Multi-dimensional imaging method for defect state distribution of perovskite photovoltaic device
Through the cross-fusion of scanning photocurrent, thermal conductivity spectrum and driving-level capacitance analysis technology, a three-dimensional image of defective state distribution of perovskite photovoltaic devices is drawn, solving the problem of insufficient single-dimensional information, and deeply revealing the microstructure of the device and Functions promote the improvement of device efficiency.
Patent Information
- Application Number
- CN202410904781.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing defect characterization technology of perovskite photovoltaic devices can only present single-dimensional information and cannot realize the distributed image drawing of defect states in three-dimensional space and energy space, resulting in an imperfect understanding of the device performance mechanism.
The cross-fusion of scanning photocurrent measurement, thermal conductivity spectrum measurement and driving-level capacitance analysis technology is used to draw the defect state distribution of perovskite photovoltaic devices by fitting the formulas of photocurrent, defect state density and carrier density. Images, combined with optical characterization technology to obtain the microstructure and characteristics of the device.
A thorough analysis of the detailed distribution of defect states of perovskite photovoltaic devices in three-dimensional space and energy space is achieved, providing more comprehensive device performance information, providing technical support for designing defect passivation strategies, and promoting device efficiency to approach theoretical limits .
Smart Images

Figure CN118914286A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of imaging defect state distribution of perovskite photovoltaic devices, and in particular to a multi-dimensional imaging method for defect state distribution of perovskite photovoltaic devices. Background Art
[0002] Perovskite is a cutting-edge material with a wide range of potential applications, showing diverse crystal structures, excellent optoelectronic and magnetoelectric properties. Due to its unique advantages such as high carrier mobility, long carrier diffusion length and solution-based preparation, perovskite has been widely used in sensors, biomedical applications, light-emitting diodes and solar cells. To promote the commercial application of perovskite solar cells, a thorough analysis of the microstructure and properties of perovskite films and devices is very helpful for understanding and exploring mechanistic issues.
[0003] Until now, defects are still the core problem that prevents the efficiency of perovskite photovoltaic devices from approaching the theoretical limit, and are also a hot research object for researchers. There are many different methods for detecting defect state information, and the characterization area involves two aspects: energy and space. Thermal admittance spectroscopy is a mature technology that can be used to explore energy-related defect state distribution information, while driver-level capacitance analysis can reveal the distribution of trap states in the vertical direction of the device space. If you want to achieve the cross-integration of defect state characterization technologies and draw a panoramic distribution map of defects related to energy or space, you need to put the characterization information on the same level, that is, the same observation object and characterization dimension. There are many types of defect state characterization on the surface of thin films. However, at present, the analysis of defect-related information of perovskite photovoltaic devices requires the preparation of multiple groups of thin film samples or devices for multiple characterization tests in order to comprehensively infer the quality of the final photovoltaic device. The characterization of defect state distribution in the horizontal direction of the device surface is still underdeveloped and urgently needs to be developed to help draw and analyze a three-dimensional panoramic map of defect states in the spatial dimension. In order to realize the horizontal analysis of defects, it is necessary to realize the synchronous feedback of electrical signals and imaging. Scanning photocurrent detection technology can realize the detection and imaging of photocurrent information in device samples, providing rich semiconductor information, including internal electric field, charge transport and recombination dynamics. This provides the prerequisite for mapping the distribution of defect states in photovoltaic devices in three-dimensional space and energy space, which is conducive to obtaining comprehensive and in-depth information related to device performance. However, no researcher has yet achieved the image mapping of this distribution.
[0004] The defect characterization technologies that have been developed so far are mainly focused on single-dimensional information presentation, including scanning photocurrent detection technology (J. Chen, GP Zhu, X. Li, Y H Lou, C. Dong, K L Wang, S. Yuan, CH Chen, Y R Shi, T. Wang, Small 2022, 18, 2201930), driver-level capacitance analysis technology (Z. Ni, C. Bao, Y. Liu, Q. Jiang, W.-Q. Wu, S. Chen, X. Dai, B. Chen, B. Hartweg, Z. Yu, Science 2020, 367, 1352-1358) and thermal admittance spectroscopy technology, which respectively present information related to defect states and horizontal drift distances, defect states and detection depths, and defect states and defect energy ranges. At present, no researchers have achieved an in-depth analysis of various characterization technologies to obtain the common points of these characterization technologies, thereby realizing the cross-integration of various characterization technologies and mapping the distribution of defect states in perovskite photovoltaic devices in multiple dimensions. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a multi-dimensional imaging method for the defect state distribution of perovskite photovoltaic devices, so as to solve the problem that the existing defect characterization technology can only present single-dimensional information, the defect-related information obtained is more one-sided, and the mechanism of device performance is not thoroughly presented.
[0006] In order to solve the above technical problems, the present invention provides a multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device, comprising the following steps:
[0007] S1. Scanning photocurrent measurement: The laser spot is focused on the sample, and the photocurrent is scanned, detected and fitted. The fitting model is an exponential decay model, and the formula is:
[0008]
[0009] Among them, y is the photocurrent obtained by fitting, A1 is the maximum photocurrent value measured by the device, x is the distance between the laser spot and the electrode, and L is the diffusion length of photogenerated carriers obtained by fitting;
[0010] S2, thermal admittance spectrum measurement and driver level capacitance analysis measurement: provide DC and AC outputs through the electrical impedance analyzer to measure the corresponding capacitance of the device;
[0011] When measuring thermal admittance spectroscopy, the distribution formula of defect state density is:
[0012]
[0013] Among them, N T (Ew) is the defect state density corresponding to a fixed energy depth, Vbi is the built-in potential of the device, W is the depletion width, obtained from CV measurements with Mott-Schottky analysis, k, q, T, w, and C are the Boltzmann constant, elementary charge, temperature, angular frequency, and specific capacitance, respectively;
[0014] The formula for the partition energy is:
[0015]
[0016] Where Ew is the boundary energy, w0 is the angular frequency of trying to escape, w0=2πv0T 2 , ν0 is the temperature-independent escape attempt frequency, measured from the temperature-dependent capacitance frequency;
[0017] When measuring the driver-level capacitance, the calculation formula for carrier density is:
[0018]
[0019] Where N is the carrier density, ε = 6.5 is the dielectric constant of perovskite, q is the basic charge, and A = 0.16 cm 2 is the active area of the photovoltaic device. The derivation of the carrier density including the deep trap state is based on the nonlinear relationship between the change in charge (δQ) and the perturbation AC bias (δV): δQ / δV=C0+C1δV+C2(δV)2+…, while DLCP (Driver Level Capacitance Analysis) uses variable δV to measure the junction capacitance and uses the information embedded in the high-order terms to obtain the capacitance contribution from the trap state, and the first-order derivative C0 and the second-order derivative C1 are obtained by differentiation;
[0020] The total carrier density minus the free carrier density gives the defect state density N at low AC frequencies. T ;
[0021] S3. Cross-combine the photocurrent measured by scanning photocurrent with the defect state density measured by thermal admittance spectrum measurement and driver-level capacitance analysis to obtain a three-dimensional image of the defect state distribution of the device.
[0022] The present invention is based on thermal admittance spectroscopy, driving-level current analysis and scanning photocurrent detection technology, combined with optical characterization technology, to collect and compare signals of various characterization technologies for perovskite photovoltaic devices with different structures, and clarify the significance and commonalities of the signals; the scanning photocurrent detection is cross-integrated with thermal admittance spectroscopy and driving-level current analysis to obtain the distribution of defect states in the complete perovskite photovoltaic device in three-dimensional space and energy space, and the internal microstructure and characteristics of the device are further analyzed through two integrated images, deeply revealing the microscopic information of the device.
[0023] Furthermore, in the three-dimensional image of defect state distribution, the X-axis is the photocurrent value obtained by scanning photocurrent detection, the Y-axis is the defect state density obtained by thermal admittance spectrum or driving level capacitance analysis, and the Z-axis is the detection range.
[0024] Furthermore, the scanning photocurrent measurement is specifically as follows: the laser beam emitted by the laser is focused on the sample through the objective lens, the electrically controlled XY scanning mirror drives the sample to move so that the focused beam scans the sample surface, thereby realizing spatial mapping of the photocurrent distribution, the sample photocurrent is de-noised and amplified through a spatial filter, and the photocurrent is converted into a voltage signal.
[0025] Furthermore, in S1, the bias voltage is set to 0V.
[0026] Furthermore, the laser is a continuous wave laser, which provides a continuous and stable light beam for scanning photocurrent measurement.
[0027] Furthermore, the objective lens focuses the laser beam into a diffraction-limited light spot to ensure high spatial resolution during the measurement process, and the objective lens is a high numerical aperture objective lens of a microscope.
[0028] Furthermore, the scanning range of the laser beam on the sample is 1600×500 μm 2 , step size ≥ 2μm.
[0029] Furthermore, when measuring the thermal admittance spectrum, the DC bias is from 0V to the open circuit voltage of the photovoltaic device, and the AC frequency scanning range is 1kHz-10MHz.
[0030] Furthermore, when the thermal admittance spectrum is measured, the DC bias is fixed at 0V and the amplitude of the AC bias is 20mV.
[0031] Furthermore, when the driver-level capacitance is analyzed and measured, the total carrier density will tend to saturate as the AC frequency further increases. The free carrier density N0 is obtained by measuring the carrier density at a high AC frequency, and the total carrier density is obtained by measuring the carrier density at a low AC frequency. The total carrier density minus the free carrier density N0 is used to obtain the defect state density N at a low AC frequency. T .
[0032] Furthermore, the variable δV is 20-300 mV.
[0033] Furthermore, in S3, the lateral migration distance and vertical detection depth of the detection range of the scanning photocurrent measurement, the thermal admittance spectrum measurement and the driving level capacitance analysis measurement are uniformly processed.
[0034] Furthermore, in S3, when the photocurrent measured by the scanning photocurrent is cross-combined with the defect state density measured by the driving-level capacitance analysis, a three-dimensional distribution image of the device defect space is obtained. The longitudinal defect distribution of the device is reflected at the edge of the three-dimensional distribution image, and the transverse defect distribution is hidden inside the three-dimensional distribution image.
[0035] Furthermore, in S3, when the photocurrent measured by the scanning photocurrent is cross-combined with the defect state density measured by the thermal admittance spectrum, a three-dimensional distribution image of the device defect energy space is obtained. The defect distribution in the device energy space is reflected on the surface of the three-dimensional distribution image, and the lateral defect distribution is hidden inside the three-dimensional distribution image.
[0036] Beneficial effects of the present invention:
[0037] The present invention realizes the defect characterization technology fusion of thermal admittance spectroscopy, drive-level capacitance analysis and scanning photocurrent detection technology by fitting the carrier migration distance and defect state density values, establishes energy space simulation and spatial three-dimensional simulation of defect distribution in the device, so as to understand the precise energy and spatial characteristics of defect distribution.
[0038] The present invention is based on the obtained three-dimensional spatial defect distribution of photovoltaic devices and combines the defect distribution in energy space to reveal the microstructure and function of perovskite in the device, providing strong technical support for designing more targeted defect passivation strategies and promoting the efficiency of perovskite photovoltaic devices to further approach the theoretical limit. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is a schematic diagram of a scanning photocurrent detection device of the present invention;
[0040] Figure 2 It is a schematic diagram of the distance between the electrode and the laser point in the scanning photocurrent detection of the present invention;
[0041] Figure 3 It is a schematic diagram of the thermal admittance spectrum and driving level capacitance analysis test device of the present invention;
[0042] Figure 4 In the figure, a, b, and c are respectively signal curves obtained by the analysis of the driving-level capacitance, the scanning photocurrent measurement, and the thermal admittance spectrum measurement in Example 1, and d and e are schematic diagrams of the defect state distribution in the three-dimensional space and the energy space, respectively;
[0043] Figure 5 In the figure, a is a three-dimensional distribution image of device defect space drawn by fusion of driver level capacitance analysis and scanning photocurrent detection signal in Example 1, and b is a three-dimensional distribution image of device defect energy space drawn by fusion of thermal admittance spectrum and scanning photocurrent detection signal in Example 1;
[0044] Figure 6 is a three-dimensional image of defect distribution in Example 2;
[0045] Figure 7 is the three-dimensional image of defect distribution in Example 3;
[0046] Figure 8 is a three-dimensional image of defect distribution in Example 4;
[0047] Explanation of the numbers in the figure: 1. laser, 2. objective lens, 3. electrically controlled XY scanning mirror, 4. spatial filter, 5. photovoltaic device. DETAILED DESCRIPTION
[0048] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0049] Example 1
[0050] This embodiment relates to a multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device, comprising the following steps:
[0051] S1. Build a device for scanning photocurrent detection technology, including a laser 1, an objective lens 2, an electrically controlled XY scanning mirror 3 and a spatial filter 4, such as Figure 1 As shown, the laser 1 is a continuous wave laser, which provides a continuous and stable light beam for scanning photocurrent measurement. The light is focused into a diffraction-limited spot on the perovskite photovoltaic device 5 through the high numerical aperture objective lens 2 of the microscope, ensuring high spatial resolution during the measurement process. The electrically controlled XY scanning mirror 3 drives the perovskite photovoltaic device to move so that the focused light beam can be scanned on the sample surface to achieve spatial mapping of the photocurrent distribution. The spatial filter helps to shape the light beam and filter any unwanted spatial patterns.
[0052] use Figure 1 The device completed the photocurrent measurement. For formamidinium lead iodine perovskite, the optimal excitation laser wavelength was confirmed to be 633nm and the power was 2mW. When the bias was 0V, the photocurrent of the sample was removed by a spatial filter and amplified, and the photocurrent was converted into a voltage signal. During the photocurrent mapping process, the laser spot was fixed and the sample-level scanning range was 1600×500μm 2 , the minimum step size is 2μm. The model of the fitting result is an exponential decay model, and the formula is Where y is the photocurrent obtained by fitting, A1 is the maximum photocurrent value measured by the device, and x is the distance between the laser spot (laser point) and the electrode (see Figure 2 ), L is the diffusion length of photogenerated carriers obtained by fitting.
[0053] S2. Build the equipment used for thermal admittance spectrum and driver-level capacitance analysis test, such as Figure 3,The electrical impedance analyzer provides DC and AC outputs and measures the corresponding capacitance of the device, and the capacitance-frequency measurement is performed on the probe station to obtain the demarcation energy.
[0054] Thermal admittance spectroscopy measurement: For capacitance voltage measurement, the DC bias is from 0 V to the open circuit voltage of the photovoltaic device. In the measurement, the DC bias is fixed to 0 V, the amplitude of the AC bias is 20 mV, and the AC frequency is scanned in the range of 1 k-10 MHz.
[0055] The distribution formula of defect state density is:
[0056]
[0057] Among them, N T (Ew) is the defect state density corresponding to a fixed energy depth, V bi is the built-in potential of the device, W is the depletion width, obtained from CV measurements with Mott-Schottky analysis, k, q, T, w, and C are the Boltzmann constant, elementary charge, temperature, angular frequency, and specific capacitance, respectively;
[0058] The formula for the partition energy is:
[0059]
[0060] Where Ew is the boundary energy, w0 is the angular frequency of trying to escape, w0=2πv0T 2 , ν0 is the temperature-independent escape attempt frequency, measured from the temperature-dependent capacitance frequency;
[0061] When measuring the driver-level capacitance, the calculation formula for carrier density is:
[0062]
[0063] Where N is the carrier density, ε = 6.5 is the dielectric constant of perovskite, q is the basic charge, and A = 0.16 cm 2 is the active area of the photovoltaic device. The derivation of the carrier density including the deep trap state is based on the nonlinear relationship between the change in charge (δQ) and the perturbation AC bias (δV): δQ / δV=C0+C1δV+C2(δV)2+…, while DLCP (Driver Level Capacitance Analysis) uses variable δV to measure the junction capacitance and uses the information embedded in the high-order terms to obtain the capacitance contribution from the trap state, and the first-order derivative C0 and the second-order derivative C1 are obtained by differentiation;
[0064] The total carrier density minus the free carrier density gives the defect state density N at low AC frequencies. T , and the contour distance from the junction barrier is represented by εA / C0.
[0065] In S1 and S2, the signal curves obtained by driver level capacitance analysis, scanning photocurrent measurement, and thermal admittance spectrum measurement are shown in Figure 2. Figure 4 As shown in a, b, and c, the schematic diagram of defect state distribution in three-dimensional space and energy space is as follows Figure 4 As shown in d and e, single-dimensional information is presented.
[0066] S3. Combine the spatial longitudinal direction with the spatial lateral direction to obtain a three-dimensional distribution diagram of the device defect state in space, realize defect distribution visualization, and cross-combine the results of the driver level capacitance analysis and the scanning photocurrent test to obtain the three-dimensional spatial distribution of the defect state in the photovoltaic device, such as Figure 5 a. Both the vertical detection depth and the lateral migration distance have been normalized to more clearly illustrate the defect distribution trend. Among them, the photogenerated carrier diffusion length is obtained by fitting the test data by scanning the physical formula listed in the photocurrent detection, which reflects the defects distributed on the surface of the device, but does not directly extract the specific defect density value. Therefore, the three-dimensional image more reflects the defect state distribution trend in the three-dimensional space, reflects the all-round spatial distribution of the defect state in the device, and visualizes it. The longitudinal defect distribution of the device is reflected at the edge of the three-dimensional image, while the lateral defect distribution is hidden inside the three-dimensional image.
[0067] By combining the spatial longitudinal direction with energy, a three-dimensional distribution diagram of the device defect state in the energy space is obtained to realize defect distribution visualization. By cross-combining the results of thermal admittance spectrum and scanning photocurrent test, the energy space distribution of defect states in photovoltaic devices is obtained, such as Figure 5 b. The scanning photocurrent test is further integrated with the thermal admittance spectrum data to simulate the energy correlation and device surface defect distribution, and the detection range is normalized. The distribution trend in the energy space is reflected on the surface of the contour map, and the lateral distribution is hidden inside the three-dimensional image.
[0068] Example 2
[0069] The butylamine iodide molecule was used to optimize the perovskite surface for post-treatment to achieve surface passivation. The reference device (device before optimization) and the optimized device were subjected to thermal admittance spectroscopy, drive-level capacitance analysis, and scanning photocurrent detection tests and data analysis. The data were integrated into a three-dimensional distribution diagram of the device defect state in space and a three-dimensional distribution diagram in energy space. Figure 6 .
[0070] Based on spatial three-dimensional image analysis, the photocurrent value and trend obtained by scanning photocurrent detection determine the x-axis position and range of the image, the defect state density and trend obtained by driver-level capacitance analysis determine the y-axis position and range of the image, and the detection range is used as the z-axis. The higher the y-axis value, the higher the maximum photocurrent obtained by the device, that is, the higher the corresponding initial film quality, and the lower the x-axis value, the lower the extreme value of the defect state density, and the defect state data distribution obtained by the driver-level capacitance analysis and the photocurrent distribution trend obtained by scanning photocurrent detection determine the surface area of the image. The smaller the area, the more concentrated the defect state distribution and the more uniform the device performance. After processing the upper interface of the device, it can be found that the defect state density of the device has decreased both vertically and horizontally, which means that the quality of the device has been improved in all aspects. However, the surface area did not show a significant difference, which means that the surface treatment failed to significantly optimize the defect state distribution of the device, that is, the optimization was not thorough.
[0071] For the defect distribution in energy space, similar to the three-dimensional space diagram, the defect state density and trend obtained by the thermal admittance spectrum test determine the y-axis position and range of the image. It can be confirmed that the surface treatment can produce a good defect passivation effect within a certain range. However, there are certain areas in the deep energy level range that fail to produce optimization effects, which is one of the reasons why the area difference of the three-dimensional space diagram is not large. In the discrete test curves, the device shows an all-round improvement before and after optimization, and the three-dimensional diagram further reveals the shortcomings of the optimization effect.
[0072] Example 3
[0073] The benzenesulfonic acid molecules were used to pre-treat the lower interface of the perovskite to achieve lower interface passivation, which showed similar results to Example 2, such as Figure 7 As shown in the figure, the quality of the optimized device in three-dimensional space has been comprehensively improved, while the surface area has not shown significant differences, and the bottom interface pretreatment has not significantly optimized the overall defect state distribution of the device. Observing the three-dimensional diagram of defect distribution in energy space, it can be found that the defect optimization effect corresponding to the deep energy level range is very obvious, while it is slightly inferior in the shallow energy level area. However, compared with the surface treatment, the bottom interface pretreatment can change the surface area of the image, because the perovskite film is grown and prepared on this basis, so it can have a profound impact on the overall film.
[0074] Example 4
[0075] The sulfaguanidine molecules were introduced into the perovskite precursor solution for defect passivation, which showed completely different effects and images from the interface treatment. Figure 8As shown, in three-dimensional space, it is significantly manifested that not only the defect states of the optimized device are passivated in all directions, but also because the defect passivation starts from the inside of the film, the surface area of the image is significantly reduced, proving the thoroughness and effectiveness of the molecular passivation optimization. In the energy space, it can be found that the defect states are well suppressed and optimized in the entire energy range, which proves that the passivation molecules not only have a good interaction with the perovskite, but also achieve a full range of passivation effects.
[0076] In summary, based on the three-dimensional spatial defect distribution of the photovoltaic device of the present invention and combined with the defect distribution in the energy space, the microstructure and function of the perovskite film in the device are revealed, providing strong technical support for designing more targeted defect passivation strategies, and further promoting the efficiency of perovskite photovoltaic devices to approach the theoretical limit.
[0077] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A multi-dimensional imaging method for defect state distribution of perovskite photovoltaic devices, characterized in that: The steps include: S1. Scanning photocurrent measurement: The laser spot is focused on the sample, and the photocurrent is scanned, detected and fitted. The fitting model is an exponential decay model, and the formula is: Among them, y is the photocurrent obtained by fitting, A1 is the maximum photocurrent value measured by the device, x is the distance between the laser spot and the electrode, and L is the diffusion length of photogenerated carriers obtained by fitting; S2, thermal admittance spectrum measurement and driver level capacitance analysis measurement: provide DC and AC outputs through the electrical impedance analyzer to measure the corresponding capacitance of the device; When measuring thermal admittance spectroscopy, the distribution formula of defect state density is: Among them, N T (Ew) is the defect state density corresponding to a fixed energy depth, V bi is the built-in potential of the device, W is the depletion width, obtained from CV measurements with Mott-Schottky analysis, k, q, T, w, and C are the Boltzmann constant, elementary charge, temperature, angular frequency, and specific capacitance, respectively; The boundary energy formula is: Where Ew is the boundary energy, w0 is the angular frequency of trying to escape, w0=2πv0T 2 , ν0 is the temperature-independent escape attempt frequency, measured from the temperature-dependent capacitance frequency; When measuring the driver-level capacitance, the calculation formula for carrier density is: Where N is the carrier density, ε = 6.5 is the dielectric constant of perovskite, q is the basic charge, and A = 0.16 cm 2 The junction capacitance is measured using a variable perturbation AC bias for the active area of the photovoltaic device, and the capacitance contribution from the trap states is obtained using the information embedded in the higher-order terms. The first-order derivative C0 and the second-order derivative C1 are derived. The total carrier density minus the free carrier density gives the defect state density N at low AC frequencies. T ; S3. Cross-combine the photocurrent measured by scanning photocurrent with the defect state density measured by thermal admittance spectrum measurement and driver-level capacitance analysis to obtain a three-dimensional image of the defect state distribution of the device.
2. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: The scanning photocurrent measurement is specifically as follows: the laser beam emitted by the laser is focused on the sample through the objective lens, the electrically controlled XY scanning mirror drives the sample to move so that the focused beam scans the sample surface to achieve spatial mapping of the photocurrent distribution, the sample photocurrent is de-noised and amplified through a spatial filter, and the photocurrent is converted into a voltage signal.
3. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 2, characterized in that: The objective lens focuses the laser beam into a diffraction-limited light spot.
4. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 2, characterized in that: The scanning range of the laser beam on the sample is 1600×500μm 2 , step size ≥ 2μm.
5. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: When measuring the thermal admittance spectrum, the DC bias is from 0V to the open circuit voltage of the photovoltaic device, and the AC frequency scanning range is 1khz-10mhz.
6. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: During the driver-stage capacitance analysis measurement, the free carrier density is obtained by measuring the carrier density at a high AC frequency, and the total carrier density is obtained by measuring the carrier density at a low AC frequency.
7. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: The variable perturbation AC bias voltage is 20-300mV.
8. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: In S3, the lateral migration distance and vertical detection depth of the detection range of the scanning photocurrent measurement, the thermal admittance spectrum measurement and the driving level capacitance analysis measurement are homogenized.
9. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: In S3, when the photocurrent measured by scanning photocurrent is cross-combined with the defect state density measured by driving-level capacitance analysis, a three-dimensional distribution image of the device defect space is obtained. The longitudinal defect distribution of the device is reflected at the edge of the three-dimensional distribution image, and the transverse defect distribution is hidden inside the three-dimensional distribution image.
10. The multi-dimensional imaging method for defect state distribution of a perovskite photovoltaic device according to claim 1, characterized in that: In S3, when the photocurrent measured by scanning photocurrent is cross-combined with the defect state density measured by thermal admittance spectrum, a three-dimensional distribution image of the device defect energy space is obtained. The defect distribution in the device energy space is reflected on the surface of the three-dimensional distribution image, and the lateral defect distribution is hidden inside the three-dimensional distribution image.
Citation Information
Patent Citations
Method for detecting mercury cadmium telluride photovoltaic detector deep energy level defect
CN101377533A
Detection device and detection method for detecting subsurface defect of optical element rapidly and three-dimensionally
CN106770128A
Perovskite cell film detection device and evaluation method thereof
CN116735558A
Locking device for walk-in seat of vehicle
KR102446335B1