Finishing method for synchronously realizing in-situ dyeing and flame retardance
By using laccase to catalyze the copolymerization of plant phenols and organophosphorus compounds on protein fiber fabrics, the problem of fabric damage caused by traditional dyeing and flame retardant methods is solved, achieving environmentally friendly and efficient simultaneous dyeing and flame retardant effects.
Patent Information
- Application Number
- CN202411149272.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Traditional dyeing and flame retardant methods cause significant damage to protein fiber fabrics and are energy and water consuming. Therefore, we are looking for environmentally friendly and efficient methods for simultaneous dyeing and flame retardant treatment.
Laccase is used to catalyze the copolymerization of plant phenols and organophosphorus compounds, achieving simultaneous dyeing and flame retardancy on protein fiber fabrics through in-situ reaction. The catalytic oxidation of laccase enables the copolymerization and cross-linking of plant phenols and organophosphorus compounds on protein fibers.
Dyeing and flame retardancy were achieved simultaneously under mild conditions, improving the color fastness and flame retardant effect of the fabric, reducing harm to the environment and human body, and maintaining the hand feel and mechanical properties of the fiber.
Smart Images

Figure CN118910904A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of simultaneous dyeing and flame retardancy, and in particular relates to a finishing method for simultaneous in-situ dyeing and flame retardancy. Background Art
[0002] Protein fibers in the textile field mainly include silk, wool, etc. They have excellent moisture absorption and air permeability and are suitable for making clothing and home textile products. In recent years, with the development of the economy, wig products have become more and more popular among beauty-conscious people, and wigs made of human hair are healthier and more comfortable, and are deeply favored by consumers. The physical and chemical structure of human hair is similar to that of wool, and it is also a kind of protein fiber. The traditional dyeing and durable flame retardant treatment methods of protein fiber fabrics require harsh conditions. For example, traditional dyeing methods generally require high temperatures, consume a lot of energy, and damage the properties of fibers or fabrics. A large amount of chemicals are also consumed during the dyeing process.
[0003] Durable flame retardancy of protein fiber / fabric is generally achieved by high-temperature baking with phosphorus-containing compounds in the presence of a crosslinking agent. Wool fiber fabrics can also be treated with metal complexes such as potassium hexafluorotitanate, but the above finishing methods can cause yellowing of the fabric, strong damage, or heavy metal pollution. Therefore, finding an environmentally friendly and efficient dyeing and flame retardant finishing method for protein fibers has attracted the attention of more and more researchers. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a finishing method for achieving in-situ dyeing and flame retardancy simultaneously, using laccase, plant phenol and organic phosphorus copolymerization, and reacting with the material to be finished to simultaneously give it color and flame retardancy, and the method is simple and feasible. The technical solution adopted is:
[0005] A finishing method for achieving simultaneous in-situ dyeing and flame retardancy, comprising the following steps:
[0006] (1) Add methanol / acetic acid-sodium acetate buffer solution as solvent into a conical flask, and place the conical flask in a shaking water bath and heat it to 50-80°C;
[0007] (2) adding plant phenol, organophosphorus compound and laccase into a conical flask in sequence, shaking well to obtain a mixed solution, and then adding the object to be treated;
[0008] (3) Oscillate the conical flask, maintain the water bath temperature at 50-80°C, and continue the reaction;
[0009] (4) After the reaction is completed, the material to be treated is soaked and cleaned with warm water and cold water, and then dried.
[0010] Preferably, the material to be finished is any one or more of wool fiber fabric, silk fabric and human hair fiber.
[0011] Preferably, the mass concentration of methanol in the solvent methanol / acetic acid-sodium acetate buffer solution is 5-20%; and its pH is 4-6.
[0012] Preferably, the plant phenols are phenolic acids, flavonoids and lignins, etc.; the organophosphorus compounds are organophosphorus compounds containing PH bonds.
[0013] Preferably, the plant phenol is any one of gallic acid, tea polyphenols, and tannin; the organophosphorus compound containing a PH bond is any one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), dimethyl phosphite, and diethyl phosphite.
[0014] Preferably, the activity of laccase in the mixed solution uniformly mixed in step (2) is 0.1-5 U / mL.
[0015] Preferably, the molar ratio of plant phenol to organophosphorus compound in the mixed solution in step (2) is 1:1 to 2.5.
[0016] Preferably, in step (3), the reaction time is 8 to 24 hours.
[0017] Preferably, in step (4), the warm water is water at 50-60°C, and the cold water is water at 0-10°C.
[0018] Preferably, the soaking time in warm water and cold water is 20 to 30 minutes; finally, the product is washed with cold water for 3 to 5 times and dried in an oven at 40 to 60°C.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention proposes a method for realizing in-situ dyeing and flame retardant simultaneously, and a method for durable in-situ dyeing and flame retardant synchronous finishing. The process flow is simple, plant phenol and organic phosphorus compound are used as catalyzed substrates, and the plant phenol and organic phosphorus compound are copolymerized and colored by means of the catalytic oxidation of laccase, and react with wool fiber fabrics, silk fabrics and human hair fibers, and the dyeing and flame retardant effects are successfully given to them without affecting the hand feel, and the breaking strength of the fiber or fabric can be enhanced;
[0021] Using laccase as a catalyst can achieve simultaneous finishing of dyeing and flame retardant functions. The process is simple and avoids the problems of water consumption, energy consumption, pollution and fiber or fabric damage caused by traditional dyeing and flame retardant finishing.
[0022] Plant phenols or organic phosphorus compounds form a stable cross-linking grafting effect with protein fibers / fabrics, which greatly improves the color fastness of dyed fabrics and the washability of the flame retardant effect.
[0023] Organophosphorus compounds have good stability and do not release large amounts of toxic gases or smoke during combustion, thus reducing harm to the environment and human body.
[0024] The reaction conditions of enzyme-catalyzed polymerization are mild. Compared with traditional chemical dyeing and flame-retardant modification methods, this process causes less damage to protein fibers. The protein fibers after dyeing and flame-retardant modification can still maintain their original soft and fluffy feel. At the same time, the cross-linking effect of plant phenols inside the protein fibers significantly improves the mechanical properties of the fabric. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The dyeing pictures of the blank wool fabric (a) and the wool fabric finished by Example 1 of the present invention (b) are compared.
[0026] Figure 2 The dyeing pictures of the blank silk fabric (a) and the silk fabric treated by Example 3 of the present invention (b) are compared.
[0027] Figure 3 The figures are a comparison of blank dyed hair (a) and dyed human hair (b) after being treated by Example 4 of the present invention.
[0028] Figure 4 This is a graph showing the changes in the flame retardant properties of human hair, where a: the original sample was exposed to the flame for 1 second; b: the original sample was ignited for 10 seconds; c: the sample was ignited for 1 second after finishing; d: the sample was ignited for 10 seconds after finishing. DETAILED DESCRIPTION
[0029] The accompanying drawings are only for illustrative purposes. The present invention is described in detail below in conjunction with the accompanying drawings. Unless otherwise specified in the present invention, the raw materials used can be purchased through conventional commercial channels.
[0030] Example 1
[0031] Add 200 mL of methanol / acetic acid-sodium acetate buffer solution solvent (methanol mass concentration: 10%; pH = 5) into a conical flask, place the conical flask in an oscillating water bath, and heat it to 50°C; then add 5 g of gallic acid, 5 g of DOPO, and 2.87 g of laccase in sequence, mix well, and then add 4 g of wool fabric; oscillate the conical flask, keep the water bath temperature at 50°C unchanged, and react for 12 hours; after the reaction is completed, soak and wash the wool fabric with warm water and cold water in turn, and then dry it.
[0032] The LOI (Limiting Oxygen Index) of the finished fabric was tested according to GB / T5454-1997 "Textile Combustion Performance Test: Oxygen Index Method". The results are shown in Table 1.
[0033] Table 1 Comparison of dyeing effect and flame retardant effect of wool fabric before and after treatment
[0034] sample Blank wool fabric Finished wool fabric K / S(360nm) 1.18 5.92 LOI(%) 26.0 27.5
[0035] Through Table 1 and Figure 1 It can be seen that the dyeing effect and flame retardant effect of the wool fabric after being finished in the embodiment are significantly improved.
[0036] According to AATCC-61 "Color Fastness to Washing: Quick Method", the dyed and flame-retardant modified wool fabrics were washed. The specific process is as follows: the sample was immersed in a 0.15% AATCC standard detergent aqueous solution, and washed at 49°C for 45 minutes with shaking (this process is a washing cycle, equivalent to 5 home washings). A sample was taken out in each cycle, and after drying, the surface color depth (K / S value) and combustion performance (LOI value) were tested to characterize the changes in the dyeing and flame-retardant properties of the fabric after different times of washing. Table 2 shows the effect of the number of washings on the dyeing and flame-retardant properties of the dyed and flame-retardant wool fabrics.
[0037] Table 2 Effect of washing times on dyeing and flame retardant properties of wool fabrics after dyeing and flame retardant
[0038] Washing times 0 5 10 15 20 25 K / S(360nm) 5.92 5.62 5.36 5.26 5.21 5.19 LOI(%) 27.5 27.3 27.3 27.2 27.2 27.2
[0039] According to GB / T5454-1997, when the LOI of the fabric is ≥26%, it is classified as a flame retardant material. From the results in Table 2, it can be seen that the LOI of the fabric is still 27.2% after washing 25 times. Therefore, the wool fabric treated by the method of the present invention has good flame retardancy and durability.
[0040] Example 2
[0041] Add 200 mL of methanol / acetic acid-sodium acetate buffer solution solvent (methanol mass concentration: 10%; pH = 5) into a conical flask, place the conical flask in an oscillating water bath, and heat it to 50°C; then add 20 g of tea polyphenols, 20 g of DOPO, and 2.87 g of laccase in sequence, mix well, and then add 4 g of wool fabric; oscillate the conical flask, keep the water bath temperature at 50°C unchanged, and react for 24 hours; after the reaction is completed, soak and wash the silk fabric with warm water and cold water in turn, and dry it.
[0042] The LOI (Limiting Oxygen Index) of the finished fabric was tested according to GB / T5454-1997 "Textile Combustion Performance Test: Oxygen Index Method". The results are shown in Table 3. Table 3 is a comparison of the dyeing effect and flame retardant effect of the wool fabric before and after treatment. The dyeing effect and flame retardant effect of the finished wool fabric are better than those of the blank wool fabric.
[0043] Table 3 Comparison of dyeing effect and flame retardant effect of silk fabrics before and after treatment
[0044] sample Blank wool fabric Finished wool fabric K / S(360nm) 1.18 6.68 LOI(%) 26.0 29.1
[0045] Example 3
[0046] Add 200 mL of methanol / acetic acid-sodium acetate buffer solution solvent (methanol mass concentration: 10%; pH = 5) into a conical flask, place the conical flask in an oscillating water bath, and heat it to 50°C; then add 10 g of gallic acid, 10 g of DOPO, and 2.87 g of laccase in sequence, mix well, and then add 4 g of silk fabric; oscillate the conical flask, keep the water bath temperature at 50°C unchanged, and react for 12 hours; after the reaction is completed, soak and wash the silk fabric with warm water and cold water in turn, and dry it.
[0047] The LOI (Limiting Oxygen Index) of the finished fabric was tested according to GB / T5454-1997 "Textile Combustion Performance Test: Oxygen Index Method". The results are shown in Table 4.
[0048] Table 4 Comparison of dyeing effect and flame retardant effect of silk fabrics before and after treatment
[0049] sample Blank silk fabric Finished silk fabric K / S(360nm) 0.35 3.68 LOI(%) 24.5 26.2
[0050] according to Figure 2 As shown in Table 4, compared with the untreated blank silk fabric, the silk fabric treated in Example 3 has improved dyeing effect and flame retardant effect.
[0051] Example 4
[0052] Add 200 mL of methanol / acetic acid-sodium acetate buffer solution solvent (methanol mass concentration: 10%; pH = 5) into a conical flask, place the conical flask in an oscillating water bath, and heat it to 50°C; then add 5 g of gallic acid, 5 g of DOPO, and 2.87 g of laccase in sequence, mix well, and then add 4 g of human hair fiber; oscillate the conical flask, keep the water bath temperature at 50°C unchanged, and react for 12 hours; after the reaction is completed, soak and wash the human hair with warm water and cold water in turn, and dry it.
[0053] Data color spectrophotometer (D65 light source, 10° field of view) was used to measure the color characteristic value (K / S) of human hair before and after treatment using a large aperture (30mm). Each sample was randomly measured at different measurement positions and the average value was calculated to obtain the K / S value of different dyed samples. Figure 3 Table 5 shows the K / S value and dyeing effect diagram of human hair fiber before and after treatment.
[0054] Table 5 Comparison of dyeing effects of human hair fabrics before and after treatment
[0055] sample Blank human hair fibers Finished human hair fibers K / S(360nm) 7.01 18.13
[0056] Depend on Figure 3 As shown in Table 5, compared with the untreated blank human hair fibers, the dyeing effect of the human hair fibers treated in Example 4 is improved.
[0057] like Figure 4 As shown, the state of human hair fiber is not convenient for limited oxygen index test. The present invention characterizes the change of flame retardant performance of human hair by comparing the vertical combustion performance of human hair before and after treatment. Figure a shows that the original sample (i.e. blank human hair fiber sample) is exposed to flame for 1 second, the dyeing is not obvious, and the bottom is just about to start burning; Figure b shows that the original sample is burned after 10 seconds, and the burning is obvious and not vertical; Figure c shows that the human hair sample after finishing in Example 4 is burned for 1 second, and it remains vertical even after burning; Figure d shows that the bottom of the sample after 10 seconds is burned, but it still remains vertical, and the upper part is not burned, indicating that the flame retardant performance of the finished human hair fabric is better.
[0058] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A finishing method for achieving simultaneous in-situ dyeing and flame retardancy, characterized in that: The following steps are involved: (1) Add methanol / acetic acid-sodium acetate buffer solution as solvent into a conical flask, and place the conical flask in a shaking water bath and heat it to 50-80° C.; (2) adding plant phenol, organophosphorus compound and laccase into a conical flask in sequence, shaking well to obtain a mixed solution, and then adding the object to be treated; (3) Oscillate the conical flask, maintain the water bath temperature at 50-80°C, and continue the reaction; (4) After the reaction is completed, the material to be treated is soaked and cleaned with warm water and cold water, and then dried.
2. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 1, characterized in that: The material to be finished is any one or more of wool fiber fabric, silk fabric and human hair fiber.
3. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 2, characterized in that: The mass concentration of methanol in the solvent methanol / acetic acid-sodium acetate buffer solution is 5-20%; and its pH is 4-6.
4. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 2, characterized in that: The plant phenols are phenolic acids, flavonoids and lignins; the organic phosphorus compounds are organic phosphorus compounds containing PH bonds.
5. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 4, characterized in that: The plant phenol is any one of gallic acid, tea polyphenols and tannin; the organic phosphorus compound containing PH bond is any one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, dimethyl phosphite and diethyl phosphite.
6. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 2, characterized in that: The activity of laccase in the mixed solution uniformly mixed in the step (2) is 0.1-5 U / mL.
7. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 2, characterized in that: The molar ratio of plant phenol to organophosphorus compound in the mixed solution in step (2) is 1:1-2.
5.
8. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 2, characterized in that: In the step (3), the reaction time is 8 to 24 hours.
9. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 2, characterized in that: In the step (4), the warm water is water at 50 to 60°C, and the cold water is water at 0 to 10°C.
10. The method for simultaneously achieving in-situ dyeing and flame retardancy according to claim 9, characterized in that: The soaking time in warm water and cold water is 20 to 30 minutes each; finally, rinse with cold water 3 to 5 times and dry in an oven at 40 to 60°C.
Citation Information
Patent Citations
Linen fiber biologic dyeing process based on laccase catalysis polymerization color generation reaction
CN103952927A
Super-hydrophobic anti-ultraviolet flame-retardant silk fabric and preparation method thereof
CN109736082A
Process for partial delignification and filling of a lignocellulosic material, and composite structure able to be obtained by this process
IN201817022033A
Synergistic flame retardant compositions and fiber blends including the same
US20200056057A1
Method for Improving Strength and Dyeing of Wool Fibers
US20220356643A1