Alumina humidity-sensitive sensor and preparation method thereof
By using silicon substrate and magnetron sputtering to deposit ZnO and ZnO:Al layers in alumina moisture-sensitive sensor and performing wet etching, the problem of difficulty in controlling the thickness of Au electrode is solved, and high sensitivity and fast recovery time are achieved Alumina moisture sensor.
Patent Information
- Application Number
- CN202411152566.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
The existing aluminum oxide moisture-sensitive sensors have narrow process windows when Au electrode thickness is controlled, resulting in incomplete signal detection and serious signal current loss. The increase in thickness will block the holes, reducing sensitivity and increasing recovery time.
Using a silicon substrate, a silicon oxide layer and a porous alumina layer, ZnO and ZnO:Al layers are deposited by magnetron sputtering, and wet etching is performed to form a second through hole to expand the manufacturing process window of the electrode plate to ensure the metal The electrode layer does not clog the holes, which improves the sensitivity and recovery time of the sensor.
The manufacturing process window of the electrode plate on the capacitor is effectively expanded, the sensitivity and recovery time of the moisture-sensitive sensor are improved, and signal integrity and the conductive effect of the electrode layer are ensured.
Smart Images

Figure CN118914306A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sensors, and in particular to an aluminum oxide humidity sensitive sensor and a preparation method thereof. Background Art
[0002] Porous alumina (Al2O3) changes its dielectric constant when absorbing and releasing water vapor, making it an excellent material for forming humidity sensors. In capacitive humidity sensors formed by porous alumina, porous Au electrodes are deposited on porous alumina. It is generally believed that a porous gold electrode with a thickness of 20nm ("Anodic alumina membrane capacitive sensors for detection of vapors", Stepan K. Podgolin, Talanta, 2020) can just form a continuous gold film and will not block the pores of porous alumina.
[0003] However, when the Au electrode thickness is controlled at 20nm, the process window is too narrow, which is not conducive to yield control; if the Au electrode thickness is reduced, the Au film cannot completely cover the surface of the porous alumina, the electrode plate of the capacitor is incomplete, which is not conducive to signal detection, and the square resistance of the film is too large, and the signal current loss is serious; if the thickness is increased, the Au electrode will block the upper opening of the porous alumina, on the one hand, hindering the entry of water vapor and reducing the sensitivity of the humidity sensor, on the other hand, it is not easy for water vapor to escape, which increases the recovery time. To this end, the present invention provides an aluminum oxide humidity sensor and a preparation method thereof. Summary of the invention
[0004] The present invention provides an aluminum oxide humidity sensor and a preparation method thereof, which effectively expands the manufacturing process window of the upper electrode plate of the capacitor and provides an aluminum oxide humidity sensor with high humidity sensitivity and better recovery time.
[0005] The first object of the present invention is to provide an aluminum oxide humidity sensor, comprising a silicon substrate, wherein a silicon oxide layer is disposed on the upper surface of the silicon substrate, and a porous aluminum oxide layer is disposed on the silicon oxide layer, wherein the porous aluminum oxide layer is provided with a first through hole;
[0006] A ZnO layer is magnetron sputtered on the porous alumina layer, and a ZnO:Al layer is magnetron sputtered on the ZnO layer; a second through hole is opened through the ZnO layer and the ZnO:Al layer; the second through hole is connected to the first through hole, and the aperture of the second through hole is larger than that of the first through hole;
[0007] A front metal electrode layer is arranged on the ZnO:Al layer, a back metal electrode layer is arranged on the lower surface of the silicon substrate, and metal pad electrodes are deposited on the back metal electrode layer and the front metal electrode layer respectively.
[0008] As a preferred implementation, the thickness of the ZnO layer is 10-50 nm, the thickness of the ZnO:Al layer is 10-100 nm, and the thickness of the front metal electrode layer is 10-80 nm.
[0009] The second object of the present invention is to provide a method for preparing the above-mentioned aluminum oxide humidity sensor, comprising the following steps:
[0010] Depositing metallic aluminum on the silicon oxide layer on the upper surface of the silicon substrate and performing anodization to obtain a porous aluminum oxide layer with a thickness of 3 to 8 μm, wherein a first through hole is formed through the porous aluminum oxide layer;
[0011] A ZnO layer with a thickness of 10 to 50 nm is magnetron sputtered on the porous alumina layer, and a ZnO:Al layer with a thickness of 10 to 100 nm is magnetron sputtered on the ZnO layer; a second through hole is opened through the ZnO layer and the ZnO:Al layer; the ZnO layer and the ZnO:Al layer are wet-etched so that the aperture of the second through hole is larger than that of the first through hole;
[0012] Depositing a front metal electrode layer with a thickness of 10 to 80 nm on the ZnO:Al layer;
[0013] Depositing a back metal electrode layer on the lower surface of the silicon substrate;
[0014] Metal pad electrodes are deposited on the back metal electrode layer and the front metal electrode layer respectively.
[0015] As a preferred implementation, the wet etching specifically includes: etching using an NH4Cl solution with a mass concentration of 6% to 8%, so that the lateral etching rate is greater than the longitudinal etching rate.
[0016] As a preferred embodiment, the preparation process of the ZnO layer comprises the following steps:
[0017] Depositing Zn atoms: using a metal Zn target on the porous alumina layer, magnetron sputtering was performed in an argon atmosphere with a flow rate of 300 sccm, the Zn target power was controlled to be 5 KW, the substrate bias voltage was -50 V, the time was 20 s, and a Zn layer was obtained;
[0018] Bombardment process: bombarding the Zn layer, controlling the argon gas flow rate to 500 sccm, the substrate bias voltage to -500 V, the time to 10 s, and removing the Zn layer attached to the first through hole;
[0019] Oxidation process: oxygen is introduced, the argon flow rate is controlled to be 400 sccm, the oxygen flow rate is controlled to be 600 sccm, and the power is 6 KW, so as to oxidize the Zn layer to form a ZnO layer.
[0020] As a preferred embodiment, the preparation process of the ZnO layer is cyclically operated 8 to 20 times.
[0021] As a preferred embodiment, the preparation process of the ZnO:Al layer comprises the following steps:
[0022] Depositing ZnAl atoms: using a metal ZnAl target on the ZnO layer, magnetron sputtering was performed in an argon atmosphere with a flow rate of 300 sccm, the ZnAl target power was controlled to be 4KW, the substrate bias voltage was -50V, the time was 20s, and the ZnAl layer was obtained;
[0023] Bombardment process: bombarding the ZnAl layer, controlling the argon gas flow rate to 500 sccm, the substrate bias voltage to -600 V, the time to 10 s, to remove the newly grown ZnAl layer attached to the upper opening pore wall of the porous alumina layer;
[0024] Oxidation process: oxygen is introduced, the argon flow rate is controlled to be 400 sccm, the oxygen flow rate is 700 sccm, and the power is 6.5 KW to oxidize the deposited ZnAl layer to form a ZnO:Al layer.
[0025] As a preferred embodiment, the preparation process of the ZnO:Al layer is cyclically operated 16 to 40 times.
[0026] As a preferred implementation, the diameter of the first through hole is ≤70 nm.
[0027] As a preferred implementation, the front metal electrode layer is an Au layer.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The present invention provides an aluminum oxide humidity sensor and a preparation method thereof. A back metal electrode layer is arranged on the lower surface of a silicon substrate, and a silicon oxide layer is arranged on the upper surface of the silicon substrate; the back metal electrode layer is provided with a first metal pad electrode; an aluminum oxide layer is arranged on the upper surface of the silicon oxide layer, and a first through hole is opened through the aluminum oxide layer; a ZnO layer is arranged on the upper surface of the aluminum oxide layer, and a ZnO:Al layer is arranged on the upper surface of the ZnO layer, and a second through hole is opened through the ZnO layer and the ZnO:Al layer; a front metal electrode layer is arranged on the upper surface of the ZnO:Al layer, and the front metal electrode layer is provided with a second metal pad electrode. After the ZnO layer and the ZnO:Al layer are deposited, the ZnO layer and the ZnO:Al layer are wet-etched to remove the intrinsic ZnO and ZnO:Al layers attached to the sidewalls of the opening on the porous alumina layer, and even a certain degree of lateral over-etching occurs inside the opening, that is, the size of the second through hole formed in the ZnO layer and the ZnO:Al layer is larger than the first through hole of the porous alumina, thereby ensuring that when the front metal electrode layer is subsequently deposited, even if the thickness of the deposited front metal electrode is relatively thick, the upper opening will not be blocked or blocked. The pore size of the porous alumina of the present invention is ≤70nm, and the lateral etching solution is not easy to enter the pores of the porous alumina, and the pore size of the porous alumina will not be damaged. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the structure of the aluminum oxide humidity sensor of the present invention.
[0031] Description of reference numerals:
[0032] 1. Silicon substrate, 2. Silicon oxide layer, 3. Porous aluminum oxide layer, 31. First through hole, 4. ZnO layer, 41. Second through hole, 5. ZnO:Al layer, 6. Front metal electrode layer, 7. Back metal electrode layer, 8. Metal pad electrode. DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.
[0034] The background technology of the present invention points out that the existing alumina humidity sensor is a capacitive humidity sensor formed by porous alumina, which is prepared by depositing a porous Au electrode on the porous alumina. However, when the thickness of the Au electrode is controlled at 20nm, the process window is too narrow, which is not conducive to yield control; if the thickness of the Au electrode is reduced, the Au film cannot completely cover the surface of the porous alumina, and the electrode plate of the capacitor is incomplete, which is not conducive to signal detection, and the square resistance of the film is too large, and the signal current loss is serious; if the thickness is increased, the Au electrode will block the upper opening of the porous alumina, on the one hand, hindering the entry of water vapor and reducing the sensitivity of the humidity sensor, and on the other hand, it is not easy for water vapor to escape, which increases the recovery time. Based on the above technical problems, the present invention provides an alumina humidity sensor, which effectively expands the manufacturing process window of the upper electrode plate of the capacitor, and at the same time provides an alumina humidity sensor with high humidity sensitivity and better recovery time.
[0035] The aluminum oxide humidity sensor provided by the present invention is described in detail below.
[0036] The present invention provides an aluminum oxide humidity sensor, comprising:
[0037] A silicon substrate 1, a back metal electrode layer 7 is provided on the lower surface of the silicon substrate 1, and a silicon oxide layer 2 is provided on the upper surface of the silicon substrate 1; the back metal electrode layer 7 is provided with a metal pad electrode 8;
[0038] A porous aluminum oxide layer 3 is disposed on the upper surface of the silicon oxide layer 2, and a first through hole 31 is formed through the porous aluminum oxide layer 3;
[0039] The ZnO layer 4 is disposed on the upper surface of the porous aluminum oxide layer 3; a high-resistance intrinsic ZnO layer 4 is disposed on the surface of the porous aluminum oxide layer 3 to passivate the surface of the porous aluminum oxide layer 3, which is conducive to the subsequent formation of a highly conductive electrode. The porous aluminum oxide layer is generally formed by double anodization of aluminum, and the surface is not a well-flat surface. The high-resistance ZnO layer 4 can passivate the surface defects of the aluminum oxide layer and improve its surface flatness, thereby promoting the stable and low-resistance transmission of charges in the upper electrode.
[0040] The ZnO:Al layer 5 is disposed on the upper surface of the ZnO layer 4; an aluminum-doped zinc oxide layer, i.e., a ZnO:Al layer 5, is disposed on the intrinsic ZnO layer 4. The aluminum-doped zinc oxide is a high conductivity material and is often used as a top electrode of electronic devices. Depositing an aluminum-doped zinc oxide layer of a certain thickness can reduce the thickness of metal top electrodes such as Au and Ag, thereby saving device costs. The aluminum-doped zinc oxide layer and the ZnO layer can also be deposited in the same chamber, with a simple deposition process and good interface characteristics between the layers.
[0041] A second through hole 41 is opened through the ZnO layer 4 and the ZnO:Al layer 5, and the specific operation method is: use an NH4Cl solution with a mass concentration of 6% to 8% to laterally etch the ZnO layer 4 and the ZnO:Al layer 5, and the horizontal etching rate is greater than the vertical etching rate, so as to remove the ZnO layer 4 and the ZnO:Al layer 5 attached to the hole wall of the first through hole 31 of the porous aluminum oxide layer 3, and obtain the second through hole 41. After the deposition of the intrinsic ZnO layer 4 and the ZnO:Al layer 5, a lateral etching process is performed to further remove the intrinsic ZnO layer 4 and the ZnO:Al layer 5 attached to the side wall of the opening of the first through hole 31 on the porous aluminum oxide layer 3, and even a certain degree of lateral over-etching occurs to the inside of the opening, that is, the size of the second through hole 41 formed in the intrinsic ZnO layer 4 and the ZnO:Al layer 5 is larger than the aperture of the first through hole 31 of the porous aluminum oxide layer, so that when the metal electrode layer is subsequently deposited, even if the thickness of the deposited metal electrode layer is relatively thick, it is not easy to block or block the upper opening. In the present invention, the aperture of the first through hole 31 of the porous aluminum oxide layer is less than or equal to 70nm, and the lateral etching solution is not easy to enter the first through hole 31 of the porous aluminum oxide layer 3, and will not damage the aperture of the first through hole 31 of the porous aluminum oxide layer 3.
[0042] A front metal electrode layer 6, which is disposed on the upper surface of the ZnO:Al layer 5; the front metal electrode layer 6 is an Au layer, which is provided with a metal pad electrode 8;
[0043] The thickness of the porous aluminum oxide layer 3 is 3-8 μm, the thickness of the ZnO layer 4 is 10-50 nm, the thickness of the ZnO:Al layer 5 is 10-100 nm, and the thickness of the front metal electrode layer 6 is 10-80 nm.
[0044] It should be noted that, when depositing the ZnO layer 4, the ZnO:Al layer 4, the front metal electrode layer 6 and the back metal electrode layer 7, the present invention adopts metal target sputtering deposition instead of ZnO and ZnO:Al ceramic targets, and the ZnO layer and the ZnO:Al layer are deposited by first sputtering metal atoms and then oxidizing them. In this way, the sputtered metal cations tend to be deposited on the upper surface of the alumina layer, and less deposited in the pore walls of the porous alumina. Even if there is deposition in the pore walls, the adhesion is significantly weaker. It is generally believed that the upper surface of the anodized alumina layer is more likely to adsorb metal ions, while the inner wall is weaker in adsorbing metal ions, that is, there is a significant difference in the adsorption of metal ions at different positions.
[0045] It is particularly noted that when depositing the ZnO layer 4 and the ZnO:Al layer 5, the method of first depositing the metal atomic layer and then oxidizing is adopted, which fully utilizes the difference in adsorption force between the upper surface of the porous aluminum oxide layer 3 and the hole wall of the first through hole 31 for the metal atoms. If the conventional reaction deposition of the ZnO layer and the ZnO:Al layer is directly adopted, that is, oxygen is introduced for reaction while sputtering and depositing Zn atoms or ZnAl atoms, the difference in adsorption force between the upper surface of the aluminum oxide layer and the hole wall of the first through hole cannot be fully utilized.
[0046] In order to achieve a better sputtering effect, when depositing the intrinsic ZnO layer 4 and the ZnO:Al layer 5, the sputtering process can select DC magnetron sputtering, and more preferably high-power pulsed magnetron sputtering (HIPIMS) of a metal target. The sputtered metal positive ions are more abundant and can be better deposited on the upper surface of the electronegative porous alumina, rather than in the first through hole 31 of the porous alumina layer 3.
[0047] In the present invention, when the intrinsic ZnO layer 4 and the ZnO:Al layer 5 are deposited, a deposition process, a bombardment process and an oxidation process are included. During the deposition process, the film-forming effect of the sputtered Zn or ZnAl atoms is significant, while the bombardment removal effect on the film layer is not significant, that is, it is a thin film growth process on a macro scale. During the bombardment process, the bombardment etching effect of the sputtered Zn or ZnAl atoms is significant, and this process mainly bombards and removes the weakly adhered Zn or ZnAl atoms attached to the upper opening hole wall of the first through hole of the aluminum oxide layer. Even in the conventional sputtering process, since most of the sputtered atoms reach the alumina layer vertically, the deposition on the upper surface is faster than the deposition on the hole wall of the first through hole. The film layer originally deposited on the hole wall is relatively thin, and the adhesion of the hole wall is relatively weak, so it is easy to be removed during the high power density deposition process. In this way, when the deposition of the intrinsic ZnO layer 4 and the ZnO:Al layer 5 is completed, the film layer deposited on the porous alumina layer 3 has little obstruction on the hole opening of the first through hole 31, and almost no obstruction. During the bombardment process, the bombardment effect can be increased and the deposition effect can be weakened by various means such as increasing the voltage, increasing the gas flow rate, and changing the deposition temperature.
[0048] When the metal electrode layer is finally deposited, since the ZnO:Al layer 5 with excellent conductive effect is already present, the thickness of the metal electrode layer can be thinner when depositing, that is, when 40nm is still used as the process center line, if the thickness is thinner, for example, as thin as 10nm, it still has a good conductive effect; in addition, the deposition of the intrinsic ZnO layer 4 obtains a passivated and flat upper surface, which also makes the upper electrode still have a good conductive effect when the thickness is thin. On the other hand, when the metal electrode layer is deposited, the thickness can be thicker, because the opening size of the second through hole 41 in the intrinsic ZnO layer 4 and the ZnO:Al layer 5 is larger than the aperture of the first through hole 31 of the aluminum oxide layer, and even if a certain degree of sidewall deposition occurs, it will not block the hole opening of the first through hole 31 of the porous aluminum oxide. That is to say, after the intrinsic ZnO layer 4 and the ZnO:Al layer 5 are first formed on the porous alumina layer 3, the process window of the metal electrode layer is expanded, and even if it is thinner or thicker, for example, even if the thickness is 10 to 80 nm, it has a good conductive effect and will not block the pore openings of the porous alumina.
[0049] In order to achieve efficient deposition of the ZnO layer 4, the preparation process of the ZnO layer 4 includes the following steps:
[0050] Deposition of Zn atoms: magnetron sputtering was performed using a metal Zn target, with the Zn target power controlled to be 5KW, the argon flow rate to be 300sccm, the oxygen flow rate to be 0, the substrate bias voltage to be -50V, and the time to be 20s to obtain a Zn layer;
[0051] Bombardment process: bombarding the Zn layer, controlling the argon gas flow rate to 500 sccm, the substrate bias voltage to -500 V, the time to 10 s, to remove the Zn layer attached to the first through hole 31;
[0052] Oxidation process: oxygen is introduced, the argon flow rate is controlled to be 400 sccm, the oxygen flow rate is controlled to be 600 sccm, and the power is 6 KW, so as to oxidize the Zn layer and form a ZnO layer 4.
[0053] In order to further achieve efficient deposition of the ZnO layer 4, the preparation process of the ZnO layer 4 is cycled 8 to 20 times.
[0054] In order to achieve efficient deposition of the ZnO:Al layer 5, the preparation process of the ZnO:Al layer 5 includes the following steps:
[0055] Deposition of ZnAl atoms: magnetron sputtering was performed using a metal ZnAl target, with the ZnAl target power controlled to be 4KW, the argon flow rate to be 300sccm, the oxygen flow rate to be 0, the substrate bias voltage to be -50V, and the time to be 20s to obtain a ZnAl layer;
[0056] Bombardment process: bombard the ZnAl layer, control the argon gas flow rate to 500 sccm, the substrate bias voltage to -600 V, the time to 10 s, and remove the newly grown ZnAl layer attached to the upper opening pore wall of the porous alumina layer 3;
[0057] Oxidation process: oxygen is introduced, the argon flow rate is controlled to be 400 sccm, the oxygen flow rate is controlled to be 700 sccm, and the power is 6.5 KW, to oxidize the deposited ZnAl layer to form a ZnO:Al layer 5.
[0058] In order to further achieve efficient deposition of the ZnO:Al layer 5, the preparation process of the ZnO:Al layer 5 is cycled 16 to 40 times.
[0059] In order to ensure the detection performance of the porous aluminum oxide 3, the pore size of the first through hole 31 is ≤70nm. On the one hand, the detection performance of the porous aluminum oxide layer 3 can be guaranteed; on the other hand, it is also important for the present invention that when the size is smaller than this, the etching liquid will not enter the first through hole 31 of the porous aluminum oxide layer 3 during the subsequent lateral etching, and will not damage the porous aluminum oxide. The larger the pores of the aluminum oxide, the easier it is for the etching liquid to fill the pores, which is undesirable.
[0060] It should be noted that the aperture of the second through hole 41 is larger than the first through hole 31. The opening size of the second through hole 41 in the intrinsic ZnO layer 4 and the ZnO:Al layer 5 is larger than the aperture of the first through hole 31 in the porous alumina layer 3, and even if a certain degree of sidewall deposition occurs, it will not block the hole opening of the first through hole 31 of the porous alumina layer 3. That is to say, after the intrinsic ZnO layer 4 and the ZnO:Al layer 5 are first formed on the porous alumina layer 3, the process window of the metal electrode layer is expanded, and even if it is thinner or thicker, for example, even if the thickness is 10 to 80 nm, it has a good conductive effect and will not block the hole opening of the porous alumina layer 3.
[0061] The effects are described below through specific embodiments and comparative examples.
[0062] Example 1
[0063] A method for preparing an aluminum oxide humidity sensor comprises the following steps:
[0064] (1) depositing a metal aluminum layer by magnetron sputtering on a silicon substrate 1 having a surface silicon oxide layer 2, with a thickness of 4 μm and a temperature of 300° C.;
[0065] (2) Anodizing the metal aluminum layer to form a porous aluminum oxide layer 3: A two-step anodizing process is used to form first through holes 31 with a pore size of about 70 nm in the metal aluminum layer to obtain a porous aluminum oxide layer 3.
[0066] (3) DC magnetron sputtering deposition of an intrinsic ZnO layer 4, using a metal Zn target to sputter and deposit an intrinsic ZnO layer 4 with a thickness of 10-50 nm;
[0067] (3.1) Low power density deposition process, depositing Zn atoms on the porous alumina layer 3: Zn target power 5 KW, argon flow rate 300 sccm, oxygen flow rate 0, substrate bias -50 V, time 20 s;
[0068] (3.2) Bombardment process: the bombardment effect on the newly grown Zn layer is strong, and the newly grown Zn layer attached to the wall of the first through hole on the upper part of the porous alumina layer 3 is removed by bombardment: argon gas flow rate 500 sccm, substrate bias voltage -500 V, time 10 s;
[0069] (3.3) Oxidation process: oxygen is introduced to oxidize the deposited Zn layer to form a ZnO layer 4: argon flow rate 400 sccm, oxygen flow rate 600 sccm, power 6 kW.
[0070] The above process of DC magnetron sputtering deposition of the intrinsic ZnO layer 4 was repeated 20 times.
[0071] (4) DC magnetron sputtering deposition of ZnO:Al layer 5, using a metal ZnAl target, sputtering deposition of ZnO:Al layer 5, with a thickness of 10-100 nm;
[0072] (4.1) Low power density deposition, deposition of ZnAl atoms: ZnAl target power 4KW, argon flow rate 300sccm, oxygen flow rate 0, substrate bias -50V, time 20s;
[0073] (4.2) During the bombardment process, the bombardment effect on the newly grown ZnAl layer is strong, and the newly grown ZnAl layer attached to the pore wall of the upper opening of the porous alumina layer is removed by bombardment: argon gas flow rate 500sccm, substrate bias voltage -600V, time 10s;
[0074] (4.3) Oxidation process: oxygen is introduced to oxidize the deposited Zn layer to form ZnO:Al layer 5: Ar flow rate 400 sccm, oxygen flow rate 700 sccm, power 6.5 KW.
[0075] The above process of DC magnetron sputtering deposition of ZnO:Al layer 5 was repeated 40 times.
[0076] (5) 7 wt % NH4Cl is used to etch the intrinsic ZnO layer 4 and the ZnO:Al layer 5 laterally, and the lateral etching rate is greater than the longitudinal etching rate, so as to remove the ZnO layer 4 and the ZnO:Al layer 5 attached to the hole wall of the first through hole 31 on the upper part of the porous aluminum oxide layer 3, and obtain the second through hole 41;
[0077] (6) sputtering deposits a gold (Au) front metal electrode layer 6, covering the entire surface of the ZnO:Al layer 5 and leaking out of the first through hole 31 of the porous aluminum oxide 3, with a deposition thickness of 10 nm;
[0078] (7) Aluminum (Al) back metal electrode layer 7 is deposited on the back side of silicon substrate 1; metal pad electrodes 8 are deposited on the back side of silicon substrate 1 and on the front side of front metal electrode layer 6, respectively.
[0079] Example 2
[0080] Compared with Example 1, the difference is that high-power pulsed magnetron sputtering is used to deposit the ZnO layer 4 and the ZnO:Al layer 5.
[0081] A method for preparing an aluminum oxide humidity sensor comprises the following steps:
[0082] (1) depositing a metal aluminum layer by magnetron sputtering on a silicon substrate 1 having a surface silicon oxide layer 2, with a thickness of 4 μm and a temperature of 300° C.;
[0083] (2) Anodizing the metal aluminum layer to form a porous aluminum oxide layer 3: A two-step anodizing process is used to form first through holes 31 with a pore size of about 60 nm in the metal aluminum layer to obtain a porous aluminum oxide layer 3.
[0084] (3) high-power pulsed magnetron sputtering deposition of an intrinsic ZnO layer 4, using a metal Zn target to sputter deposit an intrinsic ZnO layer with a thickness of 10-50 nm;
[0085] (3.1) Deposition process, depositing Zn atoms on the porous aluminum oxide layer 3: argon gas flow rate 80 sccm, discharge voltage 450 V, time 15 s;
[0086] (3.2) During the bombardment process, the bombardment effect on the newly grown Zn layer is strong, and the newly grown Zn layer attached to the wall of the first through hole on the upper part of the porous alumina layer is removed by bombardment: argon gas flow rate 150sccm, discharge voltage 700V, time 7s;
[0087] (3.3) Oxidation process: oxygen is introduced to oxidize the deposited Zn layer to form a ZnO layer: argon flow rate is 100 sccm, oxygen flow rate is 20 sccm, discharge voltage is 580 V, and time is 10 s.
[0088] The above process of high-power pulsed magnetron sputtering to deposit the intrinsic ZnO layer 4 was repeated 16 times.
[0089] (4) high power pulsed magnetron sputtering deposition of ZnO:Al layer 5, using a metal ZnAl target, sputtering deposition of ZnO:Al layer with a thickness of 10-100 nm;
[0090] (3.1) Deposition process, deposition of ZnAl atoms: argon flow rate 80 sccm, discharge voltage 450 V, time 13 s;
[0091] (3.2) During the bombardment process, the bombardment effect on the newly grown Zn layer is strong, and the newly grown Zn layer attached to the pore wall of the upper opening of the porous alumina layer 3 is removed by bombardment: argon gas flow rate 150sccm, discharge voltage 700V, time 6s;
[0092] (3.3) Oxidation process: oxygen is introduced to oxidize the deposited Zn layer to form a ZnO layer 4: argon flow rate 95 sccm, oxygen flow rate 20 sccm, discharge voltage 580 V, time 10 s.
[0093] The above process of high power pulsed magnetron sputtering deposition of ZnO:Al layer 5 was repeated 30 times.
[0094] (5) 7.7 wt % NH4Cl is used to etch the intrinsic ZnO layer 4 and the ZnO:Al layer 5 laterally, and the lateral etching rate is greater than the longitudinal etching rate, so as to remove the ZnO layer 4 and the ZnO:Al layer 5 attached to the hole wall of the first through hole 31 on the upper part of the porous aluminum oxide layer 3, and obtain the second through hole 41 at the same time;
[0095] (6) sputtering deposits a gold (Au) front metal electrode layer 6, covering the entire surface of the ZnO:Al layer 5 and leaking out of the first through hole 31 of the porous aluminum oxide layer 3, with a deposition thickness of 80 nm;
[0096] (7) Aluminum (Al) back metal electrode layer 7 is deposited on the back side of silicon substrate 1; metal pad electrodes 8 are deposited on the back side of silicon substrate 1 and on the front side of front metal electrode layer 6, respectively.
[0097] In order to further illustrate the technical effect of the present invention, the present invention is also provided with a comparative example, as follows:
[0098] Comparative Example 1
[0099] Compared with Example 1, the difference lies in that the ZnO layer, the ZnO:Al layer and the etching process are removed.
[0100] A method for preparing an aluminum oxide humidity sensor comprises the following steps:
[0101] (1) depositing a metal aluminum layer by magnetron sputtering on a silicon substrate 1 having a surface silicon oxide layer 2, with a thickness of 4 μm and a temperature of 300° C.;
[0102] (2) Anodizing the metal aluminum layer to form a porous aluminum oxide layer 3: A two-step anodizing process is used to form a first through hole with a pore size of about 70 nm in the metal aluminum layer to obtain a porous aluminum oxide layer 3.
[0103] (3) sputtering and depositing a gold (Au) front metal electrode layer 6, covering the entire surface of the porous aluminum oxide layer 3 and leaking out of the first through hole 31 of the porous aluminum oxide 3, with a deposition thickness of 10 nm;
[0104] (4) Aluminum (Al) back metal electrode layer 7 is deposited on the back side of silicon substrate 1; metal pad electrodes 8 are deposited on the back side of silicon substrate 1 and on the front side of front metal electrode layer 6, respectively.
[0105] Comparative Example 2
[0106] Compared with Example 2, the difference lies in that the ZnO layer, the ZnO:Al layer and the etching process are removed.
[0107] A method for preparing an aluminum oxide humidity sensor comprises the following steps:
[0108] (1) depositing a metal aluminum layer by magnetron sputtering on a silicon substrate 1 having a surface silicon oxide layer 2, with a thickness of 4 μm and a temperature of 300° C.;
[0109] (2) Anodizing the metal aluminum layer to form a porous aluminum oxide layer 3: A two-step anodizing process is used to form first through holes 31 with a pore size of about 60 nm in the metal aluminum layer to obtain a porous aluminum oxide layer 3.
[0110] (3) sputtering deposits a gold (Au) front metal electrode layer 6, covering the entire surface of the ZnO:Al layer 5 and leaking out of the first through hole 31 of the porous aluminum oxide 3, with a deposition thickness of 80 nm;
[0111] (4) Aluminum (Al) back metal electrode layer 7 is deposited on the back side of silicon substrate 1; metal pad electrodes 8 are deposited on the back side of silicon substrate 1 and on the front side of front metal electrode layer 6, respectively.
[0112] The performance of the aluminum oxide humidity sensors prepared in the above-mentioned Examples 1-2 and Comparative Examples 1-2 of the present invention were tested, and the results are as follows.
[0113] The sensitivity of the sensor is defined by the ratio of capacitance (pF) and ppmV (the ratio of the volume occupied by humid air to the total volume at standard temperature and pressure), that is, the capacitance value of the humidity sensor at unit humidity.
[0114] The sensitivity of Example 1 of the present invention is 0.35, and the recovery time is 243s; the sensitivity of Example 2 is 0.41, and the recovery time is 247s; the sensitivity of Comparative Example 1 is 0.31, and the recovery time is 240s, and the sensitivity of Comparative Example 2 is 0.27, and the recovery time is 340s.
[0115] It can be seen that the alumina humidity sensors prepared in Examples 1 and 2 of the present invention will not affect the sensitivity and recovery time of the sensor even if the thickness of the front metal electrode layer is thin or thick (relative to the conventional standard thickness of 20nm); while in Comparative Example 1, when the thickness of the front metal electrode layer is thin (10nm), the sensitivity decreases significantly; and in Comparative Example 2, when the thickness of the front metal electrode layer is thick (80nm), the sensitivity decreases significantly and the recovery time is long, indicating that when the thickness of the deposited front metal electrode layer is thick, the through holes of the porous alumina are seriously blocked, making it difficult for gas to enter and difficult to escape after entering.
[0116] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. An aluminum oxide humidity sensor, comprising a silicon substrate (1), a silicon oxide layer (2) being arranged on the upper surface of the silicon substrate (1), and a porous aluminum oxide layer (3) being arranged on the silicon oxide layer (2), characterized in that: The porous aluminum oxide layer (3) is provided with a first through hole (31); A ZnO layer (4) is magnetron sputtered on the porous aluminum oxide layer (3), and a ZnO:Al layer (5) is magnetron sputtered on the ZnO layer (4); a second through hole (41) is provided through the ZnO layer (4) and the ZnO:Al layer (5); the second through hole (41) is connected to the first through hole (31), and the aperture of the second through hole (41) is larger than that of the first through hole (31); A front metal electrode layer (6) is provided on the ZnO:Al layer (5), a back metal electrode layer (7) is provided on the lower surface of the silicon substrate (1), and metal pad electrodes (8) are deposited on the back metal electrode layer and the front metal electrode layer respectively.
2. The aluminum oxide humidity sensor according to claim 1, characterized in that: The thickness of the ZnO layer (4) is 10 to 50 nm, the thickness of the ZnO:Al layer (5) is 10 to 100 nm, and the thickness of the front metal electrode layer (6) is 10 to 80 nm.
3. A method for preparing an aluminum oxide humidity sensor according to any one of claims 1 or 2, characterized in that: The following steps are involved: Metal aluminum is deposited on a silicon oxide layer (2) on the upper surface of a silicon substrate (1) and anodized to obtain a porous aluminum oxide layer (3) with a thickness of 3 to 8 μm, wherein a first through hole (31) is formed through the porous aluminum oxide layer (3); A ZnO layer (4) with a thickness of 10 to 50 nm is magnetron sputtered on the porous aluminum oxide layer (3), and a ZnO:Al layer (5) with a thickness of 10 to 100 nm is magnetron sputtered on the ZnO layer (4); a second through hole (41) is opened through the ZnO layer (4) and the ZnO:Al layer (5); and the ZnO layer (4) and the ZnO:Al layer (5) are wet-etched so that the diameter of the second through hole (41) is larger than that of the first through hole (31); Depositing a front metal electrode layer (6) with a thickness of 10 to 80 nm on the ZnO:Al layer (5); Depositing a back metal electrode layer (7) on the lower surface of the silicon substrate (1); Metal pad electrodes (8) are deposited on the back metal electrode layer (7) and the front metal electrode layer (6), respectively.
4. The preparation method according to claim 3, characterized in that: The wet etching method specifically includes: etching using an NH4Cl solution with a mass concentration of 6% to 8%, so that the lateral etching rate is greater than the longitudinal etching rate.
5. The preparation method according to claim 3, characterized in that: The preparation process of the ZnO layer (4) comprises the following steps: Depositing Zn atoms: using a metal Zn target on the porous alumina layer (3), magnetron sputtering is performed in an argon atmosphere with a flow rate of 300 sccm, the Zn target power is controlled to be 5 kW, the substrate bias voltage is -50 V, and the time is 20 s to obtain a Zn layer; Bombardment process: bombarding the Zn layer, controlling the argon gas flow rate to 500 sccm, the substrate bias voltage to -500 V, the time to 10 seconds, and removing the Zn layer attached to the first through hole (31); Oxidation process: introducing oxygen, controlling the argon flow rate to 400 sccm, the oxygen flow rate to 600 sccm, and the power to 6 KW, to oxidize the Zn layer to form a ZnO layer (4).
6. The preparation method according to claim 5, characterized in that: The preparation process of the ZnO layer (4) is cyclically operated 8 to 20 times.
7. The preparation method according to claim 1, characterized in that: The preparation process of the ZnO:Al layer (5) comprises the following steps: Depositing ZnAl atoms: using a metal ZnAl target on the ZnO layer (4), magnetron sputtering is performed in an argon atmosphere with a flow rate of 300 sccm, the ZnAl target power is controlled to be 4KW, the substrate bias voltage is -50V, and the time is 20s to obtain a ZnAl layer; Bombardment process: bombarding the ZnAl layer, controlling the argon gas flow rate to 500 sccm, the substrate bias voltage to -600 V, the time to 10 s, to remove the newly grown ZnAl layer attached to the upper opening pore wall of the porous alumina layer (3); Oxidation process: oxygen is introduced, the argon flow rate is controlled to be 400 sccm, the oxygen flow rate is controlled to be 700 sccm, and the power is 6.5 KW to oxidize the deposited ZnAl layer to form a ZnO:Al layer (5).
8. The preparation method according to claim 7, characterized in that: The preparation process of the ZnO:Al layer (5) is cyclically operated 16 to 40 times.
9. The preparation method according to claim 3, characterized in that: The aperture of the first through hole (31) is ≤70 nm.
10. The preparation method according to claim 1, characterized in that: The front metal electrode layer (6) is an Au layer.