Post-treatment process of metal electrode of solar cell and preparation method of solar cell

Through light injection processing, hydrogen ions are activated and combined with double-sided laser sintering technology, the damage problem of laser film opening and hydrofluoric acid cleaning on solar cells is solved, the photoelectric conversion efficiency and battery life are improved, and more efficient solar cell performance is achieved.

CN118919601AInactive Publication Date: 2024-11-08DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD

Patent Information

Application Number
CN202411010562.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the use of laser film and hydrofluoric acid cleaning on the silicon substrate leads to a reduced photoelectric conversion efficiency of solar cells and a short battery life, and a poor bonding force between the metal electrode and the silicon substrate, resulting in an increase in series resistance.

Method used

The light injection process is used to activate hydrogen ions and migrate them to the crystalline silicon layer. Combined with the double-sided laser sintering technology, a tighter metal electrode is formed in contact with the silicon substrate, reducing contact resistance and enhancing binding force.

Benefits of technology

It improves the photoelectric conversion efficiency of solar cells, extends service life, and reduces contact resistance, providing a more efficient and reliable energy solution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a post-processing technology of a solar cell metal electrode and a preparation method of a solar cell, and particularly relates to the technical field of solar cell preparation. According to the post-processing technology of the solar cell metal electrode, light injection processing and double-face laser sintering are sequentially carried out on a solar cell with metal electrodes on the two faces. According to the post-processing technology of the solar cell metal electrode, hydrogen ions are activated through light injection processing and migrated into the crystalline silicon layer, interface passivation is achieved, and therefore the photoelectric conversion efficiency of a solar cell is improved. In addition, the double-sided laser sintering process is added after the light injection treatment, so that the metal electrode and the silicon substrate form closer contact, and the contact resistance is reduced. The laser sintering can also enhance the binding force between the metal electrode and the silicon substrate, and the service life of the solar cell is further prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cell preparation, and in particular to a post-processing process for a metal electrode of a solar cell and a method for preparing a solar cell. Background Art

[0002] As a non-contact electrode preparation technology, electroplating technology has excellent performance and can reduce costs. When preparing metal electrodes, it is usually necessary to first plate a layer of metal on the silicon surface as a diffusion barrier, and then deposit a conductive layer of metal and a protective layer of metal to form an electroplated solar cell.

[0003] At present, before electroplating the seed layer, it is necessary to remove part of the passivation layer through laser film opening to expose the silicon substrate before electroplating. The laser film opening process will generate high temperature and silicon will be easily oxidized, so it is necessary to clean the silicon substrate with hydrofluoric acid first. However, if the silicon substrate is in contact with hydrofluoric acid for too long, the silicon nitride passivation layer in other areas will be destroyed, resulting in a decrease in the photoelectric conversion efficiency of the battery. If the silicon substrate is in contact with hydrofluoric acid for a short time, the oxide layer will be difficult to remove cleanly, resulting in an increase in the series resistance of the electroplated battery and poor bonding between the entire metal grid line and the silicon substrate.

[0004] The damage to the silicon substrate caused by laser film opening and hydrofluoric acid cleaning will lead to an increase in the series resistance of the solar cells produced, a shortened battery life and a decrease in the photoelectric conversion efficiency.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] One of the purposes of the present invention is to provide a post-processing process for metal electrodes of solar cells, aiming to solve at least one of the above-mentioned technical problems in the prior art.

[0007] A second object of the present invention is to provide a method for preparing a solar cell.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A first aspect of the present invention provides a post-processing process for a metal electrode of a solar cell, comprising at least:

[0010] The solar cell with metal electrodes on both sides is subjected to light injection treatment and double-sided laser sintering in sequence.

[0011] Furthermore, the solar cell is a TOPCon solar cell.

[0012] Furthermore, the plating structure of the metal electrode includes a barrier layer, a conductive layer and a protective layer.

[0013] Preferably, the material of the barrier layer includes at least one of nickel, cobalt, titanium, tungsten and tantalum.

[0014] Preferably, the conductive layer is made of copper.

[0015] Preferably, the material of the protective layer is at least one of tin, silver and nickel.

[0016] Furthermore, the light injection process includes:

[0017] The solar cell with metal electrodes is passed through a light injection furnace at a uniform speed to perform the light injection treatment.

[0018] Furthermore, the light injection treatment is performed at a temperature of 100° C. to 160° C. and for a time of 60s to 180s.

[0019] Preferably, the light radiation intensity of the light injection treatment is 5 suns to 30 suns.

[0020] Preferably, the light source of the light injection treatment includes at least one of an infrared lamp, an LED lamp, a xenon lamp and a tungsten lamp.

[0021] Preferably, the light intensity of the light source for the light injection treatment is 1000 W / m 2 ~5000W / m 2 .

[0022] Furthermore, the laser sintering process includes:

[0023] Laser is used to irradiate the metal electrodes on the front and back of the solar cell respectively, and a forward bias is applied to the metal electrodes to achieve sintering of the metal electrodes.

[0024] Furthermore, a forward bias is applied to the metal electrode through an external power source.

[0025] Preferably, the forward bias voltage is 1.0V to 10.0V.

[0026] Furthermore, the type of the laser is picosecond pulse laser.

[0027] Preferably, the scanning speed of the picosecond pulse laser is 5 m / s to 20 m / s.

[0028] Preferably, the frequency of the laser is 100kHz to 500kHz, and the peak energy is 1.0J / cm 2 ~10.0J / cm 2 .

[0029] Preferably, the laser is in the shape of a point-shaped spot.

[0030] Preferably, the diameter of the point-shaped light spot is 20 μm to 60 μm.

[0031] Preferably, the wavelength of the laser is one of 532 nm, 755 nm, 980 nm, and 1064 nm.

[0032] Furthermore, the peak temperature of the sintering is 600°C to 800°C.

[0033] Preferably, the sintering time is 0.5s to 2s.

[0034] A second aspect of the present invention provides a method for preparing a solar cell, the method comprising the post-processing process of the metal electrode of the solar cell described in the first aspect.

[0035] Compared with the prior art, the present invention has at least the following beneficial effects:

[0036] The present invention provides a post-processing process for metal electrodes of solar cells, which activates hydrogen ions through light injection and causes them to migrate into the crystalline silicon layer, thereby achieving interface passivation and improving the photoelectric conversion efficiency of solar cells. In addition, the present invention adds a double-sided laser sintering process after the light injection process, so that the metal electrode and the silicon substrate form a closer contact and reduce the contact resistance. Laser sintering can also enhance the bonding force between the metal electrode and the silicon substrate, further improving the service life of the solar cell.

[0037] The method for preparing solar cells provided by the present invention, in view of the beneficial effects of the above-mentioned post-processing process, enables the obtained solar cells to have lower contact resistance, higher photoelectric conversion efficiency and longer service life, and can provide a more efficient and reliable energy solution for the field of solar power generation. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0039] Hereinafter, the terms "including", "having" and their cognates, which may be used in various embodiments of the present invention, are intended only to indicate specific features, numbers, steps, operations, elements, components or combinations of the foregoing items, and should not be understood as first excluding the existence of one or more other features, numbers, steps, operations, elements, components or combinations of the foregoing items or adding the possibility of one or more features, numbers, steps, operations, elements, components or combinations of the foregoing items.

[0040] A first aspect of the present invention provides a post-processing process for a metal electrode of a solar cell, comprising at least:

[0041] The solar cell with metal electrodes on both sides is subjected to light injection treatment and double-sided laser sintering in sequence.

[0042] The present invention provides a post-processing process for metal electrodes of solar cells, which activates hydrogen ions through light injection and causes them to migrate into the crystalline silicon layer, thereby achieving interface passivation and improving the photoelectric conversion efficiency of solar cells. In addition, the present invention adds a double-sided laser sintering process after the light injection process, so that the metal electrode and the silicon substrate form a closer contact and reduce the contact resistance. Laser sintering can also enhance the bonding force between the metal electrode and the silicon substrate, further improving the service life of the solar cell.

[0043] The principle of light injection treatment is to use an external light source to inject additional carriers (electrons and holes) into the silicon substrate, thereby changing the carrier distribution and concentration inside the silicon substrate, thereby affecting the electrical properties of the solar cell.

[0044] Furthermore, the solar cell is a TOPCon solar cell.

[0045] Furthermore, the plating structure of the metal electrode includes a barrier layer, a conductive layer and a protective layer.

[0046] Preferably, the material of the barrier layer includes at least one of nickel, cobalt, titanium, tungsten and tantalum.

[0047] Preferably, the conductive layer is made of copper.

[0048] Preferably, the material of the protective layer is at least one of tin, silver and nickel.

[0049] The present invention does not limit the thickness of the specific barrier layer, conductive layer and protective layer, and any thickness that can achieve electrode performance can be used.

[0050] Furthermore, the light injection process includes:

[0051] The solar cell with metal electrodes is passed through a light injection furnace at a uniform speed to perform the light injection treatment.

[0052] Furthermore, the light injection treatment is performed at a temperature of 100° C. to 160° C. and for a time of 60s to 180s.

[0053] Typically but not restrictively, the temperature of the light injection treatment can be, for example, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or 160°C, or any value in the range of 100°C to 160°C; the time of the light injection treatment can be, for example, 60s, 80s, 100s, 120s, 140s, 160s or 180s, or any value in the range of 60s to 180s.

[0054] Preferably, the light radiation intensity of the light injection treatment is 5 suns to 30 suns.

[0055] Typically, but not limiting, the illumination radiation intensity of the light injection treatment may be, for example, 5 suns, 6 suns, 7 suns, 8 suns, 9 suns, 10 suns, 11 suns, 12 suns, 13 suns, 14 suns,

[0056] 15suns, 16suns, 17suns, 18suns, 19suns, 20suns, 21suns, 22suns, 23suns, 24suns, 25suns, 26suns, 27suns, 28suns, 29suns or 30suns, or any value within the range of 5suns to 30suns.

[0057] Preferably, the light source of the light injection treatment includes at least one of an infrared lamp, an LED lamp, a xenon lamp and a tungsten lamp.

[0058] Preferably, the light intensity of the light source for the light injection treatment is 1000 W / m 2 ~5000W / m 2 .

[0059] Typically, but not limiting, the light intensity of the light source for light injection treatment may be, for example, 1000 W / m 2 、1500W / m 2 , 2000W / m 2 , 2500W / m 2 、3000W / m 2 、3500W / m 2 , 4000W / m 2 、4500W / m 2 or 5000W / m 2 , or 1000W / m 2 ~5000W / m 2 Any value in the range.

[0060] Furthermore, the laser sintering process includes:

[0061] Laser is used to irradiate the metal electrodes on the front and back of the solar cell respectively, and a forward bias is applied to the metal electrodes to achieve sintering of the metal electrodes.

[0062] Use laser to irradiate the metal electrodes on the front and back of the solar cell, and load forward bias on the metal electrodes to achieve sintering of the metal electrodes, so as to inject a large number of electron-hole pairs into the N-type battery, and form an electric field on the grid lines on the front and back surfaces of the N-type battery. This can significantly reduce the sintering time and sintering temperature required for the surface, expand the process window, effectively avoid damage to the battery surface, reduce metal recombination, and help reduce the contact resistivity of the metal grid line-silicon.

[0063] Furthermore, a forward bias is applied to the metal electrode through an external power source.

[0064] Preferably, the forward bias voltage is 1.0V to 10.0V.

[0065] Typically but not limiting, the forward bias voltage can be, for example, 1.0V, 1.5V, 2.0V, 2.5V, 3.0V, 3.5V, 4.0V, 4.5V, 5.0V, 5.5V, 6.0V, 6.5V, 7.0V, 7.5V, 8.0V, 8.5V, 9.0V or 10.0V, or any value in the range of 1.0V to 10.0V.

[0066] Furthermore, the type of the laser is picosecond pulse laser.

[0067] The pulse width of picosecond pulse laser is very short, which can provide very high peak power in a very short time, with higher precision and more controllable sintering range and process.

[0068] Preferably, the scanning speed of the picosecond pulse laser is 5 m / s to 20 m / s.

[0069] Typically but not limiting, the scanning speed of the picosecond pulse laser can be, for example, 5 m / s, 6 m / s, 7 m / s, 8 m / s, 9 m / s, 10 m / s, 11 m / s, 12 m / s, 13 m / s, 14 m / s, 15 m / s, 16 m / s, 17 m / s, 18 m / s or 20 m / s, or any value within the range of 5 m / s to 20 m / s.

[0070] Preferably, the frequency of the laser is 100kHz to 500kHz, and the peak energy is

[0071] 1.0J / cm 2 ~10.0J / cm 2 .

[0072] Typically but not limiting, the frequency of the laser may be, for example, 100 kHz, 150 kHz, 200 kHz, 250 kHz, 300 kHz, 350 kHz, 400 kHz or 500 kHz, or any value within the range of 100 kHz to 500 kHz. The peak energy of the laser may be, for example, 1.0 J / cm 2 , 2.0J / cm 2 , 3.0J / cm 2 , 4.0J / cm 2 , 5.0J / cm 2 、6.0J / cm 2 , 7.0J / cm 2 , 8.0J / cm 2 or 10.0J / cm 2 , or 1.0 J / cm 2 ~10.0J / cm 2 Any value in the range.

[0073] Preferably, the laser is in the shape of a point-shaped spot.

[0074] Preferably, the diameter of the point-shaped light spot is 20 μm to 60 μm.

[0075] Typically but not restrictively, the diameter of the point-shaped light spot may be, for example, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 50 μm or 60 μm, or any value within the range of 20 μm to 60 μm.

[0076] Preferably, the wavelength of the laser is one of 532 nm, 755 nm, 980 nm, and 1064 nm.

[0077] Furthermore, the peak temperature of the sintering is 600°C to 800°C.

[0078] Typically, but not limiting, the peak sintering temperature can be, for example, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C or 800°C, or any value within the range of 600°C to 800°C.

[0079] Preferably, the sintering time is 0.5s to 2s.

[0080] Typically but not limiting, the sintering time can be, for example, 0.5s, 0.6s, 0.7s, 0.8s, 0.9s, 1.0s, 1.1s, 1.2s, 1.3s, 1.4s, 1.5s, 1.6s, 1.7s, 1.8s, 1.9s or 2.0s, or any value within the range of 0.5s to 2s.

[0081] A second aspect of the present invention provides a method for preparing a solar cell, the method comprising the post-processing process of the metal electrode of the solar cell described in the first aspect.

[0082] The method for preparing solar cells provided by the present invention, in view of the beneficial effects of the above-mentioned post-processing process, enables the obtained solar cells to have lower contact resistance, higher photoelectric conversion efficiency and longer service life, and can provide a more efficient and reliable energy solution for the field of solar power generation.

[0083] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. The raw materials used in the examples and comparative examples of the present invention, if no specific conditions are specified, are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0084] Example 1

[0085] This embodiment provides a solar cell, and the specific steps are as follows:

[0086] 1. Laser-cut the silicon substrate to form a patterned groove, and then double-sided electroplating to form a metal electrode. The coating structure of the metal electrode is a barrier layer, a conductive layer, and a protective layer stacked in sequence.

[0087] Among them, the barrier layer is made of nickel with a thickness of 1 μm; the conductive layer is made of copper with a thickness of 9 μm; and the protective layer is made of tin with a thickness of 1 μm.

[0088] 2. Pass the double-sided electroplated solar cells through a light injection furnace at a uniform speed for light injection treatment.

[0089] The light source in the light injection furnace is a xenon lamp with a light radiation intensity of 20 suns and a light intensity of 2000 W / m 2 .

[0090] The temperature of the light injection treatment was 130°C and the time was 120s.

[0091] 3. Use picosecond pulse laser to sequentially irradiate the metal grid lines on the front and back of the double-sided electroplated solar cell after light injection treatment, and load a forward bias voltage on the metal grid lines of the double-sided electroplated solar cell through an external power supply to sinter the metal grid lines to obtain a solar cell.

[0092] The forward bias voltage is 5.0 V, the shape of the picosecond pulse laser is a point-shaped light plate with a diameter of 40 μm, the wavelength is 755 nm, the scanning speed is 10 m / s, the frequency is 300 kHz, and the peak energy is 5.0 J / cm 2 The sintering temperature at peak energy is 700°C; the sintering time is 1s.

[0093] Example 2

[0094] This embodiment provides a solar cell, and the specific steps are as follows:

[0095] 1. Same as the step in Example 1.

[0096] 2. Pass the double-sided electroplated solar cells through a light injection furnace at a uniform speed for light injection treatment.

[0097] The light source in the light injection furnace is a xenon lamp with a light radiation intensity of 10 suns and a light intensity of 3000 W / m 2 .

[0098] The temperature of the light injection treatment was 150°C and the time was 80s.

[0099] 3. Use picosecond pulse laser to sequentially irradiate the metal grid lines on the front and back of the double-sided electroplated solar cell after light injection treatment, and load a forward bias voltage on the metal grid lines of the double-sided electroplated solar cell through an external power supply to sinter the metal grid lines to obtain a solar cell.

[0100] The forward bias voltage is 8.0 V, the shape of the picosecond pulse laser is a point-shaped light plate with a diameter of 30 μm, the wavelength is 980 nm, the scanning speed is 15 m / s, the frequency is 300 kHz, and the peak energy is 8.0 J / cm 2 The sintering temperature at peak energy is 800°C; the sintering time is 0.5s.

[0101] Example 3

[0102] This embodiment provides a solar cell, and the specific steps are as follows:

[0103] 1. Same as the step in Example 1.

[0104] 2. Pass the double-sided electroplated solar cells through a light injection furnace at a uniform speed for light injection treatment.

[0105] The light source in the light injection furnace is a xenon lamp with a light radiation intensity of 15 suns and a light intensity of 4000 W / m 2 .

[0106] The temperature of the light injection treatment was 120°C and the time was 150s.

[0107] 3. Use picosecond pulse laser to sequentially irradiate the metal grid lines on the front and back of the double-sided electroplated solar cell after light injection treatment, and load a forward bias voltage on the metal grid lines of the double-sided electroplated solar cell through an external power supply to sinter the metal grid lines to obtain a solar cell.

[0108] The forward bias voltage is 4.0 V, the shape of the picosecond pulse laser is a point-shaped light plate with a diameter of 50 μm, the wavelength is 532 nm, the scanning speed is 18 m / s, the frequency is 400 kHz, and the peak energy is 4.0 J / cm 2 The sintering temperature at peak energy is 600°C; the sintering time is 2s.

[0109] Example 4

[0110] This embodiment provides a solar cell. The difference from Embodiment 1 is that in step 2, the temperature of the light injection treatment is 100° C. and the time is 180 seconds. The remaining steps are the same as those in Embodiment 1 and will not be described again.

[0111] Example 5

[0112] This embodiment provides a solar cell. The difference from Embodiment 1 is that in step 2, the temperature of the light injection treatment is 160° C. and the time is 60 seconds. The remaining steps are the same as those in Embodiment 1 and will not be described again.

[0113] Example 6

[0114] This embodiment provides a solar cell. The difference from Embodiment 1 is that in step 2, the temperature of the light injection treatment is 80° C. and the time is 180 s. The remaining steps are the same as those in Embodiment 1 and will not be described again.

[0115] Example 7

[0116] This embodiment provides a solar cell. The difference from Embodiment 1 is that in step 2, the temperature of the light injection treatment is 180° C. and the time is 60 seconds. The remaining steps are the same as those in Embodiment 1 and will not be described again.

[0117] Example 8

[0118] This embodiment provides a solar cell. The difference from the embodiment 1 is that in step 3, the peak energy of the picosecond pulse laser is 10.0 J / cm 2The sintering temperature at the peak energy is 800° C. and the sintering time is 0.5 s. The remaining steps are the same as those in Example 1 and will not be described in detail here.

[0119] Example 9

[0120] This embodiment provides a solar cell. The difference from the embodiment 1 is that in step 3, the peak energy of the picosecond pulse laser is 1.0 J / cm 2 The sintering temperature at the peak energy is 600° C. and the sintering time is 2 seconds. The remaining steps are the same as those in Example 1 and will not be described in detail here.

[0121] Example 10

[0122] This embodiment provides a solar cell. The difference from the embodiment 1 is that in step 3, the peak energy of the picosecond pulse laser is 12.0 J / cm 2 The sintering temperature at the peak energy is 1000° C. and the sintering time is 0.5 s. The remaining steps are the same as those in Example 1 and will not be described again.

[0123] Embodiment 11

[0124] This embodiment provides a solar cell. The difference from the embodiment 1 is that in step 3, the peak energy of the picosecond pulse laser is 0.5 J / cm 2 The sintering temperature at the peak energy is 400° C. and the sintering time is 2 seconds. The remaining steps are the same as those in Example 1 and will not be described in detail here.

[0125] Comparative Example 1

[0126] This comparative example provides a solar cell, the preparation method of which is as follows:

[0127] The silicon substrate is laser cut to form patterned grooves, and then double-sided electroplating is performed to form metal electrodes to obtain a solar cell.

[0128] The coating structure of the metal electrode is a barrier layer, a conductive layer and a protective layer stacked in sequence. The barrier layer is made of nickel with a thickness of 1 μm; the conductive layer is made of copper with a thickness of 9 μm; and the protective layer is made of tin with a thickness of 1 μm.

[0129] Comparative Example 2

[0130] This comparative example provides a solar cell, and the specific steps are as follows:

[0131] 1. Same as the step in Example 1.

[0132] 2. The double-sided electroplated solar cell is passed through a light injection furnace at a uniform speed for light injection treatment to obtain a solar cell.

[0133] The light source in the light injection furnace is a xenon lamp with a light radiation intensity of 20 suns and a light intensity of 2000 W / m 2 .

[0134] The temperature of the light injection treatment was 130°C and the time was 120s.

[0135] Comparative Example 3

[0136] This comparative example provides a solar cell, and the specific steps are as follows:

[0137] 1. Same as the step in Example 1.

[0138] 2. Use a picosecond pulse laser to sequentially irradiate the metal grid lines on the front and back of the double-sided electroplated solar cell, and load a forward bias voltage on the metal grid lines of the double-sided electroplated solar cell through an external power supply to sinter the metal grid lines to obtain a solar cell.

[0139] The forward bias voltage is 5.0 V, the shape of the picosecond pulse laser is a point-shaped light plate with a diameter of 40 μm, the wavelength is 755 nm, the scanning speed is 10 m / s, the frequency is 300 kHz, and the peak energy is 5.0 J / cm 2 The sintering temperature at peak energy is 700°C; the sintering time is 1s.

[0140] Test Case

[0141] The solar cells obtained in the embodiment and the comparative example were made into the same specifications and tested for electrical properties, including photoelectric conversion efficiency, open circuit voltage, series resistance, etc.

[0142] Specifically, IV test was performed at a temperature of 25° C. and an AM of 1.5G, and the obtained data is shown in Table 1 below.

[0143] In Table 1, Eta (%) refers to the efficiency of the solar cell, which refers to the efficiency of the solar cell in converting the received solar radiation energy into electrical energy, usually expressed as a percentage. Uoc (V) is the open-circuit voltage. This refers to the voltage when there is no current flowing through the two ends of the solar cell (that is, when the circuit is disconnected). The open-circuit voltage is the voltage value that the battery can provide when there is no load, and the unit is V. Isc (A) refers to the short-circuit current, which refers to the current flowing through the battery when the two ends of the solar cell are directly short-circuited. The short-circuit current is the current value that the battery can provide when there is no external load, and the unit is A. FF (%) is the fill factor, which refers to the product of the ratio of the current and voltage of the solar cell under the actual working state to the current and voltage under the ideal condition (that is, the current and voltage at the maximum power point), usually expressed as a percentage.

[0144] Table 1

[0145] Eta(%) Uoc(V) Isc(A) FF(%) Rs(Ω) Example 1 26.47 0.7223 18.63 86.77 0.00063 Example 2 26.37 0.7227 18.60 86.48 0.00065 Example 3 26.41 0.7217 18.58 86.85 0.00066 Example 4 26.43 0.7231 18.56 86.81 0.00064 Example 5 26.37 0.7207 18.55 86.97 0.00058 Example 6 26.11 0.7219 18.55 85.95 0.00056 Example 7 26.07 0.7176 18.57 86.27 0.00063 Example 8 26.35 0.7231 18.57 86.49 0.00064 Example 9 26.37 0.7191 18.60 86.98 0.00067 Example 10 26.10 0.7225 18.59 85.67 0.00060 Embodiment 11 26.18 0.7244 18.57 85.84 0.00061 Comparative Example 1 25.95 0.7223 18.59 85.17 0.00078 Comparative Example 2 26.13 0.7187 18.59 86.26 0.00075 Comparative Example 3 26.12 0.7176 18.55 86.53 0.00074

[0146] As can be seen from Table 1, the hydrogen ions are activated by light injection and migrated into the crystalline silicon layer to achieve interface passivation, thereby improving the photoelectric conversion efficiency of the solar cell. In addition, the present invention adds a double-sided laser sintering process after the light injection process to make the metal electrode and the silicon substrate form a closer contact and reduce the contact resistance.

[0147] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A post-processing process for metal electrodes of solar cells, characterized in that: The post-processing process at least includes: The solar cell with metal electrodes on both sides is subjected to light injection treatment and double-sided laser sintering in sequence.

2. The post-processing process according to claim 1, characterized in that: The solar cell is a TOPCon solar cell.

3. The post-processing process according to claim 1, characterized in that: The plating structure of the metal electrode includes a barrier layer, a conductive layer and a protective layer; Preferably, the material of the barrier layer includes at least one of nickel, cobalt, titanium, tungsten and tantalum; Preferably, the conductive layer is made of copper; Preferably, the material of the protective layer is at least one of tin, silver and nickel.

4. The post-processing process according to any one of claims 1 to 3, characterized in that: The process of the light injection treatment includes: The solar cell with metal electrodes is passed through a light injection furnace at a uniform speed to perform the light injection treatment.

5. The post-processing process according to claim 4, characterized in that: The light injection treatment is performed at a temperature of 100° C. to 160° C. and for a time of 60s to 180s. Preferably, the light radiation intensity of the light injection treatment is 5 suns to 30 suns; Preferably, the light source for the light injection treatment includes at least one of an infrared lamp, an LED lamp, a xenon lamp and a tungsten lamp; Preferably, the light intensity of the light source for the light injection treatment is 1000 W / m 2 ~5000W / m 2 .

6. The post-treatment process according to any one of claims 1 to 3, characterized in that: The laser sintering process includes: Laser is used to irradiate the metal electrodes on the front and back of the solar cell respectively, and a forward bias is applied to the metal electrodes to achieve sintering of the metal electrodes.

7. The post-processing process according to claim 6, characterized in that: A forward bias is applied to the metal electrode through an external power supply; Preferably, the forward bias voltage is 1.0V to 10.0V.

8. The post-processing process according to claim 6, characterized in that: The type of the laser is picosecond pulse laser; Preferably, the scanning speed of the picosecond pulse laser is 5m / s to 20m / s; Preferably, the frequency of the laser is 100kHz to 500kHz, and the peak energy is 1.0J / cm 2 ~10.0J / cm 2 ; Preferably, the shape of the laser is a point-shaped spot; Preferably, the diameter of the point-shaped light spot is 20 μm to 60 μm; Preferably, the wavelength of the laser is one of 532 nm, 755 nm, 980 nm, and 1064 nm.

9. The post-processing process according to claim 6, characterized in that: The peak temperature of the sintering is 600°C to 800°C; Preferably, the sintering time is 0.5s to 2s.

10. A method for preparing a solar cell, characterized in that: The preparation method comprises the post-treatment process of the metal electrode of the solar cell according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Crystalline silicon solar cell laser sintering method

    CN116705903A

  • Metallized electrode structure of solar cell and preparation method thereof

    CN117153904A

  • Solar cell and metallization method thereof, photovoltaic module and photovoltaic system

    CN118173655A

Cited By

  • Method for metalizing back electrode of TOPCon solar cell

    CN119364924A

  • Method for improving reliability of laser-assisted sintering of solar cell and solar cell

    CN121038427A

  • A method for improving reliability of laser-assisted sintering of solar cells and a solar cell

    CN121038427B