled, the single crystal raw material for Sm-PMNT growth is prepared through two-step sintering post-treatment, a proper amount of Sm2O3 can be uniformly doped into lead magnesium niobate and lead titanate, and the single crystal raw material for Sm-PMNT growth with uniformly distributed components is obtained. When the Sm-PMNT growth single crystal raw material prepared by the preparation method is used for crystal growth, the quality and piezoelectric property of the crystal can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of single crystal growth, and in particular to a raw material for growing samarium-doped lead magnesium niobate or lead titanate single crystals, a preparation method thereof, and a single crystal. Background Art

[0002] Ferroelectric crystal materials, especially the new relaxor ferroelectric single crystals represented by lead magnesium niobate lead titanate (PMNT), have excellent electromechanical coupling properties and are widely used in many fields. Studies have shown that their performance can be optimized by rare earth doping. Among them, after samarium (Sm) is doped into PMNT single crystals, the piezoelectric constant of the single crystal can be increased, and the piezoelectric performance is significantly improved, which has great potential in high-frequency medical imaging transducers and low-field drive actuators.

[0003] At present, the preparation of samarium-doped PMNT raw materials mainly adopts a two-step synthesis method: first, a magnesium niobate (MN) precursor is synthesized by a solid phase reaction of Nb2O5 and MgO, and then reacted with TiO2, PbO and Sm2O3 to obtain a samarium-doped lead magnesium niobate lead titanate (Sm-PMNPT) growth raw material. However, the crystals prepared by the Sm-PMNPT growth raw material obtained by the above preparation method have higher piezoelectric properties at the bottom of the crystal rod and lower piezoelectric properties at the top of the crystal rod, and an abnormal deviation in piezoelectric properties occurs. This is due to the uneven distribution of the components of the samarium-doped relaxor ferroelectric single crystal growth raw material, resulting in poor piezoelectric properties of the crystal. Therefore, providing an effective preparation method for the Sm-PMNPT growth raw material is the key to improving the crystal quality and piezoelectric properties. Summary of the invention

[0004] The purpose of this application is to provide a raw material for growing samarium-doped lead magnesium niobate and lead titanate single crystals, a preparation method and a single crystal, so as to improve the uneven distribution of raw material components for growing samarium-doped relaxor ferroelectric single crystals and improve the quality and piezoelectric properties of the crystals. The specific technical solution is as follows:

[0005] The first aspect of the present application provides a method for preparing a raw material for growing a samarium-doped lead magnesium niobate or lead titanate single crystal, wherein the chemical composition of the raw material for growing a samarium-doped lead magnesium niobate or lead titanate single crystal is Sm x Pb (1-1.5x) [(Mg 1 / 3Nb 2 / 3 ) 0.70 Ti 0.30 ]O3, 0.005≤x≤0.02. The preparation method comprises the following steps:

[0006] (1) The samarium oxide powder is pressed into a shape to form a ball blank.

[0007] (2) The ball blank is subjected to gas pressure sintering to obtain a rough ball.

[0008] (3) The rough ball is processed to obtain millimeter-sized Sm2O3 grinding balls.

[0009] (4) PbO, TiO2, and MgNb2O6 powders are weighed according to the stoichiometric ratio, mixed with Sm2O3 grinding balls, and wet ball milled to obtain a mixed powder; wherein the ball-to-material ratio is (1.2-1.6):1, the ball milling speed is 100-300 r / min, and the ball milling time is 10-24 h.

[0010] (5) The mixed powder is subjected to a two-step sintering post-treatment to obtain a raw material for growing samarium-doped lead magnesium niobate and lead titanate single crystals.

[0011] In some embodiments of the present application, the pressure of the pressing molding is 100-200 MPa, and the holding time of the pressing molding is 5-15 min.

[0012] In some embodiments of the present application, the sintering temperature of gas pressure sintering is 1600-1800° C., the holding time of gas pressure sintering is 2-4 hours, and the pressure of gas pressure sintering is 2-4 MPa.

[0013] In some embodiments of the present application, the diameter of the Sm2O3 grinding balls is 2-10 mm.

[0014] In some embodiments of the present application, the Sm2O3 grinding balls include large grinding balls, medium grinding balls and small grinding balls. The diameter of the large grinding balls is 8-10 mm, the diameter of the medium grinding balls is 5-7 mm, and the diameter of the small grinding balls is 2-4 mm.

[0015] In some embodiments of the present application, the mass of the large grinding balls, the medium grinding balls and the small grinding balls is (3-3.5):(2.5-3):1.

[0016] In some embodiments of the present application, the two-step sintering post-treatment includes a first sintering and a second sintering; the first sintering process is: heating from room temperature to 700-800°C for 160-200 minutes, then heating to 800-900°C for 340-380 minutes, keeping warm for 220-260 minutes, cooling to 280-320°C for 160-200 minutes, and then cooling to room temperature for 220-260 minutes; the second sintering process is: heating from room temperature to 800-900°C for 160-200 minutes, then heating to 850-950°C for 320-380 minutes, then heating to 1100-1200°C for 340-380 minutes, keeping warm for 100-140 minutes, cooling to 280-320°C for 160-200 minutes, and then cooling to room temperature for 220-260 minutes.

[0017] The second aspect of the present application provides a raw material for growing samarium-doped lead magnesium niobate and lead titanate single crystals, which is prepared according to the preparation method provided in the first aspect of the present application.

[0018] The third aspect of the present application is a samarium-doped lead magnesium niobate lead titanate single crystal, which is prepared using the samarium-doped lead magnesium niobate lead titanate single crystal growth raw material provided by the second aspect of the present application.

[0019] Beneficial effects of this application:

[0020] The present application provides a raw material for growing a samarium-doped lead magnesium niobate lead titanate single crystal, a preparation method thereof, and a single crystal, wherein the chemical composition of the raw material for growing a samarium-doped lead magnesium niobate lead titanate single crystal is Sm x Pb (1-1.5x) [(Mg 1 / 3 Nb 2 / 3 ) 0.70 Ti 0.30 ]O3, 0.005≤x≤0.02. In the preparation method provided in the present application, millimeter-level Sm2O3 grinding balls are prepared, Sm2O3 grinding balls are used for ball milling and the ball milling parameters are adjusted, and a single crystal raw material for Sm-PMNT growth is obtained by two-step sintering and post-treatment, and an appropriate amount of Sm2O3 can be uniformly added to lead magnesium niobate and lead titanate to obtain a single crystal raw material for Sm-PMNT growth with uniform component distribution. The single crystal raw material for Sm-PMNT growth obtained by the preparation method of the present application is used for single crystal growth, which can improve the abnormal deviation problem of the piezoelectric performance of the crystal and improve the piezoelectric performance of the crystal.

[0021] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0023] In the piezoelectric performance test of the Sm-PMNPT crystal obtained by the two-step synthesis method in the prior art, the piezoelectric performance at the bottom of the crystal rod is higher, and the piezoelectric performance at the top of the crystal rod is lower, and an abnormal deviation in the piezoelectric performance occurs. The inventors found that this is mainly because the dopant samarium oxide cannot be uniformly doped into PMNT, resulting in the enrichment of samarium oxide concentration, resulting in uneven composition of the raw materials for Sm-PMNPT growth, resulting in poor crystal quality and poor piezoelectric performance.

[0024] In view of this, the first aspect of the present application provides a method for preparing a raw material for growing a samarium-doped lead magnesium niobate or lead titanate single crystal, wherein the chemical composition of the raw material for growing a samarium-doped lead magnesium niobate or lead titanate single crystal is Sm x Pb (1-1.5x) [(Mg 1 / 3 Nb 2 / 3 ) 0.70 Ti 0.30 ]O3, 0.005≤x≤0.02, for example, the value of x can be 0.005, 0.006, 0.008, 0.01, 0.02, 0.15, 0.17, 0.02 or a range consisting of any two of the values. The preparation method comprises the following steps:

[0025] (1) The samarium oxide powder is pressed into a shape to form a ball blank.

[0026] (2) The ball blank is subjected to gas pressure sintering to obtain a rough ball.

[0027] (3) The rough ball is processed to obtain millimeter-sized Sm2O3 grinding balls.

[0028] (4) PbO, TiO2, and MgNb2O6 powders are weighed according to the stoichiometric ratio, mixed with Sm2O3 grinding balls, and wet ball milled to obtain a mixed powder.

[0029] (5) The mixed powder is subjected to a two-step sintering post-treatment to obtain a raw material for growing samarium-doped lead magnesium niobate and lead titanate single crystals.

[0030] The chemical composition of the raw material for growing samarium-doped lead magnesium niobate and lead titanate single crystals is shown above. The inventors have found that when the value of x is too small or too large, it is impossible to obtain a single crystal raw material for growing Sm-PMNT with uniform component distribution, which is not conducive to improving the performance of the crystal. Therefore, regulating the value of x within the above range is conducive to obtaining a single crystal raw material for growing Sm-PMNT with uniform component distribution, thereby improving the piezoelectric properties of the crystal.

[0031] In the present application, the ball-to-material ratio of wet ball milling is (1.2-1.6):1, the ball milling speed is 100-300r / min, and the ball milling time is 10-24h. For example, the ball-to-material ratio of wet ball milling can be 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, or a range consisting of any two values ​​therein, the ball milling speed can be 100r / min, 120r / min, 150r / min, 180r / min, 200r / min, 230r / min, 250r / min, 300r / min, or a range consisting of any two values ​​therein, and the ball milling time can be 10h, 12h, 15h, 17h, 20h, 22h, 24h, or a range consisting of any two values ​​therein. When the ball-to-material ratio is too small, for example, less than 1.2:1, the ball milling efficiency is poor and the powder mixing is uneven; when the ball-to-material ratio is too large, greater than 1.6:1, the powder ball milling efficiency will be reduced, and the powder mixing will also be uneven. By regulating the above parameters within the scope of this application, it is beneficial to incorporate the target content of Sm2O3 into lead magnesium niobate lead titanate (PMNT), and Sm2O3 can be uniformly incorporated into PMNT, improving the deviation and unevenness of the raw material components for Sm-PMNPT growth caused by the concentration enrichment of samarium oxide, thereby improving the quality and piezoelectric properties of the crystal.

[0032] In the preparation method provided in the present application, millimeter-sized Sm2O3 grinding balls are prepared, ball milling is performed using the Sm2O3 grinding balls, the ball milling parameters are adjusted, and a single crystal raw material for Sm-PMNT growth is obtained by two-step sintering and post-processing, so that the target content of Sm2O3 can be uniformly doped into PMNT to obtain a single crystal raw material for Sm-PMNT growth with uniform component distribution. The single crystal raw material for Sm-PMNT growth obtained by the preparation method of the present application is used for single crystal growth, which can improve the quality and piezoelectric properties of the crystal.

[0033] In the present application, the above step (1) may also include a pre-treatment step for the samarium oxide powder, and the above pre-treatment step may include but is not limited to: adding a binder to the samarium oxide for granulation, and then sieving to obtain the above samarium oxide powder. The above binder may be a polyvinyl alcohol (PVA) aqueous solution binder, based on the mass of the polyvinyl alcohol aqueous solution binder, the mass percentage of polyvinyl alcohol is 5%-12%, based on the mass of the samarium oxide powder, the mass percentage of the binder is 1% to 3%.

[0034] In the present application, after the samarium oxide powder is pressed and molded to obtain a ball blank, a debinding process may be further included, and the present application has no particular limitation on this, as long as the purpose of the present application can be achieved. For example, the ball blank may be kept at 600-650°C for 6-12 hours for debinding to remove the binder in the ball blank.

[0035] In some embodiments of the present application, the pressure of the pressing molding is 100-200Mpa, and the holding time of the pressing molding is 5-15min. For example, the pressure of the pressing molding can be 100Mpa, 120MPa, 150Mpa, 160MPa, 180MPa, 200Mpa or a range consisting of any two of the values, and the holding time of the pressing molding can be 5min, 7min, 10min, 11min, 12min, 13min, 15min or a range consisting of any two of the values. By regulating the pressure and holding time of the pressing molding within the above range, it is beneficial to better shape the ball blank to obtain high-quality samarium oxide grinding media balls, so that a single crystal raw material for Sm-PMNT growth with uniform component distribution can be obtained.

[0036] In some embodiments of the present application, the sintering temperature of gas pressure sintering is 1600-1800°C, the holding time of gas pressure sintering is 2-4 hours, and the pressure of gas pressure sintering is 2-4MPa. For example, the sintering temperature of gas pressure sintering can be 1600°C, 1650°C, 1700°C, 1750°C, 1800°C or a range consisting of any two values ​​therein, the holding time of gas pressure sintering can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours or a range consisting of any two values ​​therein, and the pressure of gas pressure sintering is 2MPa, 2.5MPa, 3MPa, 3.5MPa, 4MPa or a range consisting of any two values ​​therein. By regulating the sintering temperature, holding time and pressure of gas pressure sintering within the above range, it is beneficial to improve the density of samarium oxide grinding balls and obtain high-quality samarium oxide grinding balls, thereby obtaining single crystal raw materials for Sm-PMNT growth with uniform component distribution.

[0037] In some embodiments of the present application, the diameter of the Sm2O3 grinding ball is 2-10 mm. For example, the diameter of the Sm2O3 grinding ball can be 2 mm, 4 mm, 5 mm, 6 mm, 8 mm, 10 mm, or a range consisting of any two of these values. By regulating the diameter of the Sm2O3 grinding ball within the above range, it is beneficial to make the ball milling mixing more uniform, so that a single crystal raw material for Sm-PMNT growth with uniform component distribution can be obtained.

[0038] In some embodiments of the present application, the Sm2O3 grinding balls include large grinding balls, medium grinding balls and small grinding balls, the diameter of the large grinding balls is 8-10mm, the diameter of the medium grinding balls is 5-7mm, and the diameter of the small grinding balls is 2-4mm. For example, the diameter of the large grinding balls can be 8mm, 8.5mm, 9mm, 9.5mm, 10mm or a range consisting of any two of the values ​​therein, the diameter of the medium grinding balls can be 5mm, 5.5mm, 6mm, 6.5mm, 7mm or a range consisting of any two of the values ​​therein, and the diameter of the small grinding balls can be 2mm, 2.5mm, 3mm, 3.5mm, 4mm or a range consisting of any two of the values ​​therein. By regulating the diameters of the large grinding balls, the medium grinding balls and the small grinding balls within the above range, it is beneficial to make the ball milling mixture more uniform, so that a single crystal raw material for Sm-PMNT growth with uniform component distribution can be obtained, the abnormal deviation problem of the piezoelectric properties of the crystal can be improved, and the quality and piezoelectric properties of the crystal can be improved.

[0039] In some embodiments of the present application, the mass ratio of the large grinding balls, the medium grinding balls and the small grinding balls is (3-3.5): (2.5-3): 1, for example, the mass ratio of the large grinding balls, the medium grinding balls and the small grinding balls can be 3.3:2.5:1, 3:3:1, 3:2.6:1, 3.1:2.9:1, 3:2.8:1, 3.4:2.9:1 or a range consisting of any two of the values. By regulating the mass ratio of the large grinding balls, the medium grinding balls and the small grinding balls within the above range, the ball milling efficiency can be improved, the energy consumption during the ball milling process and the excessive wear of the grinding balls can be reduced, and at the same time, it is beneficial to improve the quality of the ball milling and the uniformity of samarium oxide, so that a single crystal raw material for Sm-PMNT growth with uniform component distribution can be obtained, the abnormal deviation problem of the piezoelectric performance of the crystal can be improved, and the quality and piezoelectric performance of the crystal can be improved.

[0040] In some embodiments of the present application, the two-step sintering post-treatment includes a first sintering and a second sintering; the first sintering process is: from room temperature to T1 = 700-800 ° C for 160-200 minutes, then to T2 = 800-900 ° C for 340-380 minutes, after 220-260 minutes of heat preservation, then to 280-320 ° C for 160-200 minutes, and then to 220-260 minutes of heat preservation. Room temperature; the second sintering process is: from room temperature to T3 = 800-900 ° C for 160-200 minutes, then to T4 = 850-950 ° C for 320-380 minutes, then to T5 = 1100-1200 ° C for 340-380 minutes, keep warm for 100-140 minutes, then cool to 280-320 ° C for 160-200 minutes, and then cool to room temperature for 220-260 minutes. For example, T1 can be 700°C, 720°C, 750°C, 770°C, 800°C or a range consisting of any two of them, T2 can be 800°C, 820°C, 850°C, 870°C, 900°C or a range consisting of any two of them, T3 can be 800°C, 820°C, 850°C, 870°C, 900°C or a range consisting of any two of them, T4 can be 850°C, 870°C, 900°C, 920°C, 950°C or a range consisting of any two of them, and T5 can be 1100°C, 1120°C, 1150°C, 1170°C, 1200°C or a range consisting of any two of them. The above two-step sintering post-treatment process can make the solid phase reaction between PbO, TiO2, MgNb2O6 and Sm2O3 more complete, so that a single crystal raw material for Sm-PMNT growth with uniform component distribution can be obtained.

[0041] In the present application, there is no particular restriction on the pressing and molding, as long as the purpose of the present application can be achieved. For example, a ball-making mold can be placed in a cold isostatic press for ball pressing to obtain a ball blank. The present application does not have any particular restrictions on the ball-making mold, and those skilled in the art can design and select according to actual needs, as long as the purpose of the present application can be achieved.

[0042] In the present application, there is no particular limitation on the atmosphere of gas pressure sintering, as long as the purpose of the present application can be achieved. For example, gas pressure sintering can be performed first in an argon atmosphere.

[0043] In the present application, there is no particular restriction on the process of processing the rough ball into the grinding ball, as long as the purpose of the present application can be achieved. For example, the rough ball can be processed by grinding. Specifically, the rough ball is coarsely ground and finely ground by a disc grinder during the grinding process to obtain millimeter-level Sm2O3 grinding balls. Generally, when preparing Sm2O3 grinding balls according to the above process, the diameter of the Sm2O3 grinding balls can be controlled by adjusting parameters such as grinding time, grinding speed, and grinding media. The present application has no particular restrictions on this, and those skilled in the art can make adjustments according to actual needs, as long as the purpose of the present application can be achieved.

[0044] In the present application, the PbO, TiO2, and MgNb2O6 powders are preferably high-purity powders with a purity of 99.99%. The present application has no particular restrictions on the solvent for wet ball milling, as long as the invention purpose of the present application can be achieved. For example, alcohol can be used as the solvent for wet ball milling.

[0045] The present application has no particular restrictions on the equipment used for the two-step sintering post-treatment, as long as the purpose of the present application can be achieved. For example, the mixed powder can be placed in a corundum crucible, covered and sealed, and placed in a box-type electric furnace for the first sintering and the second sintering treatment.

[0046] The second aspect of the present application provides a raw material for growing samarium-doped lead magnesium niobate or lead titanate single crystals, which is prepared according to the preparation method provided in the first aspect of the present application, so that the raw material for growing Sm-PMNPT has uniform components.

[0047] The third aspect of the present application is a samarium-doped lead magnesium niobate lead titanate single crystal, which is prepared using the samarium-doped lead magnesium niobate lead titanate single crystal growth raw material provided in the second aspect of the present application. The raw material for growing the Sm-PMNPT single crystal provided in the second aspect of the present application has uniform components, so that the Sm-PMNPT single crystal prepared using the raw material has high quality and good piezoelectric properties, thereby improving the problem of abnormal deviation of piezoelectric properties.

[0048] In the present application, the above-mentioned samarium-doped lead magnesium niobate lead titanate single crystal is prepared by a crucible descent method, and the present application has no particular limitation on this, as long as the purpose of the present application can be achieved.

[0049] Example

[0050] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0051] Test methods and equipment:

[0052] Inductively coupled plasma optical emission spectroscopy test:

[0053] At room temperature, the Sm-PMNT single crystal raw materials prepared in the examples and comparative examples were tested using an inductively coupled plasma mass spectrometer (ICP-MS, Agilent 7700). The Sm-PMNT single crystal raw materials prepared in each example and comparative example were randomly sampled from three different positions in the crucible, marked as A, B and C, and analyzed by inductively coupled plasma emission spectrometry to obtain the content of each element, and inversely deduce the chemical composition of the Sm-PMNT single crystal raw materials for growth.

[0054] Piezoelectric testing:

[0055] The Sm-PMNT or PMNT single crystal raw materials for growth prepared in each embodiment and comparative example were placed in a platinum crucible, and the platinum crucible was placed in a crystal growth furnace. The crystal was grown by a crucible descent method at a temperature of 1300° C. and a descent rate of 20 mm / day to obtain a Sm-PMNT relaxor ferroelectric crystal. The sample size was: 5.59 cm in diameter and 12 cm in length. The ZJ-4AN quasi-static d 33 The measuring instrument tests the piezoelectric constant d at the bottom of the crystal 33 and the piezoelectric constant d at the top of the crystal 33 '. The upper end of the crystal taken out from the crystal growth furnace is the top of the crystal, and the lower end is the bottom of the crystal. The sampling position of the top of the crystal is 1 cm away from the upper end, and the sampling position of the bottom of the crystal is 1 cm away from the lower end.

[0056] Compared with PMNT without Sm doping, the more the piezoelectric constants at the top and bottom of the crystal increase, the better the piezoelectric performance; the lower the piezoelectric constants at the top and bottom of the crystal, the worse the piezoelectric performance. Abnormal piezoelectric performance deviations at the top and bottom also indicate poor piezoelectric performance. Usually, for PMNT without Sm doping, the bottom piezoelectric constant is lower than the top piezoelectric constant. When Sm is doped, if the piezoelectric constant at the bottom of the crystal is higher than the piezoelectric constant at the top, it is considered that there is an abnormal piezoelectric performance deviation problem. The greater the difference between the piezoelectric constants at the bottom and the top, the more obvious the abnormal piezoelectric performance deviation problem is.

[0057] Example 1

[0058] Chemical composition: Sm 0.01 Pb 0.985 [(Mg 1 / 3 Nb 2 / 3 ) 0.7 Ti 0.3 The method for preparing a raw material for growing a relaxor ferroelectric single crystal of ]O3 (i.e., a single crystal raw material for growing Sm-PMNT) comprises the following steps:

[0059] (1) Add 8% by weight of polyvinyl alcohol (PVA) aqueous solution binder to samarium oxide powder, granulate, and sieve through a 50-mesh standard sieve. Based on the mass of the samarium oxide powder, the mass percentage of the binder is 1%. Then, the sieved samarium oxide powder is loaded into spherical ball molds with diameters of 3 mm, 9 mm, and 15 mm, respectively, and placed in a cold isostatic press for ball pressing to obtain small grinding ball blanks, medium grinding ball blanks, and large grinding ball blanks. The pressing pressures are 120 MPa, 160 MPa, and 180 MPa, respectively, and the holding time is 5 min, 8 min, and 10 min, respectively. Then, the powder is placed in a box-type electric furnace and kept at 650°C for 10 hours for debinding treatment.

[0060] (2) The ball blank obtained in step (1) is placed in an argon atmosphere pressure sintering furnace for gas pressure sintering to obtain a blank ball. The sintering temperature is 1700° C., the pressure is 3 MPa, and the holding time is 2 hours.

[0061] (3) The rough balls prepared above are subjected to two steps of coarse grinding and fine grinding to obtain small grinding balls with a diameter of 2 mm, medium grinding balls with a diameter of 6 mm, and large grinding balls with a diameter of 10 mm, i.e., millimeter-grade Sm2O3 grinding balls.

[0062] (4) High-purity (purity of 99.99%) powdered MgNb2O6, PbO and TiO2 are weighed and mixed according to the stoichiometric ratio, and then the Sm2O3 grinding balls prepared in the above step and alcohol are added to perform wet ball milling to obtain slurry, and the slurry is dried to obtain a mixed powder. The Sm2O3 grinding balls used include the large grinding balls, medium grinding balls and small grinding balls prepared above, the mass ratio of the large grinding balls, medium grinding balls and small grinding balls is 3.3:2.5:1, the ball-to-material ratio is 1.5:1, the ball-to-material ratio is 190 r / min, and the ball milling time is 18 h.

[0063] (5) The mixed powder is placed in a corundum crucible, which is sealed with a lid and placed in a box-type electric furnace. The temperature is raised from room temperature to T1 = 750 ° C over 180 min, then raised to T2 = 850 ° C over 360 min, kept at this temperature for 240 min, then cooled to 300 ° C over 180 min, and then cooled to room temperature over 240 min.

[0064] (6) The sintered material of step (5) is sintered for a second time, heating from room temperature to T3 = 850°C over 180 minutes, heating to T4 = 900°C over 360 minutes, heating to T5 = 1100°C over 360 minutes, and keeping the temperature for 120 minutes, cooling to 300°C over 180 minutes, and cooling to room temperature over 240 minutes to obtain a single crystal raw material for Sm-PMNT growth.

[0065] Example 2 to Example 7

[0066] Except for adjusting the parameters according to Table 1, the rest is the same as Example 1.

[0067] Example 8

[0068] Except that only medium grinding balls with a diameter of 6 mm were used in wet ball milling, the rest was the same as in Example 1.

[0069] Comparative Example 1

[0070] The chemical composition is Sm 0.01 Pb 0.985 [(Mg 1 / 3 Nb 2 / 3 ) 0.7 Ti 0.3 The method for preparing a raw material for growing a relaxor ferroelectric single crystal of ]O3 comprises the following steps:

[0071] (1) High-purity powdered MgO and Nb2O5 were mixed in a stoichiometric ratio and sintered at 1200°C for 6 h to synthesize the precursor MgNb2O6.

[0072] (2) High-purity powdered Sm2O3, PbO, TiO2 and the above-prepared precursor MgNb2O6 are mixed in a stoichiometric ratio, and the above raw materials are mixed through a 16-mesh sieve using a sieving mixing method, sieved twice, and evenly mixed to obtain an initial raw material.

[0073] (3) The initial raw materials are placed in a crucible, which is sealed with a lid and placed in a high-temperature frit furnace. The temperature is raised from room temperature to 750°C over 180 minutes, then raised to 850°C over 360 minutes, kept at that temperature for 180 minutes, then lowered to 300°C over 180 minutes, and then lowered to room temperature over 240 minutes to obtain a sintered material.

[0074] (4) Sintering synthesis is performed again under the following conditions: the sintered material is heated from room temperature to 850°C over 180 minutes, then heated to 900°C over 360 minutes, then heated to 1100°C over 360 minutes and kept at this temperature for 120 minutes, then cooled to 300°C over 180 minutes, and then cooled to room temperature over 240 minutes to obtain a raw material for growing samarium-doped lead magnesium niobate lead titanate (Sm-PMNT) single crystals.

[0075] Comparative Example 2

[0076] The chemical composition is 0.67[Pb(Mg 1 / 3 Nb 2 / 3 The method for preparing a raw material for growing a relaxor ferroelectric single crystal of )O3]-0.33(PbTiO3) comprises the following steps:

[0077] (1) High-purity powdered MgNb2O6, PbO and TiO2 are weighed and mixed according to a stoichiometric ratio, zirconium oxide grinding balls and alcohol are added, and wet ball milling is performed to obtain a slurry, and the slurry is dried to obtain a mixed powder. The zirconium oxide grinding balls used include large grinding balls with a diameter of 10 mm, medium grinding balls with a diameter of 6 mm and small grinding balls with a diameter of 2 mm. The mass ratio of the large grinding balls, the medium grinding balls and the small grinding balls is 3:3:1, the ball-to-material ratio is 1.5:1, the ball milling speed is 150 r / min, and the time is 18 h.

[0078] (2) The mixed powder is placed in a corundum crucible, which is sealed with a lid and placed in a box-type electric furnace. The temperature is raised from room temperature to T1 = 800°C over 180 minutes, and then raised to T2 = 850°C over 360 minutes. After keeping the temperature for 240 minutes, the temperature is lowered to 300°C over 180 minutes, and then lowered to room temperature over 240 minutes.

[0079] (3) The sintered material of step (2) is sintered for a second time, heating from room temperature to T3 = 850°C over 180 minutes, heating to T4 = 900°C over 360 minutes, heating to T5 = 1150°C over 360 minutes, and keeping the temperature for 120 minutes, cooling to 300°C over 180 minutes, and cooling to room temperature over 240 minutes to obtain single crystal raw material for PMNT growth.

[0080] The relevant parameters of each embodiment and comparative example are shown in Table 1 and Table 2.

[0081] Table 1

[0082]

[0083]

[0084] Note: “ / ” in Table 1 means there is no corresponding parameter.

[0085] Table 2

[0086]

[0087] Note: " / " in Table 2 means there is no corresponding parameter.

[0088] It can be seen from Examples 1 to 8 and Comparative Examples 1 to 2 that the relative error between the measured value of the mass percentage of the Sm element and the target value in the single crystal raw material for Sm-PMNT growth obtained by the preparation method provided by the present application is small, especially in Examples 1 to 7, the relative error between the measured value of the mass percentage of the Sm element and the target value is less than 10%; and the measured values ​​of the mass percentage of the Sm element at different points A, B, and C are relatively close. This shows that in the preparation method of the present application, the realization of efficient doping of samarium oxide by ball milling makes the actual chemical composition of the Sm element component in the single crystal raw material for Sm-PMNT growth highly consistent with the pre-designed chemical composition, and the overall uniformity of the powder is significantly improved, which is conducive to the growth of high-quality Sm-PMNT relaxor ferroelectric single crystals, so that the piezoelectric constants of the bottom and top of the obtained crystals are relatively close. In the single crystal raw material for Sm-PMNT growth prepared by the conventional synthesis method used in Comparative Example 1, there is a significant difference between the mass percentage of the Sm element and the target value, the average relative error of the mass percentage of the Sm element is as high as 61.814%, and the measured values ​​of the mass percentage of the Sm element at different A, B, and C points are quite different, indicating that the powder uniformity of the single crystal raw material for Sm-PMNT growth prepared by this method is very poor. Compared with Comparative Example 2, the piezoelectric constant at the bottom of the crystal in Comparative Example 1 is greatly increased, while the piezoelectric constant at the top of the crystal is reduced, and the difference between the piezoelectric constants at the bottom and the top of the crystal is too large, resulting in obvious abnormal deviation of piezoelectric performance. Compared with Comparative Example 2, the piezoelectric constants at the bottom and top of the crystal of Example 8 are both improved, among which the piezoelectric constant at the bottom is improved more, and the piezoelectric constant at the top is improved less, and there is a slight abnormal deviation problem in the piezoelectric performance. However, the relative error between the measured value of the mass percentage of the Sm element and the target value is smaller than that in Comparative Example 1, and the difference between the piezoelectric constants at the top and bottom is also smaller than that in Comparative Example 1, indicating that compared with Comparative Example 1, the abnormal deviation problem of the piezoelectric performance of the crystal in Example 8 is improved.

[0089] The preparation method provided in the present application can effectively reduce the composition deviation of the Sm element in the single crystal raw material for Sm-PMNT growth, so that the composition of the single crystal raw material for Sm-PMNT growth actually prepared is highly consistent with the chemical composition of the original design, thereby being beneficial to the growth of Sm-PMNT relaxor ferroelectric single crystals and improving the quality and piezoelectric properties of the crystals.

[0090] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method or article including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method or article.

[0091] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing a raw material for growing samarium-doped lead magnesium niobate and lead titanate single crystals, wherein: The chemical composition of the raw material for growing the samarium-doped lead magnesium niobate titanium single crystal is Sm x Pb (1-1.5x) [(Mg 1 / 3 Nb 2 / 3 ) 0.70 Ti 0.30 ]O3, 0.005≤x≤0.02; The preparation method comprises the following steps: (1) pressing the samarium oxide powder into a ball blank; (2) sintering the ball blank under gas pressure to obtain a rough ball; (3) processing the rough ball to obtain a millimeter-sized Sm2O3 grinding ball; (4) weighing PbO, TiO2, and MgNb2O6 powders according to the stoichiometric ratio, mixing them with the Sm2O3 grinding balls, and performing wet ball milling to obtain a mixed powder; wherein the ball-to-material ratio is (1.2-1.6):1, the rotation speed of the ball mill is 100-300 r / min, and the ball milling time is 10-24 h; (5) The mixed powder is subjected to a two-step sintering post-treatment to obtain the raw material for growing the samarium-doped lead magnesium niobate and lead titanate single crystal.

2. The preparation method according to claim 1, wherein The pressing pressure is 100-200 MPa, and the holding time of the pressing is 5-15 min.

3. The preparation method according to claim 1, wherein The sintering temperature of the gas pressure sintering is 1600-1800° C., the heat preservation time of the gas pressure sintering is 2-4 hours, and the pressure of the gas pressure sintering is 2-4 MPa.

4. The preparation method according to claim 1, wherein The diameter of the Sm2O3 grinding balls is 2-10 mm.

5. The preparation method according to claim 1, wherein The Sm2O3 grinding balls include large grinding balls, medium grinding balls and small grinding balls. The diameter of the large grinding balls is 8-10 mm, the diameter of the medium grinding balls is 5-7 mm, and the diameter of the small grinding balls is 2-4 mm.

6. The preparation method according to claim 5, wherein: The mass of the large grinding balls, the medium grinding balls and the small grinding balls is (3-3.5):(2.5-3):

1.

7. The preparation method according to claim 1, wherein The two-step sintering post-treatment includes a first sintering and a second sintering; The first sintering process is: heating from room temperature to 700-800°C for 160-200 minutes, then heating to 800-900°C for 340-380 minutes, keeping the temperature for 220-260 minutes, cooling to 280-320°C for 160-200 minutes, and then cooling to room temperature for 220-260 minutes; The second sintering process is: heating from room temperature to 800-900°C for 160-200 minutes, then heating to 850-950°C for 320-380 minutes, then heating to 1100-1200°C for 340-380 minutes and keeping the temperature for 100-140 minutes, then cooling to 280-320°C for 160-200 minutes, and then cooling to room temperature for 220-260 minutes.

8. A raw material for growing samarium-doped lead magnesium niobate or lead titanate single crystals, which is obtained according to the preparation method described in any one of claims 1 to 7.

9. A samarium-doped lead magnesium niobate lead titanate single crystal, which is prepared by using the samarium-doped lead magnesium niobate lead titanate single crystal growth raw material according to claim 8.