Laminate for flexible display device, laminate for display device, and flexible display device
Patent Information
- Application Number
- CN202410942385.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-09
- Filing Date
- 2021-03-09
- Publication Date
- 2024-11-08
Smart Images

Figure CN118918776A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese invention patent application with the application date of March 9, 2021, the invention name of "Laminate for flexible display device, laminate for display device and flexible display device", and the application number of 202180030768.1. Technical Field
[0002] The present invention relates to a laminate for a flexible display device, a laminate for a display device, and a flexible display device. Background Art
[0003] A laminate having a functional layer having various properties such as hard coating, scratch resistance, antireflection, antiglare, antistatic, and antifouling properties is disposed on the surface of the display device.
[0004] As the substrate layer in such a laminate, for example, a glass substrate or a resin substrate is used. However, the glass substrate and the resin substrate are easily charged due to their high insulation properties, and may be contaminated by the adhesion of dust or dirt. In addition, if static electricity is generated in the manufacturing process of the display device, the so-called electrostatic breakdown may sometimes be caused by the discharge of charged static electricity, that is, the electronic components constituting the display device are damaged. In addition, when a battery or other equipment is installed in the display device, there is also the possibility that the display device is charged. Therefore, in the past, in order to prevent such charging, it is known to use a laminate with an antistatic layer.
[0005] In recent years, not only smartphones and tablet terminals but also display devices such as notebook personal computers have touch functions. Display devices with touch functions are operated by directly touching the surface with fingers or the like, so wear resistance and sliding properties are required.
[0006] In addition, portable display devices such as smartphones and tablet terminals are sometimes stored in, for example, clothing pockets or bags, and the surface of the display device is sometimes rubbed by the fabric of the clothing or bag, other storage items in the clothing pocket or bag, etc. Therefore, portable display devices are further required to have wear resistance.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2016-125063
[0010] Patent Document 2: Japanese Patent No. 6140348 Summary of the invention
[0011] Problems to be solved by the invention
[0012] In recent years, flexible displays such as foldable displays, rollable displays, and bendable displays have attracted attention, and the development of laminates arranged on the surface of flexible displays is being actively carried out. For example, the use of resin substrates instead of glass substrates is being studied, and for example, Patent Document 1 proposes a display device window film, which includes a plastic substrate with high hardness and excellent optical properties, and a hard coating layer arranged on at least one surface of the plastic substrate.
[0013] Since a flexible display is used or stored in a bent state, for example, the surface of the bent portion is easily rubbed. Therefore, in a flexible display, the bent portion is further required to have excellent wear resistance.
[0014] Generally, in order to improve the wear resistance, it is known to increase the surface hardness or reduce the friction coefficient, for example.
[0015] However, in the case of the method of increasing the surface hardness, if the surface hardness of the laminate used for the flexible display is increased, there is a possibility that flexibility such as foldability, rollability, and bendability may be impaired.
[0016] In addition, as a method for reducing the friction coefficient, for example, a technique of imparting low friction by applying a fluorine-based surface treatment agent or adding a fluorine-based additive is known. For example, Patent Document 2 discloses a surface treatment agent containing a polymer composition containing a fluorine-containing oxyalkylene group, which can provide a coating having excellent water and oil repellency, scratch resistance, low dynamic friction, and wear resistance.
[0017] However, since the surface of the functional layer in the above-mentioned laminate is rubbed, the components contained in the functional layer may be rubbed off or the functional layer may be worn thin, and the performance of the functional layer may sometimes be reduced. As mentioned above, in flexible displays, further improvement in wear resistance is expected.
[0018] The present invention has been made in view of the above-mentioned actual situation, and a main object of the present invention is to provide a laminate for a flexible display device, a laminate for a display device, and a flexible display device having excellent wear resistance.
[0019] Means for solving problems
[0020] The inventors of the present invention have conducted intensive research on the wear resistance of a laminate for a flexible display device in order to solve the above-mentioned problems, and surprisingly found that there is a correlation between the wear resistance and the surface resistance. The present invention is based on this technical idea.
[0021] One embodiment of the present invention provides a laminate for a flexible display device, which is a laminate for a flexible display device having a substrate layer and an antistatic layer, wherein the surface resistance of the surface of the laminate for a flexible display device on the antistatic layer side is 9×10 13 Ω / □ or less. After a rubber test was performed on the surface of the antistatic layer side of the laminate for the flexible display device, in which a load of 9.8N was applied using a rubber with a diameter of 6mm and the surface resistance of the surface of the antistatic layer side of the laminate for the flexible display device was 9×10 13 Ω / □ or less.
[0022] In the laminate for a flexible display device of the present invention, the ratio of the surface resistance after the rubber test to the initial surface resistance of the surface on the antistatic layer side of the laminate for a flexible display device before the rubber test is preferably 20.0 or less.
[0023] Furthermore, the laminate for a flexible display device in the present invention may include a functional layer on the surface side of the antistatic layer of the substrate layer.
[0024] In the laminate for a flexible display device according to the present invention, the antistatic layer is preferably disposed on the outermost surface.
[0025] Furthermore, the laminate for a flexible display device in the present invention may include a shock absorbing layer on the surface of the substrate layer opposite to the antistatic layer, or between the substrate layer and the antistatic layer.
[0026] Furthermore, the laminate for a flexible display device in the present invention may include an adhesive layer for sticking on the surface of the substrate layer opposite to the antistatic layer.
[0027] Another embodiment of the present invention provides a display device laminate having a substrate layer and an antistatic layer, wherein the surface resistance of the surface of the display device laminate on the antistatic layer side is 9×10 13 Ω / □ or less. After a rubber test was performed on the surface of the antistatic layer side of the display device laminate using a 6 mm diameter rubber with a load of 9.8 N and rubbing back and forth 2500 times, the surface resistance of the surface of the antistatic layer side of the display device laminate was 9×10 13 Ω / □ or less.
[0028] Another embodiment of the present invention provides a flexible display device including: a display panel; and the above-mentioned laminate for a flexible display device disposed on a viewer side of the display panel.
[0029] Effects of the Invention
[0030] The present invention exerts an effect of being able to provide a flexible display device laminate, a display device laminate, and a flexible display device having excellent abrasion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic cross-sectional view illustrating a laminate for a flexible display device in the present invention.
[0032] Figure 2 It is a schematic diagram explaining the method of measuring the friction force with respect to rubber.
[0033] Figure 3 is a schematic diagram illustrating a dynamic bending test.
[0034] Figure 4 This is a schematic cross-sectional view illustrating a laminate for a flexible display device in the present invention.
[0035] Figure 5 This is a schematic cross-sectional view illustrating a laminate for a flexible display device in the present invention.
[0036] Figure 6 This is a schematic cross-sectional view illustrating a laminate for a flexible display device in the present invention.
[0037] Figure 7 is a schematic cross-sectional view illustrating a flexible display device in the present invention. DETAILED DESCRIPTION
[0038] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, etc. Among them, the present invention can be implemented in a variety of different ways, and is not to be construed as being limited to the contents of the embodiments illustrated below. In addition, in order to make the description clearer, the drawings sometimes schematically represent the width, thickness, shape, etc. of each part compared to the actual situation, but it is always an example and does not limit the interpretation of the present invention. In addition, in this specification and the drawings, the same reference numerals are given to the same elements as those in the drawings that have appeared, and the detailed description is appropriately omitted.
[0039] In this specification, when describing a method of arranging another component above a certain component, if it is simply described as "above" or "below", unless otherwise stated, it includes both the case where the other component is arranged directly above or directly below in a manner of contacting the certain component, and the case where the other component is arranged above or below the certain component with another component further interposed therebetween. In addition, in this specification, when describing a method of arranging another component on the surface of a certain component, if it is simply described as "surface side" or "surface", unless otherwise stated, it includes both the case where the other component is arranged directly above or directly below in a manner of contacting the certain component, and the case where the other component is arranged above or below the certain component with another component further interposed therebetween.
[0040] The inventors of the present invention have conducted intensive studies on the wear resistance of a laminate for a flexible display device and have obtained the following findings.
[0041] Generally, in order to improve the wear resistance, it is known to increase the surface hardness or reduce the friction coefficient, for example.
[0042] However, in the case of the method of increasing the surface hardness, in the laminate for a flexible display device, if the surface hardness is increased, there is a possibility that the flexibility is impaired. Therefore, the method of increasing the surface hardness is not suitable for the laminate for a flexible display device.
[0043] In addition, in the case of methods for reducing the friction coefficient, for example, it is known that a technique of imparting low friction by coating a fluorine-based surface treatment agent or adding a fluorine-based additive is used. However, for example, in the case where a laminate for a flexible display device has a functional layer having various properties, since the surface of the functional layer is rubbed, the components contained in the functional layer may be rubbed off, or the functional layer may be rubbed thin, thereby sometimes reducing the performance of the functional layer.
[0044] Therefore, the inventors of the present invention first prepared a laminate for a flexible display device having a substrate layer and a functional layer, and conducted a wear test on the laminate for a flexible display device, and studied the change in friction before and after the wear test. In addition, focusing on the rubber test and the surface resistance, the friction and surface resistance before and after the rubber test were measured, and it was found that: compared with before the rubber test, after the rubber test, although there was a tendency for both the friction and surface resistance to increase, when the surface resistance after the rubber test was relatively small, there was a tendency for the change in friction before and after the rubber test to become relatively small; and when the surface resistance after the rubber test was relatively large, there was a tendency for the change in friction before and after the rubber test to become relatively large. In addition, it was found that: when the initial surface resistance before the rubber test was small, there was a tendency for the surface resistance after the rubber test to become smaller. That is, it was found that: there is a correlation between wear resistance and the surface resistance after the rubber test. In addition, it was found that: the wear resistance can be easily inferred by the initial surface resistance before the rubber test. That is, it was newly found that: there is a good correlation between wear resistance and the surface resistance before and after the rubber test. Furthermore, the relationship between the wear resistance and the surface resistance before and after the rubber test was studied in detail. As a result, it was found that in order to impart excellent wear resistance, it is important to set the surface resistance before and after the rubber test to a predetermined value or less.
[0045] In the present invention, it is found that the surface resistance after the rubber test is reduced as an index for improving wear resistance, which is of great significance. In addition, it is found that the initial surface resistance before the rubber test is an index that can be used to infer wear resistance, which is of great significance.
[0046] Here, the reason for using the abrasion test using an eraser is that the friction using an eraser is similar to the friction using a stylus pen, and the abrasion resistance to relatively soft objects such as a stylus pen, a finger, clothes, or bag fabric can be evaluated through the eraser test. It should be noted that, as an abrasion test, for example, a steel wool test is also known, but since steel wool is a thin metal wire, it is obviously different from the relatively soft objects mentioned above, and therefore the abrasion resistance to the relatively soft objects mentioned above cannot be evaluated through the steel wool test.
[0047] Hereinafter, the laminate for a flexible display device, the laminate for a display device, and the flexible display device in the present invention will be described in detail.
[0048] A. Laminate for flexible display device
[0049] The laminate for a flexible display device in the present invention is a laminate for a flexible display device having a substrate layer and an antistatic layer, wherein the surface resistance of the surface of the laminate for a flexible display device on the antistatic layer side is 9×10 13Ω / □ or less. After a rubber test was performed on the surface of the antistatic layer side of the laminate for the flexible display device, in which a load of 9.8N was applied using a rubber with a diameter of 6mm and the surface resistance of the surface of the antistatic layer side of the laminate for the flexible display device was 9×10 13 Ω / □ or less.
[0050] Figure 1 Schematic cross-sectional view showing an example of a laminate for a flexible display device in the present invention. Figure 1 As shown, the laminate 1 for a flexible display device includes a substrate layer 2 and an antistatic layer 3. The surface resistance of the surface of the laminate 1 for a flexible display device on the antistatic layer 3 side is less than a specified value, and the surface resistance of the surface of the laminate 1 for a flexible display device on the antistatic layer 3 side after a specified rubber test is also less than a specified value.
[0051] As described above, the present invention is based on the new discovery that there is a correlation between the wear resistance and the surface resistance before and after the rubber test in the laminate for a flexible display device. In the present invention, excellent wear resistance can be obtained by making the surface resistance of the antistatic layer side of the laminate for a flexible display device before and after the rubber test less than a specified value.
[0052] The reason is not clear yet, but it is speculated as follows. That is, if a rubber test is performed on the surface of the laminate for a flexible display device, the surface of the laminate for a flexible display device will be charged due to friction using a rubber. And if discharge occurs, the layers constituting the laminate for a flexible display device deteriorate and sometimes electrostatic breakdown occurs. If such electrostatic breakdown occurs, it is believed that the surface state of the laminate for a flexible display device changes, and the wear resistance sometimes decreases. In contrast, in the present invention, since the surface resistance of the surface on the antistatic layer side of the laminate for a flexible display device after the rubber test is below the specified value, it is believed that the charging of the surface on the antistatic layer side of the laminate for a flexible display device caused by the rubber test can be suppressed, and the degradation and electrostatic breakdown of the above-mentioned layer can be suppressed. As a result, it is speculated that excellent wear resistance can be obtained.
[0053] In addition, in the present invention, since the surface resistance of the antistatic layer side of the laminate for a flexible display device after the rubber test is below a specified value, the wear resistance against relatively soft objects such as a stylus pen, fingers, clothes or bag fabrics can be improved.
[0054] In addition, in the present invention, since the wear resistance can be easily estimated from the initial surface resistance before the rubber test, it is possible to provide a laminate for a flexible display device that can be easily designed to achieve the target wear resistance.
[0055] Hereinafter, each structure of the laminate for a flexible display device in the present invention will be described.
[0056] 1. Characteristics of laminates for flexible display devices
[0057] In the present invention, the surface resistance of the antistatic layer side of the laminate for a flexible display device can be 9×10 13 Ω / □ or less, preferably 9×10 12 Ω / □ or less. If the initial surface resistance of the surface on the antistatic layer side of the laminate for a flexible display device is within the above range, the surface resistance of the surface on the antistatic layer side of the laminate for a flexible display device after a predetermined rubber test tends to be within a predetermined range, and it can be inferred that excellent wear resistance is obtained. In addition, if the initial surface resistance of the surface on the antistatic layer side of the laminate for a flexible display device is within the above range, excellent antistatic properties can be obtained.
[0058] In addition, in the present invention, the surface of the antistatic layer side of the laminate for a flexible display device is subjected to a rubber test in which a load of 9.8 N is applied using a rubber with a diameter of 6 mm and the surface resistance of the surface of the antistatic layer side of the laminate for a flexible display device is 9×10 13 Ω / □ or less, preferably 5×10 13 Ω / □ or less, more preferably 9×10 12 Ω / □ or less. By setting the surface resistance of the antistatic layer side of the laminate for a flexible display device after a predetermined rubber test to be within the above range, excellent abrasion resistance can be obtained and excellent antistatic properties can be maintained.
[0059] In addition, on the surface of the antistatic layer side of the laminate for flexible display device, the ratio of the surface resistance after the rubber test to the initial surface resistance is, for example, preferably less than 20.0, more preferably less than 10.0, and further preferably less than 5.0. By making the ratio of the above surface resistance within the above range, the wear resistance can be improved. The reason is not yet clear, but it is speculated as follows. That is, the ratio of the above surface resistance becomes larger, for example, in the following case: the initial surface resistance is small, and the surface resistance after the rubber test becomes larger. On the other hand, the ratio of the above surface resistance becomes smaller, for example, in the following case: the initial surface resistance is small, and the surface resistance after the rubber test also becomes smaller. In the latter case, it is believed that the surface of the laminate for flexible display device is not easily charged due to friction using rubber, and electrostatic breakdown is not easy to occur. Therefore, it is believed that by making the ratio of the above surface resistance smaller than the above range, the charging of the surface on the antistatic layer side of the laminate for flexible display device caused by the rubber test can be further suppressed, and electrostatic breakdown can be further suppressed. As a result, it is speculated that the wear resistance can be improved. In addition, since the surface resistance after the rubber test tends to be larger than that before the rubber test, the ratio of the surface resistance can be, for example, 1.0 or more.
[0060] When the surface resistance of the antistatic layer side of the initial flexible display device laminate before the rubber test is A and the surface resistance of the antistatic layer side of the flexible display device laminate after the rubber test is B, the ratio of the surface resistances is calculated by the following formula.
[0061] Surface resistance ratio = B / A
[0062] Here, the rubber test can be performed by the following method. That is, a rubber with a diameter of 6 mm is used, and a fixture with a hole with a diameter of 6 mm is inserted in such a way that the front end of the rubber is exposed by 4 mm. The fixture with the rubber is installed in a Gakushin type friction tester, and the surface of the antistatic layer side of the laminate for the flexible display device is rubbed back and forth 2500 times with a load of 9.8 N and a moving speed of 80 mm / second using the rubber. As a rubber with a diameter of 6 mm, for example, a φ6 mm rubber manufactured by Minoan can be used. In addition, as a Gakushin type friction tester, for example, a Gakushin type friction fastness tester AB-301 manufactured by TESTER SANGYO can be used.
[0063] In addition, regarding the surface resistance, the Hiresta UX MCP-HT type manufactured by Mitsubishi Chemical Analytech can be used as a resistivity meter, and as a probe, the MCP-HTO 14UR S probe is used after the rubber test, and the MCP-HTP11 UA probe is used in the initial stage before the rubber test, and the measurement is performed with an applied voltage of 1000 V. In addition, the surface resistance is measured at 10 locations on the surface of the antistatic layer side of the laminate for the flexible display device, and the arithmetic mean of the values measured at the 10 locations. It should be noted that when measuring the surface resistance, the laminate for the flexible display device is left to stand for 1 hour under an environment of a temperature of 23±2°C and a humidity of 50±10% before the measurement.
[0064] In addition, the surface on the antistatic layer side of the laminate for a flexible display device refers to the surface on the side where the antistatic layer is arranged among the substrate layer and the antistatic layer in the laminate for a flexible display device having at least a substrate layer and an antistatic layer. In the laminate for a flexible display device, there is not only a case where the antistatic layer is arranged on the outermost surface, but there is also a case where the substrate layer, the antistatic layer and the functional layer are sequentially stacked, for example, as described later. In this way, for example, in the case where the substrate layer, the antistatic layer and the functional layer are sequentially stacked, the surface on the side where the functional layer is arranged becomes the surface where the antistatic layer is arranged.
[0065] In addition, in the present invention, the average value of the friction force of the surface of the antistatic layer side of the laminate for a flexible display device against the rubber is, for example, preferably 0.98 N to 9.80 N, more preferably 1.96 N to 8.80 N, and further preferably 2.45 N to 7.80 N. If the average value of the initial friction force against the rubber is within the above range, the wear resistance can be improved.
[0066] In addition, in the present invention, after a rubber test in which a load of 9.8 N is applied to the surface of the antistatic layer side of the laminate for a flexible display device and rubbed back and forth 2500 times using a rubber with a diameter of 6 mm, the maximum value of the friction force of the surface of the antistatic layer side of the laminate for a flexible display device against the rubber is, for example, preferably 0.98 N to 9.80 N, more preferably 1.96 N to 8.80 N, and further preferably 2.45 N to 7.80 N. By setting the maximum value of the friction force of the surface of the antistatic layer side of the laminate for a flexible display device against the rubber after the predetermined rubber test to be within the above range, excellent wear resistance can be obtained and excellent antistatic properties can be maintained.
[0067] In addition, the ratio of the maximum value of the friction force of the surface on the antistatic layer side of the laminate for a flexible display device to the rubber after the rubber test to the average value of the initial friction force to the rubber is, for example, preferably 1.50 or less, more preferably 1.48 or less, and further preferably 1.45 or less. By making the ratio of the friction force to the rubber within the above range, the wear resistance can be improved. In addition, the ratio of the friction force to the rubber can be, for example, 1.00 or more.
[0068] When the average value of the friction force of the antistatic layer side of the initial flexible display device laminate with respect to the rubber before the rubber test is set to C, and the maximum value of the friction of the antistatic layer side of the flexible display device laminate with respect to the rubber after the rubber test is set to D, the ratio of the above friction force with respect to the rubber is calculated by the following formula.
[0069] The ratio of friction to rubber = D / C
[0070] Here, regarding the friction force with the rubber, a rubber with a diameter of 6 mm can be used, and a fixture with a hole with a diameter of 6 mm can be inserted in such a way that the front end of the rubber is exposed by 4 mm. The fixture with the rubber is mounted on a friction measuring machine, and the surface of the antistatic layer side of the laminate for the flexible display device is rubbed with the rubber at a load of 1.96 N and a moving speed of 840 mm / min to perform the measurement. As an eraser with a diameter of 6 mm, for example, a φ6 mm eraser manufactured by Minoan can be used. In addition, as a friction measuring machine, for example, TRIBOGEAR TYPE18 manufactured by Shinto Science Co., Ltd. can be used. Specifically, as Figure 2As shown, first, the above-mentioned rubber test is performed on a portion of the surface 30 on the antistatic layer side of the laminate 1 for the flexible display device to form a rectangular rubber test implementation portion 32. Next, a rubber is used to rub the surface 30 on the antistatic layer side of the laminate 1 for the flexible display device in the order of the rubber test non-implemented portion 31, the rubber test implemented portion 32, and the rubber test non-implemented portion 31 as shown by the arrows, and the friction force is measured. At this time, the rubber is moved perpendicularly to the long side direction of the rectangular rubber test implementation portion 32 as shown by the arrow. The average value of the friction force of the rubber non-implemented portion to the rubber can be taken as the average value of the initial friction force to the rubber, and the maximum value of the friction force of the rubber test implemented portion to the rubber can be taken as the maximum value of the friction force to the rubber after the rubber test. In addition, regarding the initial average value of the friction force to the rubber, as shown in FIG. Figure 2 As shown, when the point where the friction force of the rubber to the rubber in the rubber test implementation part 32 reaches the maximum value is set to 0 mm, it is the average value of the friction force in the range of 4.2 mm to 9.8 mm in the rubber test non-implemented part 31 with the above point (0 mm) as the reference.
[0071] In addition, in the present invention, the contact angle of the surface of the antistatic layer side of the laminate for a flexible display device to water is preferably, for example, 100° or more. If the contact angle to water is within the above range, sufficient antifouling properties can be obtained, thereby suppressing the adhesion of fingerprints or dirt, and even if fingerprints or dirt are attached, they can be easily wiped off. In addition, the contact angle to water is preferably, for example, 150° or less.
[0072] Here, the contact angle with respect to water can be measured by a sessile drop method in accordance with JIS R3257:1999. Specifically, 2 μL of water is dropped on the surface of the antistatic layer side of the laminate for a flexible display device, and the contact angle immediately after the dropping is measured. Regarding the contact angle with respect to water, the contact angle of the surface of the antistatic layer side of the laminate for a flexible display device with respect to water is measured at 10 locations, and the arithmetic mean of the measured values at the 10 locations is obtained. As a measuring device, for example, a contact angle meter DropMaster300 manufactured by Kyowa Interface Science Co., Ltd. can be used. It should be noted that the contact angle of the surface of the antistatic layer side of the laminate for a flexible display device with respect to water refers to the initial contact angle of the surface of the antistatic layer side of the laminate for a flexible display device with respect to water before the above-mentioned rubber test.
[0073] The total light transmittance of the laminate for a flexible display device in the present invention is preferably 85% or more, more preferably 88% or more, and further preferably 90% or more. Such a high total light transmittance can provide a laminate for a flexible display device with good transparency.
[0074] Here, the total light transmittance of the laminate for a flexible display device can be measured in accordance with JIS K7361-1:1997, for example, by using a haze meter HM150 manufactured by Murakami Color Research Laboratory.
[0075] The haze of the laminate for a flexible display device in the present invention is, for example, preferably 5% or less, more preferably 2% or less, and further preferably 1% or less. By making the haze so low, a laminate for a flexible display device having good transparency can be obtained.
[0076] Here, the haze of the laminate for a flexible display device can be measured in accordance with JIS K-7136:2000, for example, by using a haze meter HM150 manufactured by Murakami Color Research Laboratory.
[0077] The laminate for a flexible display device in the present invention preferably has bending resistance.
[0078] Specifically, it is preferred that the flexible display device laminate does not produce cracks or breaks when the dynamic bending test described below is repeated 200,000 times, and it is further preferred that the flexible display device laminate does not produce cracks or breaks when the dynamic bending test described below is repeated 500,000 times.
[0079] In the dynamic bending test, the flexible display device laminate can be folded with the antistatic layer on the outside or on the inside. Preferably, in either case, the flexible display device laminate does not produce cracks or breaks.
[0080] (Dynamic bending test)
[0081] The dynamic bending test was conducted as follows. First, a 20 mm × 100 mm laminate for a flexible display device was prepared. Figure 3 As shown in (a), the short side 10C of the flexible display device laminate 1 and the short side 10D facing the short side 10C are fixed by the fixing parts 51 arranged in parallel. Figure 3 As shown in (a), the fixing portion 51 can slide in the horizontal direction. Figure 3 As shown in (b), the fixing parts 51 are moved so as to approach each other, thereby deforming the laminate 1 for the flexible display device in a folded manner, and then, as shown in Figure 3 As shown in (c), the fixing portion 51 is moved to a position where the interval d between the two opposing short sides 10C and 10D fixed by the fixing portion 51 of the flexible display device laminate 1 reaches 30 mm, and then the fixing portion 51 is moved in the reverse direction to eliminate the deformation of the flexible display device laminate 1. Figure 3By moving as shown in (a) to (c), the flexible display device laminate 1 can be folded 180°. In addition, by performing a dynamic bending test in a manner such that the bent portion 10E of the flexible display device laminate 1 does not protrude from the lower end of the fixing portion 51, and controlling the interval when the fixing portion 51 is closest, the interval d between the two opposing short sides 10C and 10D of the flexible display device laminate 1 can be set to 30 mm. In this case, the outer diameter of the bent portion 10E is considered to be 30 mm.
[0082] In the laminate for a flexible display device, it is preferred that no cracks or breaks are generated when a dynamic bending test in which the laminate 1 for a flexible display device is folded 180° with a spacing d of 30 mm between the opposing short sides 10C, 10D is repeated 200,000 times, wherein it is further preferred that no cracks or breaks are generated when a dynamic bending test in which the laminate 1 for a flexible display device is folded 180° with a spacing d of 20 mm between the opposing short sides 10C, 10D is repeated 200,000 times, and it is particularly preferred that no cracks or breaks are generated when a dynamic bending test in which the laminate 1 for a flexible display device is folded 180° with a spacing d of 10 mm between the opposing short sides 10C, 10D is repeated 200,000 times.
[0083] 2. Antistatic layer
[0084] The antistatic layer in the present invention is a layer disposed on one surface side of the base layer and is used to impart antistatic properties to the laminate for a flexible display device.
[0085] The antistatic layer is not particularly limited as long as it has antistatic properties, and may contain at least an antistatic agent. In addition, the antistatic layer may contain, for example, an antistatic agent and a resin.
[0086] As the antistatic agent, for example, any of a low molecular weight antistatic agent and a polymer antistatic agent can be used. In addition, as the antistatic agent, for example, an ion conductive antistatic agent, an electron conductive antistatic agent, etc. can be cited. The antistatic agent can be used alone or in combination of two or more.
[0087] Examples of the ion-conducting antistatic agent include: cationic antistatic agents such as quaternary ammonium salts and pyridinium salts; anionic antistatic agents such as alkali metal salts of sulfonic acid, phosphoric acid, carboxylic acid, etc. such as lithium salts, sodium salts, potassium salts, etc.; amphoteric antistatic agents such as amino acid series and amino acid sulfate series; nonionic antistatic agents such as amino alcohol series, glycerol series, polyethylene glycol series; ionic liquids, etc. Among these, quaternary ammonium salts and lithium salts are preferred because they have excellent compatibility with resins.
[0088] As the above-mentioned electron conductive antistatic agent, for example, conductive polymers such as polyacetylene and polythiophene can be cited; conductive particles such as metal particles, metal oxide particles, carbon nanotubes, or conductive fibers can be cited. In addition, antistatic agents in which conductive polymers such as polyacetylene and polythiophene are combined with dopants, or antistatic agents containing conductive particles in the above-mentioned conductive polymers can also be used. Among these, conductive polymers are preferred from the aspect of maintaining antistatic properties.
[0089] As the conductive polymer, specifically, polyacetylene, polyaniline, polythiophene, polypyrrole, polyphenylene sulfide, poly(1,6-heptadiyne), polybiphenylene (polyparaphenylene), polyparaphenylene sulfide, polyphenylene vinylene, poly(2,5-thiophene), or their derivatives can be cited. Preferably, polythiophene-based conductive polymers such as 3,4-ethylenedioxythiophene (PEDOT) can be cited. By using the conductive polymer as an antistatic agent, antistatic properties can be maintained for a long time.
[0090] Examples of the metal constituting the metal fine particles include single metals such as Au, Ag, Cu, Al, Fe, Ni, Pd, and Pt, and alloys of these metals.
[0091] The metal oxide constituting the metal oxide particles is not particularly limited, and examples thereof include tin oxide, antimony oxide, antimony-doped tin oxide (ATO), tin-doped indium oxide (ITO), aluminum-doped zinc oxide (AZO), fluorine-doped tin oxide (FTO), zinc oxide (ZnO), etc. Among them, antimony-doped tin oxide (ATO) is preferred from the perspective of exerting excellent antistatic properties. In addition, among ATO, chain-like ATO formed by connecting a plurality of ATO particles is preferred.
[0092] Among the above antistatic agents, non-granular antistatic agents are preferred. The reason is that, compared with granular antistatic agents, non-granular antistatic agents are easy to maintain antistatic properties. The antistatic agent is particularly preferably a polymer antistatic agent. The reason is that: polymer antistatic agents can impart antistatic properties even in a small amount and can maintain optical properties or hardness.
[0093] The content of the antistatic agent is not particularly limited as long as it is an amount that can obtain an antistatic layer satisfying the above-mentioned surface resistance, and is appropriately selected depending on the material of the antistatic layer and the like.
[0094] For example, when antistatic layer contains antistatic agent and resin, the content of antistatic agent can be more than 0.1 mass part and less than 100 mass parts relative to above-mentioned resin composition 100 mass parts, can also be more than 0.2 mass part and less than 50 mass parts, can also be more than 0.3 mass part and less than 20 mass parts.If the content of antistatic agent is too little, then there is the situation that antistatic layer cannot be given sufficient antistatic property or the situation that antistatic layer that satisfies above-mentioned surface resistance cannot be obtained.In addition, if the content of antistatic agent is too much, then there is the formation difficulty of antistatic layer or the reduction of wear resistance.
[0095] The resin can be appropriately selected depending on the performance to be imparted to the antistatic layer.
[0096] For example, when the antistatic layer may not have hard coating properties, as the resin, specifically, at least one selected from the group consisting of (meth) acrylic resin, cellulose resin, carbamate resin, vinyl chloride resin, polyester resin, polyolefin resin, polycarbonate, nylon, polystyrene and ABS resin can be cited. Among these, from the aspect of ease of processing and hardness, (meth) acrylic resin, polyester resin, etc. are preferred.
[0097] Examples of the (meth)acrylic resin include polymethyl methacrylate, etc. Examples of the cellulose resin include diacetyl cellulose, cellulose acetate propionate (CAP), cellulose acetate butyrate (CAB), etc. Examples of the urethane resin include urethane resin, etc.
[0098] Examples of the vinyl chloride resin include polyvinyl chloride and vinyl chloride-vinyl acetate copolymers. Examples of the polyester resin include polyethylene terephthalate. Examples of the polyolefin resin include polyethylene and polypropylene.
[0099] In addition, for example, when the antistatic layer has hard coating properties, the resin may be, specifically, a cured product of a polymerizable compound. It should be noted that the polymerizable compound may be the same as the polymerizable compound used in the hard coating layer described later, and thus the description here is omitted.
[0100] The antistatic layer may contain an antifouling agent, thereby providing the laminate for a flexible display device with antifouling properties.
[0101] The antifouling agent is not particularly limited, and examples thereof include silicone antifouling agents, fluorine antifouling agents, and silicone and fluorine antifouling agents. In addition, the antifouling agent may also be an acrylic antifouling agent. The antifouling agent may be used alone or in combination of two or more.
[0102] The antistatic layer containing silicone antifouling agents and fluorine antifouling agents is not easy to be attached with fingerprints (not conspicuous) and has good wiping properties. In addition, when silicone antifouling agents and fluorine antifouling agents are included, the surface tension when the antistatic layer composition is applied can be reduced, so the leveling property is good, and the appearance of the obtained antistatic layer becomes good.
[0103] In addition, the antistatic layer containing the silicone antifouling agent has good sliding properties and good scratch resistance. The display device having the flexible display device laminate having the antistatic layer containing the silicone antifouling agent has good sliding properties when touched with a finger or a stylus pen, and thus has good touch.
[0104] In order to improve the durability of the antifouling performance, the antifouling agent preferably has a reactive functional group. In the case where the antifouling agent does not have a reactive functional group, regardless of whether the flexible display device laminate is in a roll or sheet form, when the flexible display device laminate is overlapped, the antifouling agent will be transferred to the surface of the flexible display device laminate opposite to the surface of the antistatic layer side, and when other layers are attached or coated on the surface of the flexible display device laminate opposite to the surface of the antistatic layer side, the other layers may peel off, and in addition, when repeatedly bent, the other layers may easily peel off. In contrast, when the antifouling agent has a reactive functional group, the performance sustainability of the antifouling performance becomes good.
[0105] The number of reactive functional groups possessed by the antifouling agent may be 1 or more, and is preferably 2 or more. By using an antifouling agent having 2 or more reactive functional groups, excellent scratch resistance can be imparted to the antistatic layer.
[0106] The content of the antifouling agent is, for example, preferably 0.01 parts by mass or more and 3.0 parts by mass or less relative to 100 parts by mass of the resin component. If the content of the antifouling agent is too little, sufficient antifouling property may not be imparted to the antistatic layer. In addition, if the content of the antifouling agent is too much, the wear resistance may be reduced.
[0107] The antistatic layer may contain additives such as inorganic particles, organic particles, ultraviolet absorbers, antioxidants, light stabilizers, antiglare agents, leveling agents, surfactants, lubricants, various sensitizers, flame retardants, tackifiers, polymerization inhibitors, surface modifiers, etc. as needed.
[0108] The thickness of the antistatic layer is not particularly limited as long as the amount of the antistatic layer that satisfies the above-mentioned surface resistance can be obtained, for example, preferably 0.5 μm to 50 μm, more preferably 1.0 μm to 40 μm, and further preferably 1.5 μm to 30 μm. If the thickness of the antistatic layer is too thin, sufficient antistatic properties may not be obtained. In addition, if the thickness of the antistatic layer is too thick, flexibility may be impaired.
[0109] Here, the thickness of the antistatic layer may be the average value of the thickness of any 10 locations measured in the thickness direction of the laminate for a flexible display device observed by a transmission electron microscope (TEM), a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM). It should be noted that the method for measuring the thickness of other layers of the laminate for a flexible display device may also be the same.
[0110] The antistatic layer may be disposed on one side of the substrate layer, and in the laminate for a flexible display device, the antistatic layer is preferably disposed on the outermost surface, because the surface resistance of the antistatic layer side of the laminate for a flexible display device can easily satisfy the above surface resistance.
[0111] As a method for forming the antistatic layer, for example, there is a method of applying a composition for an antistatic layer on a base layer and curing the composition.
[0112] 3. Base material layer
[0113] The base layer in the present invention is a member that supports the antistatic layer and has transparency.
[0114] The substrate layer is not particularly limited as long as it has transparency, and examples thereof include a resin substrate and a glass substrate.
[0115] (1) Resin substrate
[0116] As the resin constituting the resin substrate, there is no particular limitation as long as a transparent resin substrate can be obtained, and examples thereof include polyimide resins, polyamide resins, polyester resins, etc. As the polyimide resins, examples thereof include polyimide, polyamide-imide, polyether-imide, polyester-imide, etc. As the polyester resins, examples thereof include polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc. Among them, from the aspects of having bending resistance, excellent hardness and transparency, polyimide resins, polyamide resins, or mixtures thereof are preferred, and polyimide resins are more preferred.
[0117] The polyimide resin is not particularly limited as long as a transparent resin substrate can be obtained, and among the above, polyimide and polyamideimide are preferably used.
[0118] (a) Polyimide
[0119] The polyimide is obtained by reacting a tetracarboxylic acid component with a diamine component. The polyimide is not particularly limited as long as it satisfies the average value of the tensile storage modulus and has transparency. For example, from the perspective of having excellent transparency and excellent rigidity, it is preferred to have at least one structure selected from the group consisting of structures represented by the following general formula (1) and the following general formula (3).
[0120] [Chemistry 1]
[0121]
[0122] In the above general formula (1), R 1 represents a tetravalent group which is a tetracarboxylic acid residue, R 2 represents at least one divalent group selected from the group consisting of a trans-cyclohexanediamine residue, a trans-1,4-bismethylenecyclohexanediamine residue, a 4,4'-diaminodiphenyl sulfone residue, a 3,4'-diaminodiphenyl sulfone residue, and a divalent group represented by the following general formula (2). n represents the number of repeating units and is 1 or more.
[0123] [Chemistry 2]
[0124]
[0125] In the above general formula (2), R 3 and R 4 Each independently represents a hydrogen atom, an alkyl group, or a perfluoroalkyl group.
[0126] [Chemistry 3]
[0127]
[0128] In the above general formula (3), R 5 represents at least one tetravalent group selected from the group consisting of a cyclohexanetetracarboxylic acid residue, a cyclopentanetetracarboxylic acid residue, a dicyclohexane-3,4,3',4'-tetracarboxylic acid residue and a 4,4'-(hexafluoroisopropylidene)diphthalic acid residue, and R 6 represents a divalent group which is a diamine residue. n' represents the number of repeating units and is 1 or more.
[0129] It should be noted that the "tetracarboxylic acid residue" refers to a residue obtained by removing four carboxyl groups from tetracarboxylic acid, and has the same structure as a residue obtained by removing the dianhydride structure from tetracarboxylic dianhydride. In addition, the "diamine residue" refers to a residue obtained by removing two amino groups from diamine.
[0130] In the above general formula (1), R 1It is a tetracarboxylic acid residue, and may be a residue obtained by removing the dianhydride structure from tetracarboxylic dianhydride. As tetracarboxylic dianhydride, for example, tetracarboxylic dianhydride described in International Publication No. 2018 / 070523 may be mentioned. As R in the above general formula (1), 1 , wherein, from the perspective of improving transparency and improving rigidity, it is preferred to contain at least one selected from the group consisting of 4,4'-(hexafluoroisopropylidene)diphthalic acid residues, 3,3',4,4'-biphenyltetracarboxylic acid residues, pyromellitic acid residues, 2,3',3,4'-biphenyltetracarboxylic acid residues, 3,3',4,4'-benzophenonetetracarboxylic acid residues, 3,3',4,4'-diphenylsulfonetetracarboxylic acid residues, 4,4'-oxydiphthalic acid residues, cyclohexanetetracarboxylic acid residues and cyclopentanetetracarboxylic acid residues, and further preferably contains at least one selected from the group consisting of 4,4'-(hexafluoroisopropylidene)diphthalic acid residues, 4,4'-oxydiphthalic acid residues and 3,3',4,4'-diphenylsulfonetetracarboxylic acid residues.
[0131] R 1 The total amount of these preferred residues is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more.
[0132] In addition, as R 1 It is also preferred to mix the following group A and group B, wherein group A is a tetracarboxylic acid residue group selected from the group consisting of 3,3',4,4'-biphenyltetracarboxylic acid residues, 3,3',4,4'-benzophenonetetracarboxylic acid residues and pyromellitic acid residues, and at least one such tetracarboxylic acid residue group suitable for improving rigidity, and group B is a tetracarboxylic acid residue group selected from the group consisting of 4,4'-(hexafluoroisopropyl)diphthalic acid residues, 2,3',3,4'-biphenyltetracarboxylic acid residues, 3,3',4,4'-diphenylsulfonetetracarboxylic acid residues, 4,4'-oxydiphthalic acid residues, cyclohexanetetracarboxylic acid residues and cyclopentanetetracarboxylic acid residues, and at least one such tetracarboxylic acid residue group suitable for improving transparency.
[0133] In this case, regarding the content ratio of the tetracarboxylic acid residue group (group A) suitable for improving rigidity and the tetracarboxylic acid residue group (group B) suitable for improving transparency, the tetracarboxylic acid residue group (group A) suitable for improving rigidity is preferably 0.05 mol to 9 mol, more preferably 0.1 mol to 5 mol, and even more preferably 0.3 mol to 4 mol, per 1 mol of the tetracarboxylic acid residue group (group B) suitable for improving transparency.
[0134] As R in the above general formula (1) 2In terms of improving transparency and rigidity, at least one divalent group selected from the group consisting of a 4,4'-diaminodiphenyl sulfone residue, a 3,4'-diaminodiphenyl sulfone residue and a divalent group represented by the general formula (2) is preferred, and more preferably selected from the group consisting of a 4,4'-diaminodiphenyl sulfone residue, a 3,4'-diaminodiphenyl sulfone residue, and R 3 and R 4 At least one divalent group selected from the group consisting of divalent groups represented by the above general formula (2) which is a perfluoroalkyl group.
[0135] As R in the above general formula (3) 5 Among them, from the viewpoint of improving transparency and improving rigidity, it is preferred to contain a 4,4′-(hexafluoroisopropylidene)diphthalic acid residue, a 3,3′,4,4′-diphenylsulfonetetracarboxylic acid residue, and an oxydiphthalic acid residue.
[0136] R 5 The preferred residues are preferably contained in an amount of 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more.
[0137] In the above general formula (3), R 6 It is a diamine residue, and may be a residue obtained by removing two amino groups from a diamine. Examples of diamines include diamines described in International Publication No. 2018 / 070523. As R in the general formula (3), 6 Among them, from the perspective of improving transparency and improving rigidity, it is preferred to contain a 2,2'-bis(trifluoromethyl)benzidine residue, a bis[4-(4-aminophenoxy)phenyl]sulfone residue, a 4,4'-diaminodiphenylsulfone residue, a 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane residue, a bis[4-(3-aminophenoxy)phenyl]sulfone residue, a 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether residue, a 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene residue, a 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane residue, a bis[4-(3-aminophenoxy)phenyl]sulfone residue, a 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether residue, a 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene residue, a 2,2-bis[4-(4- The present invention further preferably contains at least one divalent group selected from the group consisting of a 2,2'-bis(trifluoromethyl)benzidine residue, a bis[4-(4-aminophenoxy)phenyl]sulfone residue and a 4,4'-diaminodiphenyl sulfone residue.
[0138] R 6The total amount of these preferred residues is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more.
[0139] In addition, as R 6 It is also preferred to use the following group C mixed with group D, wherein group C is a diamine residue group suitable for improving rigidity selected from the group consisting of bis[4-(4-aminophenoxy)phenyl]sulfone residue, 4,4'-diaminobenzanilide residue, N,N'-bis(4-aminophenyl)terephthalamide residue, p-phenylenediamine residue, m-phenylenediamine residue and 4,4'-diaminodiphenylmethane residue, and group D is a diamine residue selected from the group consisting of 2,2'-bis(trifluoromethyl)benzidine residue, 4,4'-diaminodiphenylsulfone residue, 2,2-bis[4-(4-aminophenyl)terephthalamide residue, p-phenylenediamine residue, m-phenylenediamine residue and 4,4'-diaminodiphenylmethane residue. The invention also provides a diamine residue group suitable for improving transparency, which comprises at least one of the group consisting of a bis[4-(3-aminophenoxy)phenyl]hexafluoropropane residue, a bis[4-(3-aminophenoxy)phenyl]sulfone residue, a 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether residue, a 1,4-bis[4-amino-2-(trifluoromethyl)phenoxy]benzene residue, a 2,2-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane residue, a 4,4'-diamino-2-(trifluoromethyl)diphenyl ether residue and a 9,9-bis(4-aminophenyl)fluorene residue.
[0140] In this case, regarding the content ratio of the above-mentioned diamine residue group (group C) suitable for improving rigidity and the diamine residue group (group D) suitable for improving transparency, the diamine residue group (group C) suitable for improving rigidity is preferably 0.05 mol to 9 mol, more preferably 0.1 mol to 5 mol, and even more preferably 0.3 mol to 4 mol, relative to 1 mol of the diamine residue group (group D) suitable for improving transparency.
[0141] In the structures represented by the general formula (1) and the general formula (3), n and n' each independently represent the number of repeating units and are greater than 1. The number of repeating units n in the polyimide can be appropriately selected according to the structure and is not particularly limited. The average number of repeating units can be, for example, greater than 10 and less than 2000, preferably greater than 15 and less than 1000.
[0142] The polyimide may contain a polyamide structure in part thereof. Examples of the polyamide structure that may be contained include a polyamideimide structure containing a tricarboxylic acid residue such as trimellitic anhydride, and a polyamide structure containing a dicarboxylic acid residue such as terephthalic acid.
[0143] From the perspective of improving transparency and surface hardness, R 1 or R 5 The tetravalent group of the tetracarboxylic acid residue, and the2 or R 6 At least one of the divalent groups of the diamine residue preferably contains an aromatic ring and contains at least one selected from the group consisting of (i) fluorine atoms, (ii) aliphatic rings, and (iii) aromatic rings connected to each other with sulfonyl groups or fluorine-substituted or unsubstituted alkylene groups. By making the polyimide contain at least one selected from tetracarboxylic acid residues having aromatic rings and diamine residues having aromatic rings, the molecular skeleton becomes rigid, thereby improving orientation and surface hardness, but the rigid aromatic ring skeleton has a tendency to extend the absorption wavelength to a long wavelength, and the transmittance in the visible light region tends to decrease. On the other hand, if the polyimide contains (i) fluorine atoms, the transparency is improved from the aspect that the electronic state in the polyimide skeleton is not easily subject to charge transfer.
[0144] In addition, if the polyimide contains (ii) an aliphatic ring, the transparency is improved from the aspect that the movement of charges in the polyimide skeleton can be inhibited by cutting the conjugation of π electrons in the polyimide skeleton. In addition, if the polyimide contains (iii) a structure in which aromatic rings are linked to each other by a sulfonyl group or a fluorine-substituted or unsubstituted alkylene group, the transparency is improved from the aspect that the movement of charges in the polyimide skeleton can be inhibited by cutting the conjugation of π electrons in the polyimide skeleton.
[0145] Among them, from the perspective of improving transparency and surface hardness, R 1 or R 5 The tetravalent group of the tetracarboxylic acid residue, and the 2 or R 6 At least one of the divalent groups of the diamine residue preferably contains an aromatic ring and a fluorine atom, and as R 2 or R 6 The divalent group of the diamine residue preferably contains an aromatic ring and a fluorine atom.
[0146] As a specific example of such a polyimide, a substance having a specific structure described in International Publication No. 2018 / 070523 can be mentioned.
[0147] The polyimide can be synthesized by a known method. In addition, commercially available polyimides can be used. Examples of commercially available polyimides include Neopulim (registered trademark) manufactured by Mitsubishi Gas Chemical Co., Ltd.
[0148] The weight average molecular weight of the polyimide is, for example, preferably 3000 to 500,000, more preferably 5000 to 300,000, and further preferably 10,000 to 200,000. If the weight average molecular weight is too small, sufficient strength may not be obtained, and if the weight average molecular weight is too large, viscosity increases and solubility decreases, so that a substrate layer with a smooth surface and uniform thickness may not be obtained.
[0149] It should be noted that the weight average molecular weight of polyimide can be measured by gel permeation chromatography (GPC). Specifically, polyimide is made into a 0.1 mass% concentration of N-methylpyrrolidone (NMP) solution, and the developing solvent uses a 30mmol% LiBr-NMP solution with a water content of less than 500ppm, using a GPC device manufactured by Tosoh (HLC-8120, column used: GPC LF-804 manufactured by SHODEX), and is measured under the conditions of sample injection volume 50μL, solvent flow rate 0.4mL / min, and 37°C. The weight average molecular weight is obtained by using a polystyrene standard sample with the same concentration as the sample as a benchmark.
[0150] (b) Polyamide-imide
[0151] As a polyamide-imide, there is no particular limitation as long as a transparent resin substrate can be obtained, and examples thereof include substances having the following first block and second block, wherein the first block includes a structural unit from a dianhydride and a structural unit from a diamine, and the second block includes a structural unit from an aromatic dicarbonyl compound and a structural unit from an aromatic diamine. In the above-mentioned polyamide-imide, the above-mentioned dianhydride may include, for example, biphenyltetracarboxylic dianhydride (BPDA) and 2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA). In addition, the above-mentioned diamine may include bistrifluoromethylbenzidine (TFDB). That is, the above-mentioned polyamide-imide has a structure in which a polyamide-imide precursor having the following first block and second block is imidized, and the first block is formed by copolymerizing a monomer containing a dianhydride and a diamine, and the second block is formed by copolymerizing a monomer containing an aromatic dicarbonyl compound and an aromatic diamine.
[0152] The polyamide-imide has a first block including an imide bond and a second block including an amide bond, so that not only optical properties but also thermal properties and mechanical properties are excellent. In particular, by using bistrifluoromethylbenzidine (TFDB) as a diamine forming the first block, thermal stability and optical properties can be improved. In addition, by using 2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA) and biphenyltetracarboxylic dianhydride (BPDA) as dianhydrides forming the first block, birefringence can be improved and heat resistance can be ensured.
[0153] The dianhydride forming the first block includes two dianhydrides, namely 6FDA and BPDA. In the first block, the polymer to which TFDB and 6FDA are bonded and the polymer to which TFDB and BPDA are bonded may be separately contained based on different repeating units, or may be arranged regularly in the same repeating unit, or may be contained in a completely random arrangement.
[0154] The monomers forming the first block preferably contain BPDA and 6FDA as dianhydrides at a molar ratio of 1:3 to 3:1. This is because optical properties can be ensured while reduction in mechanical properties and heat resistance can be suppressed, thereby achieving excellent birefringence.
[0155] The molar ratio of the first block to the second block is preferably 5:1 to 1:1. When the content of the second block is significantly low, the improvement effect of the thermal stability and mechanical properties brought by the second block cannot be fully obtained. In addition, when the content of the second block is further higher than the content of the first block, the thermal stability and mechanical properties can be improved, but sometimes the optical properties such as yellowness and transmittance are reduced, and the birefringence characteristics are also improved. It should be noted that the first block and the second block can be random copolymers or block copolymers. The repeating unit of the block is not particularly limited.
[0156] Examples of the aromatic dicarbonyl compound forming the second block include at least one selected from the group consisting of p-Terephthaloyl chloride (TPC), terephthalic acid (Terephthalic acid), isophthaloyl dichloride (Iso-phthaloyl dichloride) and 4,4'-benzoyl chloride (4,4'-benzoyl chloride). Preferably, it may be at least one selected from p-Terephthaloyl chloride (TPC) and isophthaloyl dichloride (Iso-phthaloyl dichloride).
[0157] Examples of the diamine forming the second block include 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane (HFBAPP), bis(4-(4-aminophenoxy)phenyl)sulfone (BAPS), bis(4-(3-aminophenoxy)phenyl)sulfone (BAPSM), 4,4'-diaminodiphenylsulfone (4DDS), 3,3'-diaminodiphenylsulfone (3DDS), 2,2-bis(4-(4-aminophenoxy)phenylpropane (BAPP), 4,4'-diaminodiphenylpropane (6HDA), 1,3-bis(4-aminophenoxy)benzene (134A) and 1,3-bis(4-aminophenoxy)phenylsulfone (134B). PB), 1,3-bis(3-aminophenoxy)benzene (133APB), 1,4-bis(4-aminophenoxy)biphenyl (BAPB), 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl (6FAPBP), 3,3-diamino-4,4-dihydroxydiphenyl sulfone (DABS), 2,2-bis(3-amino-4-hydroxyoxyphenyl)propane (BAP), 4,4'-diaminodiphenylmethane (DDM), 4,4'-oxydiphenylamine (4-ODA) and 3,3'-oxydiphenylamine (3-ODA).
[0158] In the case of using an aromatic dicarbonyl compound, high thermal stability and mechanical properties are easily achieved, but due to the benzene ring in the molecular structure, high birefringence is sometimes shown. Therefore, in order to suppress the reduction of birefringence caused by the second block, diamines preferably use diamines with soft groups introduced into the molecular structure. Specifically, diamines are more preferably selected from bis (4- (3-aminophenoxy) phenyl) sulfone (BAPSM), 4,4'-diaminodiphenyl sulfone (4DDS) and 2,2-bis (4- (4-aminophenoxy) phenyl) hexafluoropropane (HFBAPP) One or more diamines. In particular, the longer the length of the soft group is like BAPSM and the position of the substituent is in the meta position of the diamine, the more excellent birefringence can be shown.
[0159] The polyamide-imide precursor including the following first block and second block in its molecular structure has a weight average molecular weight of, for example, preferably 200,000 to 215,000 as measured by GPC, and a viscosity of, for example, preferably 2400 poise to 2600 poise, wherein the first block is copolymerized with a dianhydride including biphenyltetracarboxylic dianhydride (BPDA) and 2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA) and a diamine including bistrifluoromethylbenzidine (TFDB), and the second block is copolymerized with an aromatic dicarbonyl compound and an aromatic diamine.
[0160] Polyamideimide can be obtained by imidizing a polyamideimide precursor. In addition, polyamideimide can be used to obtain a polyamideimide film. Regarding the method of imidizing a polyamideimide precursor and the method for producing a polyamideimide film, for example, reference can be made to Japanese Patent Table No. 2018-506611.
[0161] (2) Glass substrate
[0162] The glass constituting the glass substrate is not particularly limited as long as it has transparency, and examples thereof include silicate glass and silica glass. Among them, borosilicate glass, aluminosilicate glass, and aluminoborosilicate glass are preferred, and alkali-free glass is more preferred. Commercially available products of the glass substrate include, for example, the ultra-thin plate glass G-Leaf of Nippon Electric Glass Co., Ltd. and the ultra-thin film glass of Matsunami Glass Industries Co., Ltd.
[0163] In addition, the glass constituting the glass substrate is also preferably chemically strengthened glass. Chemically strengthened glass is excellent in mechanical strength and can be thinned accordingly, and is therefore preferred from this point of view. Chemically strengthened glass is typically glass in which the mechanical properties are enhanced by chemical methods by partially exchanging ion species such as sodium for potassium near the surface of the glass, and has a compressive stress layer on the surface.
[0164] Examples of the glass constituting the chemically strengthened glass substrate include aluminosilicate glass, soda-lime glass, borosilicate glass, lead glass, alkali barium glass, and aluminoborosilicate glass.
[0165] Examples of commercially available chemically strengthened glass substrates include Gorilla Glass from Corning and Dragontrail from AGC.
[0166] As the substrate layer, among the above, a polyimide-based resin substrate containing a polyimide-based resin or a glass substrate is preferred because the substrate layer can be made to have bending resistance and excellent hardness and transparency.
[0167] (3) Composition of base material layer
[0168] The thickness of the substrate layer is not particularly limited as long as it is a thickness that allows flexibility, and can be appropriately selected depending on the type of the substrate layer and the like.
[0169] The thickness of the resin substrate is preferably, for example, 10 μm to 100 μm, more preferably 25 μm to 80 μm. By making the thickness of the resin substrate within the above range, good flexibility can be obtained while sufficient hardness can be obtained. In addition, the curling of the laminate for the flexible display device can be suppressed. In addition, it is preferred in terms of lightweighting of the laminate for the flexible display device.
[0170] The thickness of the glass substrate is, for example, preferably 200 μm or less, more preferably 15 μm or more and 100 μm or less, further preferably 20 μm or more and 90 μm or less, and particularly preferably 25 μm or more and 80 μm or less. By making the thickness of the glass substrate within the above range, good flexibility can be obtained while sufficient hardness can be obtained. In addition, the curling of the laminate for a flexible display device can be suppressed. In addition, it is preferred in terms of lightweighting of the laminate for a flexible display device.
[0171] 4. Functional layer
[0172] The laminate for a flexible display device in the present invention may have a functional layer on the surface side of the antistatic layer of the substrate layer. Examples of the functional layer include a hard coat layer, an antireflection layer, an antiglare layer, an antiscattering layer, an antifouling layer, and a primer layer.
[0173] In addition, the functional layer may be a single layer or a plurality of layers. In addition, the functional layer may be a layer having a single function or a plurality of layers having mutually different functions.
[0174] As for the configuration of the functional layer, there is no particular limitation as long as the functional layer is configured on the surface side of the antistatic layer of the substrate layer. For example, it can be configured between the substrate layer and the antistatic layer, or it can be configured on the surface side of the antistatic layer opposite to the substrate layer. Among them, the functional layer is preferably configured between the substrate layer and the antistatic layer, that is, the antistatic layer is configured on the outermost surface.
[0175] Hereinafter, a hard coat layer will be exemplified as a functional layer.
[0176] (1) Hard coating
[0177] The laminate for a flexible display device in the present invention can have a hard coating layer on the surface side of the antistatic layer of the substrate layer. The hard coating layer is a component for improving the surface hardness. By configuring the hard coating layer, the scratch resistance can be improved. In particular, when the substrate layer is a resin substrate, the scratch resistance can be effectively improved by configuring the hard coating layer.
[0178] The arrangement of the hard coating layer is not particularly limited as long as the hard coating layer is arranged on the surface side of the antistatic layer of the substrate layer. Figure 4As shown, the hard coating layer 4 is disposed between the substrate layer 2 and the antistatic layer 3, and may also be Figure 5 As shown, the hard coating layer 4 is arranged on the surface side of the antistatic layer 3 opposite to the substrate layer 2. Among them, the hard coating layer is preferably arranged between the substrate layer and the antistatic layer, that is, the antistatic layer is arranged on the outermost surface.
[0179] As the material of the hard coat layer, for example, an organic material, an inorganic material, an organic-inorganic composite material, or the like can be used.
[0180] Among them, the material of the hard coat is preferably an organic material. Specifically, the hard coat preferably comprises a cured product of a resin composition containing a polymerizable compound. The cured product of the resin composition containing a polymerizable compound can be obtained by using a polymerization initiator as needed to polymerize the polymerizable compound using a known method.
[0181] The polymerizable compound has at least one polymerizable functional group in the molecule. As the polymerizable compound, for example, at least one of a radical polymerizable compound and a cation polymerizable compound can be used.
[0182] A free radical polymerizable compound refers to a compound having a free radical polymerizable group. The free radical polymerizable group possessed by the free radical polymerizable compound is not particularly limited as long as it is a functional group capable of undergoing free radical polymerization reaction, and examples thereof include groups containing carbon-carbon unsaturated double bonds, and specifically, vinyl, (meth) acryloyl, etc. It should be noted that when the free radical polymerizable compound has two or more free radical polymerizable groups, these free radical polymerizable groups may be the same or different.
[0183] From the viewpoint of increasing the hardness of the hard coat layer, the number of radically polymerizable groups contained in one molecule of the radically polymerizable compound is preferably 2 or more, more preferably 3 or more.
[0184] As a free radical polymerizable compound, from the aspect of high reactivity, a compound having a (meth) acryloyl group is preferred. For example, polyfunctional (meth) acrylate monomers and oligomers having a molecular weight of several hundred to several thousand and having several (meth) acryloyl groups in the molecule such as urethane (meth) acrylate, polyester (meth) acrylate, epoxy (meth) acrylate, melamine (meth) acrylate, polyfluoroalkyl (meth) acrylate, silicone (meth) acrylate, etc. can be preferably used. In addition, polyfunctional (meth) acrylate polymers having two or more (meth) acryloyl groups in the side chain of the acrylate polymer can also be preferably used. Among them, polyfunctional (meth) acrylate monomers having two or more (meth) acryloyl groups in one molecule can be preferably used. By making the hard coat layer contain a cured product of a polyfunctional (meth) acrylate monomer, the hardness of the hard coat layer can be increased, and then the adhesion can be improved. In addition, polyfunctional (meth) acrylate oligomers or polymers having two or more (meth) acryloyl groups in one molecule can also be preferably used. By making the hard coat layer contain the cured product of the polyfunctional (meth)acrylate oligomer or polymer, the hardness and bending resistance of the hard coat layer can be improved, and the adhesion can be improved.
[0185] In addition, in this specification, (meth)acryloyl group represents an acryloyl group and a methacryloyl group, respectively, and (meth)acrylate represents an acrylate and a methacrylate, respectively.
[0186] About the specific example of multifunctional (meth) acrylate monomer, for example, the material described in Japanese Patent Publication No. 2019-132930 can be cited.Wherein, from the aspect of high reactivity, the hardness of hard coating layer is improved and the aspect of close adhesion, preferably 1 molecule has 3 or more and 6 or less (meth) acryloyl groups, for example, pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), trimethylolpropane tri (meth) acrylate, tripentaerythritol eight (meth) acrylate, four pentaerythritol ten (meth) acrylate, etc., particularly preferably selected from pentaerythritol tri (meth) acrylate, dipentaerythritol five (meth) acrylate and dipentaerythritol six acrylate and PO, EO or caprolactone etc. are modified and obtained by at least one of the substances.
[0187] In order to adjust hardness or viscosity, improve adhesion, etc., the resin composition may contain a monofunctional (meth) acrylate monomer as a radical polymerizable compound. Specific examples of monofunctional (meth) acrylate monomers include, for example, those described in Japanese Patent Application Laid-Open No. 2019-132930.
[0188] Cationic polymerizable compounds refer to compounds having cationic polymerizable groups. As the cationic polymerizable groups possessed by the cationic polymerizable compounds, as long as they are functional groups capable of cationic polymerization, there is no particular limitation, and examples thereof include epoxy groups, oxetane groups, vinyl ether groups, etc. It should be noted that when the cationic polymerizable compounds have two or more cationic polymerizable groups, these cationic polymerizable groups may be the same or different.
[0189] From the viewpoint of increasing the hardness of the hard coat layer, the number of cationically polymerizable groups contained in one molecule of the cationically polymerizable compound is preferably 2 or more, more preferably 3 or more.
[0190] In addition, as a cationic polymerizable compound, a compound having at least one of an epoxy group and an oxetane group as a cationic polymerizable group is preferred, and a compound having at least one of two epoxy groups and an oxetane group in one molecule is more preferred. From the aspect of the small shrinkage associated with the polymerization reaction, cyclic ether groups such as epoxy groups and oxetane groups are preferred. In addition, compounds having epoxy groups in cyclic ether groups have the following advantages: it is easy to obtain compounds with diverse structures, it will not adversely affect the durability of the obtained hard coating, and the compatibility with free radical polymerizable compounds is also easy to control. In addition, the oxetane group in the cyclic ether group has the following advantages: compared with epoxy groups, the polymerization degree is high and the toxicity is low. When the obtained hard coating is combined with a compound having an epoxy group, the speed of forming a network structure obtained by the cationic polymerizable compound in the coating film can be accelerated. Even in the area mixed with the free radical polymerizable compound, unreacted monomers will not remain in the film, and an independent network structure can be formed.
[0191] Examples of the cationically polymerizable compound having an epoxy group include, for example, polyglycidyl ethers of polyols having an alicyclic ring, or alicyclic epoxy resins obtained by epoxidizing a compound containing a cyclohexene ring or a cyclopentene ring using an appropriate oxidizing agent such as hydrogen peroxide or a peracid; aliphatic epoxy resins such as polyglycidyl ethers of aliphatic polyols or alkylene oxide adducts thereof, polyglycidyl esters of aliphatic long-chain polyacids, and homopolymers and copolymers of glycidyl (meth)acrylate; glycidyl ethers produced by the reaction of bisphenols such as bisphenol A, bisphenol F, hydrogenated bisphenol A, or their derivatives such as alkylene oxide adducts and caprolactone adducts with epichlorohydrin; and glycidyl ether-type epoxy resins derived from bisphenols such as novolac epoxy resins.
[0192] Specific examples of alicyclic epoxy resins, glycidyl ether epoxy resins, and cationically polymerizable compounds having an oxetane group include those described in JP-A-2018-104682.
[0193] The above-mentioned resin combination may also contain a polymerization initiator as required. As the polymerization initiator, free radical polymerization initiator, cationic polymerization initiator, free radical and cationic polymerization initiator etc. may be appropriately selected for use. These polymerization initiators are decomposed by at least one of light irradiation and heating, and free radicals or cations are generated to allow free radical polymerization and cationic polymerization to proceed. It should be noted that, in the hard coat, the polymerization initiator is sometimes completely decomposed and does not remain.
[0194] The hard coat layer may further contain additives as required. The additives are appropriately selected according to the functions imparted to the hard coat layer, are not particularly limited, and include, for example, inorganic particles, organic particles, ultraviolet absorbers, infrared absorbers, antifouling agents, antiglare agents, antistatic agents, leveling agents, surfactants, lubricants, various sensitizers, flame retardants, tackifiers, polymerization inhibitors, antioxidants, light stabilizers, surface modifiers, etc.
[0195] The thickness of the hard coat layer can be appropriately selected according to the function of the hard coat layer and the purpose of the laminate for a flexible display device. The thickness of the hard coat layer is preferably 0.5 μm to 50 μm, more preferably 1.0 μm to 40 μm, further preferably 1.5 μm to 30 μm, and particularly preferably 2 μm to 20 μm. If the thickness of the hard coat layer is within the above range, a hardness sufficient for the hard coat layer can be obtained.
[0196] Examples of a method for forming the hard coat layer include a method of applying a hard coat layer composition containing the polymerizable compound and the like onto the substrate layer or the antistatic layer and curing the composition.
[0197] 5. Impact absorbing layer
[0198] The laminate for a flexible display device in the present invention may have an impact absorbing layer on the surface side of the substrate layer opposite to the antistatic layer, or between the substrate layer and the antistatic layer. By configuring the impact absorbing layer, when an impact is applied to the laminate for a flexible display device, the impact can be absorbed, and the impact resistance can be improved. In addition, when the substrate layer is a glass substrate, cracks in the glass substrate can be suppressed.
[0199] The material of the impact absorbing layer is not particularly limited as long as a shock absorbing layer having impact absorbency and transparency can be obtained, and examples thereof include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), urethane resin, epoxy resin, polyimide, polyamide-imide, acrylic resin, triacetyl cellulose (TAC), silicone resin, etc. These materials may be used alone or in combination of two or more.
[0200] The impact absorbing layer may further contain additives as necessary. Examples of the additives include inorganic particles, organic particles, ultraviolet absorbers, antioxidants, light stabilizers, surfactants, and adhesion improvers.
[0201] The impact absorbing layer may be disposed on the side of the substrate layer opposite to the antistatic layer, or may be disposed between the substrate layer and the antistatic layer.
[0202] The thickness of the impact absorbing layer may be a thickness capable of absorbing impact, and is, for example, preferably 5 μm to 150 μm, more preferably 10 μm to 120 μm, and still more preferably 15 μm to 100 μm.
[0203] As the impact absorbing layer, for example, a resin film can be used. Alternatively, for example, the impact absorbing layer can be formed by coating a composition for an impact absorbing layer on the above-mentioned base layer.
[0204] 6. Adhesive layer for attachment
[0205] For example Figure 6 As shown, the laminate for a flexible display device in the present invention can have an adhesive layer 6 for sticking on the surface of the substrate layer 2 opposite to the antistatic layer 3. The laminate for a flexible display device can be stuck to, for example, a display panel via the adhesive layer for sticking.
[0206] The adhesive used for the adhesive layer for attaching is not particularly limited as long as it is transparent and can adhere the laminate for the flexible display device to the display panel, etc., and examples thereof include thermosetting adhesives, ultraviolet curing adhesives, two-liquid curing adhesives, hot melt adhesives, pressure-sensitive adhesives (so-called adhesives), etc.
[0207] As the pressure-sensitive adhesive used for the pressure-sensitive adhesive layer, for example, acrylic adhesives, silicone adhesives, rubber adhesives, urethane adhesives, etc. can be cited, and can be appropriately selected according to the material of the above-mentioned impact absorbing layer, etc. Among them, acrylic adhesives are preferred because they are excellent in transparency, weather resistance, durability, and heat resistance, and are low in cost.
[0208] The thickness of the adhesive layer for attachment is preferably, for example, from 10 μm to 100 μm, more preferably from 25 μm to 80 μm, and further preferably from 40 μm to 60 μm. If the thickness of the adhesive layer for attachment is too thin, it may not be possible to fully bond the laminate for the flexible display device to the display panel, etc. In addition, in the case where the adhesive layer for attachment is a pressure-sensitive adhesive layer, if the thickness of the adhesive layer for attachment is too thin, when an impact is applied to the laminate for the flexible display device, the effect of easily deforming the impact absorbing layer may not be fully obtained. On the other hand, if the thickness of the adhesive layer for attachment is too thick, the flexibility may sometimes be impaired.
[0209] As the adhesive layer for sticking, for example, an adhesive film can be used. Alternatively, for example, an adhesive composition can be applied on a support or a base material layer to form the adhesive layer for sticking.
[0210] 7. Interlayer bonding layer
[0211] In the laminate for a flexible display device of the present invention, an interlayer adhesive layer may be disposed between the layers.
[0212] The adhesive used in the interlayer adhesive layer may be the same as the adhesive used in the above-mentioned adhesive layer for sticking.
[0213] Among them, as described above, when an impact absorbing layer is arranged on the surface side of the substrate layer opposite to the antistatic layer, and an adhesive layer for sticking is arranged on the surface side of the impact absorbing layer opposite to the substrate layer and an interlayer adhesive layer is arranged between the substrate layer and the impact absorbing layer, the adhesive layer for sticking and the interlayer adhesive layer preferably contain a pressure-sensitive adhesive, that is, they are preferably pressure-sensitive adhesive layers.
[0214] The pressure-sensitive adhesive layer may be the same as the pressure-sensitive adhesive layer used for the above-mentioned adhesive layer for sticking.
[0215] The thickness, formation method, etc. of the interlayer adhesive layer may be the same as the thickness, formation method, etc. of the above-mentioned adhesive layer for bonding.
[0216] 8. Application of laminates for flexible display devices
[0217] The laminate for a flexible display device in the present invention can be used as a front panel disposed closer to the observer side than the display panel in the flexible display device. The laminate for a flexible display device in the present invention can be preferably used as a front panel in a flexible display device such as a foldable display, a rollable display, a bendable display, etc., because it can improve the wear resistance of the bent portion, and can be more preferably used as a front panel in a foldable display.
[0218] In addition, the laminate for a flexible display device in the present invention can be used as a front panel in display devices such as smartphones, tablet terminals, wearable terminals, personal computers, televisions, digital signage, public information displays (PIDs), and car displays.
[0219] B. Laminate for display device
[0220] The display device laminate of the present invention is a display device laminate having a substrate layer and an antistatic layer, wherein the surface resistance of the surface of the display device laminate on the antistatic layer side is 9×10 13 Ω / □ or less. After a rubber test was performed on the surface of the antistatic layer side of the display device laminate using a 6 mm diameter rubber with a load of 9.8 N and rubbing back and forth 2500 times, the surface resistance of the surface of the antistatic layer side of the display device laminate was 9×10 13 Ω / □ or less.
[0221] The details of the display device laminate in the present invention may be the same as those of the flexible display device laminate described above, and thus the description thereof will be omitted here.
[0222] C. Flexible display device
[0223] The flexible display device in the present invention includes a display panel and the flexible display device laminate disposed on the viewer side of the display panel.
[0224] Figure 7 is a schematic cross-sectional view showing an example of a flexible display device in the present invention. Figure 7 As shown, the flexible display device 20 includes a display panel 21 and a flexible display device laminate 1 disposed on the viewer side of the display panel 21. In the flexible display device 20, the flexible display device laminate 1 and the display panel 21 can be bonded together by, for example, an adhesive layer 6 of the flexible display device laminate 1.
[0225] When the laminate for a flexible display device in the present invention is disposed on the surface of a flexible display device, it is preferably disposed so that the antistatic layer is on the outside and the base material layer is on the inside.
[0226] The method of disposing the laminate for a flexible display device in the present invention on the surface of the flexible display device is not particularly limited, and examples thereof include a method using an adhesive layer.
[0227] Examples of the display panel in the present invention include display panels used in display devices such as organic EL display devices and liquid crystal display devices.
[0228] The flexible display device in the present invention can include a touch panel member between the display panel and the laminate for the flexible display device.
[0229] The flexible display device in the present invention is preferably foldable, that is, the flexible display device in the present invention is preferably a foldable display.
[0230] It should be noted that the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative only, and any other embodiments having substantially the same configuration as the technical concept described in the claims of the present invention and having the same effects are included in the technical scope of the present invention.
[0231] Example
[0232] Hereinafter, the present invention will be further described with reference to Examples and Comparative Examples.
[0233] [Example 1]
[0234] First, each component was mixed so as to have the composition shown below to obtain a composition 1 for an antistatic layer.
[0235] (Composition of Antistatic Layer Composition 1)
[0236] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0237] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0238] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0239] Antistatic agent (photocurable resin composition containing PEDOT, product name "BEAMSET MT-2", manufactured by Arakawa Chemical Industries, Ltd.): 5 parts by mass (based on 100% solid content)
[0240] Methyl isobutyl ketone: 250 parts by mass
[0241] Next, a polyimide resin substrate (product name "Neopulim", manufactured by Mitsubishi Gas Chemical Co., Ltd.) with a thickness of 50 μm was prepared as a substrate layer, and the antistatic layer composition 1 was applied by a rod coater to form a coating film. In addition, the coating film was heated at 70° C. for 1 minute to evaporate the solvent in the coating film, and an ultraviolet irradiation device (manufactured by Fusion UV Systems Japan, light source H bulb) was used to irradiate the coating film at an oxygen concentration of 200 ppm or less and a cumulative light intensity of 380 mJ / cm 2 The coating film was cured by irradiating ultraviolet rays in a manner of 10 μm to form an antistatic layer having a film thickness of 10 μm. In this way, a laminate having a substrate layer and an antistatic layer was obtained.
[0242] [Example 2]
[0243] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 2 was used.
[0244] (Composition of Antistatic Layer Composition 2)
[0245] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0246] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0247] Antistatic agent (Li salt-containing photocurable resin composition, product name "BEAMSET 1604", manufactured by Arakawa Industries, Ltd.): 100 parts by mass (solid content 100% conversion value)
[0248] Methyl isobutyl ketone: 240 parts by mass
[0249] [Example 3]
[0250] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 3 was used.
[0251] (Composition of Antistatic Layer Composition 3)
[0252] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0253] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0254] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0255] Antistatic agent (quaternary ammonium salt-containing polymer antistatic agent, product name "1SX-1090", manufactured by Taisei Fine Chemical Co., Ltd.): 20 parts by mass (solid content 100% conversion value)
[0256] Methyl isobutyl ketone: 290 parts by mass
[0257] [Example 4]
[0258] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 4 was used.
[0259] (Composition of Antistatic Layer Composition 4)
[0260] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0261] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0262] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0263] Antistatic agent (photocurable resin composition containing PEDOT, product name "BEAMSET MT-2", manufactured by Arakawa Chemical Industries, Ltd.): 4 parts by mass (solid content 100%)
[0264] Methyl isobutyl ketone: 250 parts by mass
[0265] [Example 5]
[0266] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 5 was used.
[0267] (Composition of Antistatic Layer Composition 5)
[0268] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0269] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0270] Antistatic agent (Li salt-containing photocurable resin composition, product name "BEAMSET 1604", manufactured by Arakawa Industries, Ltd.): 75 parts by mass (solid content 100% conversion value)
[0271] Methyl isobutyl ketone: 240 parts by mass
[0272] [Example 6]
[0273] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 6 was used.
[0274] (Composition of Antistatic Layer Composition 6)
[0275] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0276] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0277] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0278] Antistatic agent (quaternary ammonium salt-containing polymer antistatic agent, product name "1SX-1090", manufactured by Taisei Fine Chemical Co., Ltd.): 10 parts by mass (solid content 100% conversion value)
[0279] Methyl isobutyl ketone: 290 parts by mass
[0280] [Example 7]
[0281] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 7 was used.
[0282] (Composition of Antistatic Layer Composition 7)
[0283] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0284] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0285] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0286] Antistatic agent (ATO particle dispersion, product name "ELECOM V-3560", manufactured by JGC Catalysts & Chemicals Co., Ltd.): 15 parts by mass (based on 100% solid content)
[0287] Methyl isobutyl ketone: 280 parts by mass
[0288] [Comparative Example 1]
[0289] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 8 was used.
[0290] (Composition of Antistatic Layer Composition 8)
[0291] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0292] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0293] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0294] Antistatic agent (photocurable resin composition containing PEDOT, product name "BEAMSET MT-2", manufactured by Arakawa Chemical Industries, Ltd.): 2.5 parts by mass (based on 100% solid content)
[0295] Methyl isobutyl ketone: 250 parts by mass
[0296] [Comparative Example 2]
[0297] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 9 was used.
[0298] (Composition of Antistatic Layer Composition 9)
[0299] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0300] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0301] Antistatic agent (Li salt-containing photocurable resin composition, product name "BEAMSET 1604", manufactured by Arakawa Industries, Ltd.): 30 parts by mass (solid content 100% conversion value)
[0302] Methyl isobutyl ketone: 240 parts by mass
[0303] [Comparative Example 3]
[0304] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 10 was used.
[0305] (Composition of the antistatic layer composition 10)
[0306] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0307] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0308] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0309] Antistatic agent (quaternary ammonium salt-containing polymer antistatic agent, product name "1SX-1090", manufactured by Taisei Fine Chemical Co., Ltd.): 4 parts by mass (solid content 100% conversion value)
[0310] Methyl isobutyl ketone: 290 parts by mass
[0311] [Comparative Example 4]
[0312] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 11 was used.
[0313] (Composition of Antistatic Layer Composition 11)
[0314] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0315] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0316] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0317] Antistatic agent (ATO particle dispersion, product name "ELECOM V-3560", manufactured by JGC Catalysts & Chemicals Co., Ltd.): 10 parts by mass (based on 100% solid content)
[0318] Methyl isobutyl ketone: 280 parts by mass
[0319] [Comparative Example 5]
[0320] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 12 was used.
[0321] (Composition of Antistatic Layer Composition 12)
[0322] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0323] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0324] Antifouling agent (product name "BYK-UV3510", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0325] Methyl isobutyl ketone: 240 parts by mass
[0326] [Comparative Example 6]
[0327] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 13 was used.
[0328] (Composition of Antistatic Layer Composition 13)
[0329] Urethane acrylate (product name "UV-7650B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0330] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0331] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0332] Methyl isobutyl ketone: 240 parts by mass
[0333] [Comparative Example 7]
[0334] A laminate was produced in the same manner as in Example 1 except that the following antistatic layer composition 14 was used.
[0335] (Composition of Antistatic Layer Composition 14)
[0336] Urethane acrylate (product name "UV-7600B", manufactured by Mitsubishi Chemical Corporation): 100 parts by mass (solid content 100% conversion value)
[0337] Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, product name "Omnirad 184", manufactured by IGM Resins BV): 4 parts by mass
[0338] Antifouling agent (product name "BYK-UV3500", manufactured by BYK Chemical Japan Ltd.): 0.5 parts by mass (based on 100% solid content)
[0339] Methyl isobutyl ketone: 240 parts by mass
[0340] [evaluate]
[0341] (1) Surface resistance before and after rubber test
[0342] The following rubber test was performed on the antistatic layer side surface of the laminates of Examples and Comparative Examples, and the surface resistance of the antistatic layer side surface of the laminates before and after the rubber test was measured.
[0343] In the rubber test, first, prepare a laminate of 15cm×10cm in size. Then, perform a rubber test on the surface of the antistatic layer side of the laminate. Specifically, use a rubber with a diameter of 6mm manufactured by Minoan, insert a fixture with a hole of 6mm in diameter in such a way that the front end of the rubber is exposed by 4mm, and install the fixture with the rubber to a Gakushin type friction fastness tester (product name "AB-301", manufactured by TESTER SANGYO), and use the rubber to rub the surface of the antistatic layer side of the above-mentioned laminate back and forth 2500 times with a load of 9.8N, a moving speed of 80mm / second and a moving distance of 40mm.
[0344] Next, the surface resistance of the rubber test implementation part and the rubber test non-implementation part on the surface of the antistatic layer side of the above-mentioned laminate is measured. When measuring the surface resistance, the laminate is left to stand for 1 hour under an environment of temperature 23±2°C and humidity 50±10% before measurement. Regarding the surface resistance, a resistivity meter (Hiresta UX MCP-HT type manufactured by Mitsubishi Chemical Analytech) is used, and the MCP-HTO14 URS probe is used in the rubber test implementation part, and the MCP-HTP11 UA probe is used in the rubber test non-implementation part, and the voltage is applied to measure 1000V. Regarding the surface resistance, the surface resistance of the rubber test implementation part and the rubber test non-implementation part of the surface of the antistatic layer side of the above-mentioned laminate is measured at 10 locations respectively, and the arithmetic average of the measured values at 10 locations is obtained.
[0345] (2) Sliding properties before and after the rubber test
[0346] The following rubber test was performed on the antistatic layer side surface of the laminates of Examples and Comparative Examples, and the sliding properties of the antistatic layer side surface of the laminates before and after the rubber test were evaluated.
[0347] The rubber test was performed in the same manner as above.
[0348] Next, the sliding properties of the rubber test-implemented portion and the rubber test-unimplemented portion on the antistatic layer side of the laminate were evaluated. Specifically, the rubber test-unimplemented portion, the rubber test-implemented portion, and the rubber test-unimplemented portion were rubbed with fingertips at a moving speed of 10 cm / sec in sequence, and the sliding properties of the rubber test-implemented portion at this time were evaluated according to the following criteria.
[0349] A: More than 7 out of 10 people did not feel hung
[0350] B: 5 or 6 out of 10 people did not feel hung
[0351] C: 6 or 7 out of 10 people feel hung up
[0352] D: More than 8 out of 10 people feel anxious
[0353] (3) Friction before and after the rubber test
[0354] The following rubber test was performed on the surface of the antistatic layer side of the laminate of the embodiment and the comparative example, and the friction force of the surface of the antistatic layer side of the laminate against the rubber was measured before and after the rubber test. First, the rubber test was performed in the same manner as described above. Next, the friction force of the rubber on the surface of the antistatic layer side of the laminate was measured for the rubber test implementation part and the rubber test non-implementation part. Specifically, a rubber with a diameter of 6 mm manufactured by minoan was used, and a clamp having a hole with a diameter of 6 mm was inserted in such a way that the front end of the rubber was exposed 4 mm. The clamp with the rubber was installed in a continuous load scratch strength tester (product name "TRIBOGEAR 18 type", manufactured by Shinto Scientific Co., Ltd.), and the rubber was used to rub the rubber test non-implementation part, the rubber test implementation part and the rubber test non-implementation part on the surface of the antistatic layer side of the laminate in turn with a load of 1.96 N and a moving speed of 840 mm / min to measure the friction force. At this time, if Figure 2 As shown in FIG. 1 , the rubber is moved perpendicularly to the long side direction of the rectangular rubber test implementation part 32 as shown by the arrow. Next, the maximum value of the friction force of the rubber test implementation part on the rubber is obtained. In addition, the friction force of the rubber test non-implemented part on the rubber is obtained as shown in FIG. Figure 2 As shown, when the point where the friction force of the rubber to the rubber in the rubber test implementation part 32 reaches the maximum value is set to 0 mm, it is the average value of the friction force in the range of 4.2 mm to 9.8 mm in the rubber test non-implemented part 31 with the above point (0 mm) as the reference.
[0355]
[0356] As shown in Table 1, the surface resistance before and after the rubber test is 9×10 13 Ω / □ or less (Examples 1 to 7), the sliding properties are all good, but the surface resistance before and after the rubber test exceeds 9×10 13 When Ω / □ (Comparative Examples 1 to 7), the evaluation of sliding property was poor.
[0357] When the ratio of the surface resistance after the rubber test to the surface resistance before the rubber test (initial surface resistance) exceeded 20.0 (Example 7), the sliding property was slightly inferior to that when the ratio was 20.0 or less.
[0358] Explanation of symbols
[0359] 1…Laminate for flexible display device
[0360] 2…Base material layer
[0361] 3…Antistatic layer
[0362] 4…Hard coating
[0363] 5…Shock absorbing layer
[0364] 6…Adhesive layer for attachment
[0365] 7…Interlayer bonding layer
[0366] 20…Flexible display device
[0367] 21…Display panel.
Claims
1. A laminate for a flexible display device, comprising a substrate layer and an antistatic layer, wherein: The surface resistance of the antistatic layer side of the laminate for a flexible display device is 1.3×10 12 Ω / □More than 9×10 13 Ω / □ or less, The surface of the antistatic layer side of the laminate for the flexible display device was subjected to a rubber test in which a load of 9.8 N was applied using a rubber with a diameter of 6 mm and the surface resistance of the surface of the antistatic layer side of the laminate for the flexible display device was 1.7×10 13 Ω / □ or less.
2. The laminate for a flexible display device according to claim 1, wherein: On the surface of the antistatic layer side of the laminate for a flexible display device, a ratio of the surface resistance after the rubber test to the initial surface resistance is 20.0 or less. 3 . The laminate for a flexible display device according to claim 1 , further comprising a functional layer on the surface of the base layer facing the antistatic layer.
4. The laminate for a flexible display device according to claim 1, wherein: The antistatic layer is disposed on the outermost surface.
5. The laminate for a flexible display device according to claim 1, wherein: An impact absorbing layer is provided on the surface side of the substrate layer opposite to the antistatic layer or between the substrate layer and the antistatic layer.
6. The laminate for a flexible display device according to claim 1, wherein: The substrate layer has an adhesive layer for sticking on the side opposite to the antistatic layer.
7. The laminate for a flexible display device according to claim 1, wherein: For the surface of the antistatic layer side of the laminate for the flexible display device, after a rubber test using an eraser with a diameter of 6 mm to apply a load of 9.8 N and rub back and forth 2500 times, the maximum friction force of the surface of the antistatic layer side of the laminate for the flexible display device against the rubber is greater than 0.98 N and less than 9.80 N.
8. The laminate for a flexible display device according to claim 7, wherein: The ratio of the maximum value of the friction force of the surface of the antistatic layer side of the laminate for a flexible display device with respect to the rubber after the rubber test to the average value of the initial friction force with respect to the rubber is 1.50 or less.
9. A laminate for a display device, comprising a substrate layer and an antistatic layer, wherein: The surface resistance of the surface of the display device laminate on the antistatic layer side is 1.3×10 12 Ω / □More than 9×10 13 Ω / □ or less, The surface of the display device laminate on the antistatic layer side was subjected to a rubber test in which a load of 9.8 N was applied using an eraser with a diameter of 6 mm and the surface resistance of the surface of the display device laminate on the antistatic layer side was 1.7×10 13 Ω / □ or less.
10. A flexible display device comprising: display panel; and The laminate for a flexible display device according to any one of claims 1 to 8, which is disposed on the viewer side of the display panel.