Rapid method for digesting high-phosphorus iron ore by wet process

Through mixed acid wet digestion and two-stage heating treatment, combined with multiple analytical methods, the problem of long-term decomposition of high phosphate iron ore is solved, and fast and accurate elemental analysis is achieved, suitable for large-scale industrial production and improved resource utilization Rate.

CN118913811AActive Publication Date: 2024-11-08HUBEI XINGFA CHEM GRP CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410522788.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-08
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The existing high-phosphorus iron ore decomposition methods are time-consuming and energy-saving, making it difficult to meet the needs of rapid detection and analysis, affecting the accuracy of elemental analysis and resource utilization.

Method used

The mixed acid wet digestion method is adopted, and the proportion optimization of perchloric acid and sulfuric acid and the addition of oxalic acid, combined with two sections of heating treatment, the complete decomposition of high phosphate iron ore is achieved, and potassium dichromate titration method and quinomolyte lemon Elemental analysis was performed by ketone weight method and ICP standard curve method.

Benefits of technology

It improves the rapid digestion efficiency of high-phosphorus iron ore, ensures the accuracy of multi-element analysis, is suitable for large-scale industrial production, reduces the volatile loss and insoluble residues of the components to be tested, and improves the detection efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

According to the rapid method for digesting the high-phosphorus iron ore by the wet method, the high-phosphorus iron ore can be rapidly and accurately decomposed, so that the test requirements of scientific research and industrial production on multi-element analysis of the high-phosphorus iron ore are met. According to the method, the high-phosphorus iron ore difficult to digest is decomposed by adopting a mixed acid digestion method, the adding proportion of each acid is optimized, the optimal decomposition condition is determined, the contents of iron and phosphorus elements in the high-phosphorus iron ore are respectively determined by adopting a potassium dichromate titration method and a quimocion gravimetric method, and meanwhile, the contents of impurity elements in the ore are analyzed by utilizing an ICP standard curve method. Experimental results show that the sample is completely decomposed and the determination result is reliable. The method is rapid, convenient and good in reproducibility, and an accurate and rapid method is provided for daily batch analysis of the high-phosphorus iron ore.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of mineral analysis. The method can provide new ideas and methods for the rapid decomposition of high-phosphorus iron ore, which is of great significance for improving the resource utilization rate of phosphorus iron ore. The method can also be applied to the steel industry and iron ore processing fields to promote the sustainable development of my country's iron ore industry. Background Art

[0002] my country has a large reserve of Ningxiang-style iron ore resources, and the research on the resource utilization of Ningxiang-style iron ore is of great significance. Ningxiang-style iron ore is mainly composed of oolitic hematite, followed by limonite, siderite and chlorite. The iron grade is generally 45%-60%, and the phosphorus grade is between 0.45%-1.15%. Hematite is one of the main raw materials for ironmaking. Better utilization of this part of resources will have great practical significance for the development of my country's steel industry.

[0003] High-phosphorus iron ore has a complex mineral composition and a high organic matter content. The complete digestion of the sample is the basis for accurately determining its element content. In order to decompose the high-phosphorus iron ore smoothly, the ore sample needs to be crushed to pass through a 150-mesh sieve. For a long time, the decomposition of high-phosphorus iron ore samples has always adopted the "alkali fusion acid leaching" mode, which has cumbersome steps, time-consuming and energy-consuming, and it is urgent to explore a more accurate and efficient detection method. Invention patents CN110963746A and CN115367722A disclose the use of a single inorganic acid and phosphorus iron ore for full acid leaching to achieve ore decomposition, and the leached acid solution is prepared through a series of steps such as concentration, impurity removal, extraction, solid-liquid separation, crystallization, spray drying and calcination to prepare high-quality battery-grade iron phosphate materials. However, in the process of phosphorus iron ore decomposition, single acid dissolution will have problems such as long time consumption, no energy saving and slow analysis speed. Considering the above-mentioned energy consumption and efficiency problems, single acid dissolution cannot meet the needs of rapid detection and analysis of daily high-phosphorus iron ore batch samples. In addition, rapid and complete decomposition of the sample is a prerequisite for ensuring the accuracy of the composition analysis of high-phosphorus iron ore, which is directly related to the accurate evaluation of the utilization rate of valuable elements in the ore, especially the use of element content characteristics to provide strong support for the mining and utilization of high-phosphorus iron ore.

[0004] Based on the above research, it is necessary to provide a method for rapid digestion of high-phosphorus iron ore to ensure the accuracy of multi-element analysis, thereby accelerating the development and utilization of high-phosphorus iron ore in my country. Summary of the invention

[0005] In view of the above, the purpose of the present invention is to provide a method for quickly and completely digesting high-phosphorus iron ore, using mixed acid wet digestion, optimizing the mixed acid ratio, and quantifying the heating process. Oxalic acid is a low-molecular organic acid that has the ability to destroy silicate minerals and clay minerals in the sample, and perfectly achieves the complete decomposition of the ore. The method has a simple operation process, improves the detection efficiency, can better meet the requirements of rapid analysis of high-phosphorus iron ore, and is suitable for application in large-scale industrial production. To this end, the present invention provides a rapid method for wet digestion of high-phosphorus iron ore, the method comprising the following steps: S1: Weigh the sieved high-phosphorus iron ore sample and add ultrapure water to moisten it; S2: Add a mixed acid system to S1 for digestion, add oxalic acid after digestion, cover with a watch glass, perform heat treatment until the sample is completely dissolved, remove and cool to room temperature; S3: The above solution is completely transferred to a volumetric flask, diluted to the mark and shaken well; the fixed volume solution is filtered through a microporous filter membrane to separate insoluble residues, and the filtrate is retained as the main solution; S4: Use a pipette to transfer the above main solution, and use potassium dichromate titration method and quinoline molybdate weight method to analyze the iron and phosphorus content in the mineral, and use ICP standard curve method to analyze the content of other elements in the ore.

[0006] In some embodiments, the mixing of raw materials or the digestion process of the present invention is carried out in a glass container, such as a triangular pancake, a digestion glass tube, etc.

[0007] The sample described in step S1 belongs to the Ningxiang type high-phosphorus iron ore in western Hubei. The iron in the ore mainly exists in the form of hematite, with a small amount of limonite, siderite and trace magnetite. The phosphate mineral is mainly fluorapatite, and the oolitic core is oolite and is closely connected to hematite and fluorapatite to form a concentric layered structure. The iron grade is 45%-60%, and the phosphorus content is 0.45%-1.15%.

[0008] The sample mentioned in step S1 needs to be crushed to pass through a 150-250 mesh sieve. The purpose of crushing and screening is to reduce impurities as much as possible and increase the specific surface area of ​​the ore after grinding as finely as possible. The water is ultrapure water, and the ultrapure water should meet the specifications of the standard GB / T 6682 secondary water.

[0009] The mixed acid system described in step S2 is perchloric acid and sulfuric acid, the mass percentage concentration of sulfuric acid is 95.0%-98.0%, and the mass percentage concentration of perchloric acid is 70.0%-72.0%; the volume ratio of sulfuric acid to perchloric acid is 1-3:10-20.

[0010] The mass fraction of oxalic acid mentioned in step S2 is 99% or more, and the amount of oxalic acid added is 1-2 times the amount of the sample, so as to destroy the silicate minerals and clay minerals in the sample and achieve complete digestion of the sample.

[0011] The heat treatment in step S2 adopts a two-stage heating method; first, low-temperature digestion is performed, and the temperature of the electric furnace is set to 120°C-200°C. At this time, perchloric acid is used as the digestion main body, and the temperature is increased after the reaction is stable. After further reaction after oscillation, the temperature is increased to 290-400°C for digestion treatment, and digestion is completed after the liquid is clarified.

[0012] The specification of the volumetric flask in step S3 is 10mL-50mL.

[0013] The diameter of the microporous filtration membrane in step S3 is 0.2 μm-0.45 μm.

[0014] The specification of the pipette in step S4 is 1 mL-50 mL.

[0015] The specific operating steps of the potassium dichromate titration method and the quinoline molybdate weight method described in step S2 can refer to the test method for iron and phosphorus content described in the standard HG / T4701-2021 "Iron Phosphate for Batteries".

[0016] The invention provides a rapid method for wet digestion of high-phosphorus iron ore, which has the following beneficial effects: the invention completely decomposes the high-phosphorus iron ore sample by adding a mixed acid system and an appropriate amount of oxalic acid and adopts a two-stage temperature rise treatment method, thereby avoiding the volatilization loss of the components to be tested, and the treated solution does not retain fine crumbs or powder of the original sample, and the main content and trace components in the mineral are analyzed by potassium dichromate titration method, quinoline molybdate weight method and ICP standard curve method. DETAILED DESCRIPTION

[0017] The embodiments of the present invention are described in detail below, and the digestion method provided by the present invention is clearly and completely described, but the protection scope of the present invention is not limited to the following specific embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. The contents of the following embodiments are configured according to the proportional relationship of the content of the invention.

[0018] Example 1 A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0019] Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) and 15 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 2:15) to the conical beaker in sequence, and cover with a watch glass. Place the conical beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the conical beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white thick smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and cool to room temperature.

[0020] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0021] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0022] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0023] Example 2 The method and conditions were the same as in Example 1, except that the digestion temperature was changed.

[0024] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0025] Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) and 15 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 2:15) to the beaker in sequence, and cover with a watch glass. Place the beaker on an electric furnace at 180°C for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 350°C and heat it until white thick smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and let it cool to room temperature.

[0026] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0027] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0028] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0029] Example 3 The method and conditions were the same as in Example 1, except that the amount of oxalic acid was changed to 0.4 g.

[0030] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0031] Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) and 15 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 2:15) to the conical beaker in sequence, and cover with a watch glass. Place the conical beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the conical beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.4 g of oxalic acid (i.e., the amount of oxalic acid is twice that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and cool to room temperature.

[0032] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0033] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0034] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0035] Example 4 The method and conditions were the same as those in Example 1, except that the amount of perchloric acid added was changed to 3 mL.

[0036] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0037] Step S2: Add 3 mL of perchloric acid (mass percentage concentration of 70%) and 15 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 2:15) to the beaker in sequence, and cover with a watch glass. Place the beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and cool to room temperature.

[0038] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0039] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0040] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0041] Example 5 The method and conditions were the same as in Example 1, except that the amount of sulfuric acid was 20 mL and the sample weight was 0.4 g.

[0042] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.4 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0043] Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) and 20 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 2:15) to the conical beaker in sequence, and cover with a watch glass. Place the conical beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the conical beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white thick smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and cool to room temperature.

[0044] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0045] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0046] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0047] Comparative Example 1 The method and conditions were the same as in Example 1, except that the digestion solution was sulfuric acid, and the sample digestion was incomplete.

[0048] Step S1: weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water; Step S2: Add 15 mL of sulfuric acid (98% by mass concentration) to the beaker and cover with a watch glass. Place the beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), and continue to digest. If the sample is not completely digested, remove the beaker and let it cool to room temperature.

[0049] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0050] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0051] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0052] Comparative Example 2 The method and conditions were the same as in Example 1, except that the digestion solution was perchloric acid, and the sample digestion was incomplete.

[0053] Step S1: weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water; Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) to the beaker and cover with a watch glass. Place the beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), continue to digest, and if the sample is not completely digested, remove the beaker and let it cool to room temperature.

[0054] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0055] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0056] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0057] Comparative Example 3 The method and conditions were the same as in Example 1, except that oxalic acid was not added, and the sample digested slowly and was accompanied by a small amount of insoluble impurities.

[0058] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water; Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) to the beaker and cover with a watch glass. Place the beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke appears in the bottle and a large amount of foam appears on the liquid surface, start shaking the beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white smoke appears. Continue to digest until a little white smoke remains at the bottom of the bottle. Continue to digest. The sample digests slowly and is accompanied by a small amount of insoluble impurities. Remove the beaker and let it cool to room temperature.

[0059] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0060] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0061] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0062] Comparative Example 4 The method and conditions were the same as those in Example 1, except that the volume ratio of perchloric acid to sulfuric acid was changed to 1:25.

[0063] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0064] Step S2: 1 mL of perchloric acid (mass percentage concentration of 70%) and 25 mL of sulfuric acid (mass percentage concentration of 98%) are added to the beaker in sequence (i.e., the volume ratio of perchloric acid to sulfuric acid is 1:25), and a watch glass is placed on the beaker. The beaker is placed on a 200°C electric furnace for low-temperature digestion. When brown smoke is emitted from the bottle and a large amount of foam appears on the liquid surface, the beaker is shaken. When uniform and large foam appears on the liquid surface in the bottle, the beaker is stopped from being shaken, and the temperature is raised to 400°C until white thick smoke is emitted. The digestion is continued until a small amount of white smoke remains at the bottom of the bottle, and 0.3 g of oxalic acid (i.e., the amount of oxalic acid used is 1.5 times that of the ore) is added. The digestion is continued until the solution in the bottle becomes clear, and the beaker is removed and cooled to room temperature.

[0065] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0066] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0067] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0068] Comparative Example 5 The method and conditions were the same as those in Example 1, except that the volume ratio of perchloric acid to sulfuric acid was changed to 4:10.

[0069] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0070] Step S2: Add 4 mL of perchloric acid (mass percentage concentration of 70%) and 10 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 4:10) to the conical beaker in sequence, and cover with a watch glass. Place the conical beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the conical beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white thick smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of oxalic acid (i.e., the amount of oxalic acid is 1.5 times that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and cool to room temperature.

[0071] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0072] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0073] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0074] Comparative Example 6 The method and conditions were the same as in Example 1, except that oxalic acid was replaced by acetic acid.

[0075] A rapid method for wet digestion of high-phosphorus iron ore, specifically comprising the following steps: Step S1: Weigh 0.2 g of high-phosphorus iron ore that has passed through a 150-mesh sieve into a conical beaker and moisten it with 10 mL of ultrapure water.

[0076] Step S2: Add 2 mL of perchloric acid (mass percentage concentration of 70%) and 15 mL of sulfuric acid (mass percentage concentration of 98%) (i.e., the volume ratio of perchloric acid to sulfuric acid is 2:15) to the beaker in sequence, and cover with a watch glass. Place the beaker on a 200°C electric furnace for low-temperature digestion. When brown smoke comes out of the bottle and a large amount of foam appears on the liquid surface, start shaking the beaker. When uniform and large foam appears on the liquid surface in the bottle, stop shaking the beaker, place it at 400°C and heat it until white smoke comes out. Continue to digest until a little white smoke remains at the bottom of the bottle, add 0.3 g of acetic acid (i.e., the amount of acetic acid is 1.5 times that of the ore), continue to digest until the solution in the bottle becomes clear, remove the beaker and let it cool to room temperature.

[0077] S3: The cooled solution was completely transferred to a 100 mL volumetric flask, diluted to the mark and shaken well; the fixed solution was filtered through a microporous filter membrane with a pore size of 0.25 um, and the filtrate was retained as the main solution.

[0078] S4: Use a 25 mL pipette to transfer the above main solution, and use potassium dichromate titration and quinoline molybdate gravimetric method to analyze the iron and phosphorus content in the mineral.

[0079] S5: Use a 1 mL pipette to transfer the above main solution, dilute it to 250 mL with ultrapure water, and then use the ICP standard curve method to analyze the content of other elements in the ore.

[0080] Table 1 Elemental analysis results of wet digestion of high phosphorus iron ore samples of Examples 1-5 and Comparative Examples 1-6

[0081] As shown in Table 1, from the results of Examples 1-5, the results of the determination of iron and phosphorus by titration and gravimetric method are similar to the results of the ICP standard curve method analysis, and the two methods have good reproducibility and accurate results. From the results of the comparative example, the determination results are low due to incomplete digestion. In summary, the method of the present invention can provide an accurate and fast method for daily batch analysis of high-phosphorus iron ore.

[0082] As described above, the above embodiments are only for illustrating the technical concept and features of the present invention, and those skilled in the art can understand that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and purpose of the present invention. The scope of the present invention is defined by the claims and their equivalents.

Claims

1. A rapid method for wet digestion of high-phosphorus iron ore, characterized in that The wet digestion comprises the following steps: S1: Weigh the sieved high-phosphorus iron ore sample and add ultrapure water to moisten it; S2: Add a mixed acid system to S1 for digestion, add oxalic acid after digestion, cover with a watch glass, perform heat treatment until the sample is completely dissolved, remove and cool to room temperature; S3: The above solution is completely transferred to a volumetric flask, diluted to the mark and shaken well; the fixed volume solution is filtered through a microporous filter membrane to separate insoluble residues, and the filtrate is retained as the main solution; S4: Use a pipette to transfer the above main solution, and use potassium dichromate titration method and quinoline molybdate weight method to analyze the iron and phosphorus content in the mineral, and use ICP standard curve method to analyze the content of other elements in the ore.

2. A rapid method for wet digestion of high-phosphorus iron ore according to claim 1, characterized in that: The sample described in step S1 belongs to the Ningxiang-type high-phosphorus iron ore in western Hubei, with an iron grade of 45%-60% and a phosphorus content of 0.45%-1.15%.

3. A rapid method for wet digestion of high-phosphorus iron ore according to claim 1, characterized in that: The sample mentioned in step S1 needs to be crushed to pass through a 150-250 mesh sieve.

4. A rapid method for wet digestion of high-phosphorus iron ore according to claim 1, characterized in that: The mixed acid system described in step S2 is perchloric acid and sulfuric acid, the mass percentage concentration of sulfuric acid is 95.0%-98.0%, and the mass percentage concentration of perchloric acid is 70.0%-72.0%; the volume ratio of sulfuric acid to perchloric acid is 1-3:10-20.

5. A rapid method for wet digestion of high-phosphorus iron ore according to claim 1, characterized in that: The mass fraction of oxalic acid mentioned in step S2 is 99% or more, and the amount of oxalic acid added is 1-2 times the sample weight.

6. A rapid method for wet digestion of high-phosphorus iron ore according to claim 1, characterized in that: The heat treatment in step S2 adopts a two-stage heating method; first, low-temperature digestion is performed, and the temperature of the electric furnace is set to 120°C-200°C. When the decomposition temperature of perchloric acid is reached, the temperature is increased to 290°C-400°C for digestion after further reaction is stable after oscillation, and digestion is completed after the liquid is clarified.

Citation Information

Patent Citations

  • Method for determining content of phosphor in ferrotungsten

    CN102830154A

  • Method for detecting silicon content in silicon-calcium alloy or silicon-iron alloy

    CN114813594A

  • Method for detecting boron content in alloy

    CN114858728A

  • Foreign matter inclusion evaluation method

    JP2023104853A