TOPCon solar cell with double-layer passivation contact structure and preparation method of TOPCon solar cell

By using a double-layer passivation contact structure and increasing oxygen flow in TOPCon batteries, the problem of insufficient annealing capacity of low phosphorus diffusion temperature is solved, the crystallization rate and battery efficiency are improved, and the higher Tunneling effect and passivation capability.

CN118919604AActive Publication Date: 2024-11-08HUAIAN JIETAI NEW ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411161636.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

TOPCon batteries have low temperature and low annealing ability when phosphorus diffusion, resulting in a decrease in the crystallization rate of the polysilicon layer, increasing the backside recombination and reducing the electrical output, affecting the battery conversion efficiency.

Method used

The TOPCon solar cell preparation method adopts a double-layer passivation contact structure includes depositing a first tunneling oxide layer, a barrier polysilicon layer, a second tunneling oxide layer and a doped polysilicon layer on the back of the silicon substrate, and a stacked structure of a polysilicon layer on the back of the silicon substrate, and Increase the oxygen flow before diffusion to form a silica film masking film, increase the phosphorus diffusion propulsion temperature and optimize the crystallization ability.

Benefits of technology

By increasing the phosphorus diffusion propulsion temperature, improving crystallization capacity, maintaining the tunneling effect, significantly improving the efficiency of TOPCon batteries, avoiding the increase in internal expansion caused by high-temperature phosphorus expansion, and maintaining the contact passivation ability of the polysilicon layer and the tunneling layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919604A_ABST
    Figure CN118919604A_ABST
Patent Text Reader

Abstract

The invention discloses a TOPCon solar cell with a double-layer passivation contact structure and a preparation method of the TOPCon solar cell, and belongs to the field of TOPCon cells. A first tunneling oxide layer and a barrier polycrystalline silicon layer are deposited on the back surface of a treated silicon substrate; depositing a second tunneling oxide layer and a doped polycrystalline silicon layer on the deposited barrier polycrystalline silicon layer again; increasing the oxygen flow, and forming a silicon dioxide mask film on the back surface; and back phosphorus diffusion is carried out. The method has the beneficial effects that through the improvement of the process, the propulsion temperature of phosphorus diffusion can be greatly increased, the crystallization capability is improved, the internal expansion increase caused by high-temperature phosphorus expansion is avoided, the good tunneling effect is kept unchanged, the contact passivation capability of the polycrystalline silicon layer and the tunneling layer is maintained, and finally, the efficiency of the TOPCon battery is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of TOPCon cells, and in particular to a TOPCon solar cell with a double-layer passivation contact structure and a preparation method thereof. Background Art

[0002] In recent years, high-efficiency and low-cost solar cells have been one of the research hotspots in the photovoltaic industry. TOPCon solar cells refer to first preparing a 1-2nm tunneling oxide layer on the back of the cell, and then depositing a layer of doped polysilicon. The two together form a passivation contact structure, providing good interface passivation for the back of the silicon wafer. The ultra-thin oxide layer allows majority electrons to tunnel into the polysilicon layer while blocking minority hole recombination, and then the electrons are transported laterally in the polysilicon layer and collected by the metal, thereby greatly reducing the metal contact recombination current and improving the open circuit voltage and short circuit current of the battery.

[0003] The main methods for preparing tunnel oxide layer and doped polysilicon layer in TOPCon battery preparation process are APCVD (atmospheric pressure chemical vapor deposition), LPCVD (low pressure chemical vapor deposition) and PECVD (plasma enhanced chemical vapor deposition). LPCVD is widely used due to its low impurity content, excellent uniformity, superior film density and high production capacity. Since the polysilicon layer generated on the front of TOPCon products will increase the parasitic absorption of light and reduce efficiency, the polysilicon layer is avoided as much as possible on the front, and a thin polysilicon layer is used on the back to reduce the optical parasitic absorption of the polysilicon on the back. In order to match the thin polysilicon, phosphorus diffusion is promoted by low-temperature deposition to form a good passivation and contact layer, but the low annealing ability of phosphorus diffusion at low temperature will have some negative effects on the crystallization degree of the polysilicon layer, increase the back recombination and reduce the electrical output, resulting in low battery conversion efficiency, which needs to be improved urgently!

[0004] In view of this, the inventor conducted in-depth research on this demand, and thus the present case was produced. Summary of the invention

[0005] In order to solve the problem in the prior art that the TOPCon cell has low annealing ability at low temperature during phosphorus diffusion, which leads to a decrease in the crystallization rate of the polysilicon layer, increases back recombination and reduces electrical output, and affects the cell conversion efficiency, the present invention provides a method for preparing a TOPCon solar cell with a double-layer passivation contact structure, comprising the following steps:

[0006] Step 1: Clean and texturize the silicon substrate, diffuse boron on the front side, and perform etching and alkaline polishing treatment in sequence;

[0007] Step 2, depositing a first tunneling oxide layer and a blocking polysilicon layer on the back side of the processed silicon substrate;

[0008] Step 3, depositing a second tunneling oxide layer and a doped polysilicon layer again on the deposited blocking polysilicon layer;

[0009] Step 4, increasing the oxygen flow rate to form a silicon dioxide film mask on the back side;

[0010] Step 5: back phosphorus diffusion;

[0011] Step six, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence.

[0012] Compared with the conventional production line process, in order to achieve a higher level of improvement in the tunneling effect, the present invention has developed a new type of stacked structure process. By depositing a stacked structure of a first tunneling oxide layer - a blocking polysilicon layer - a second tunneling oxide layer - a doped polysilicon layer on the back of a silicon substrate, the advancement temperature of phosphorus diffusion can be greatly increased, thereby improving the crystallization ability. At the same time, it can avoid the increase in internal expansion caused by high-temperature phosphorus expansion, maintain a good tunneling effect unchanged, maintain the contact passivation ability of the polysilicon layer and the tunneling layer, and ultimately greatly improve the efficiency of the TOPCon battery.

[0013] Preferably, in step 1, the silicon substrate is textured on both sides to obtain a textured silicon wafer, so as to remove surface damage and form a surface pyramid light trapping structure. Boron is diffused on the front side of the textured silicon wafer to form the P + The doping layer and the borosilicate glass layer are then removed by etching, and the back surface of the crystalline silicon substrate is polished by alkali polishing to remove the phosphosilicate glass layer formed during the boron diffusion process.

[0014] Preferably, in the step 2, LPCVD equipment is used, oxygen is introduced under normal pressure, and the reaction is carried out at a temperature of 600-620°C for 950-1200s to form a first tunneling oxide layer on the surface of the silicon substrate. Subsequently, a blocking polysilicon layer is deposited on the surface of the first tunneling oxide layer by reacting at a low pressure of 200-300mtorr and a temperature of 590-630°C for 200-400s.

[0015] Preferably, the thickness of the first tunneling oxide layer is 1-1.5 nm, and the thickness of the blocking polysilicon layer is 20-40 nm.

[0016] Preferably, in the step three, LPCVD equipment is used, oxygen is introduced under normal pressure, and the reaction is carried out at a temperature of 590-630°C for 200-400s to form a second tunneling oxide layer on the surface of the silicon substrate. Subsequently, a doped polysilicon layer is deposited on the surface of the second tunneling oxide layer by reacting at a low pressure of 200-300mtorr and a temperature of 590-630°C for 1000-1400s.

[0017] Preferably, the thickness of the second tunneling oxide layer is 0.3-0.5 nm, and the thickness of the doped polysilicon layer is 100-130 nm.

[0018] The present invention adopts Doe experimental design to verify the gradient of oxide layers and polysilicon layers with different thicknesses, and obtains the optimal thickness result of the first tunneling oxide layer (1-1.5nm) - blocking polysilicon layer (20-40nm) - second tunneling oxide layer (0.3-0.5nm) - doped polysilicon layer (100-130nm).

[0019] Preferably, in step 4, a low-pressure diffusion deposition device is used to form a silicon dioxide masking film through low-pressure oxidation with an oxygen flow rate of 1100 to 1400 sccm and a reaction time of 200 to 300 seconds.

[0020] In step 4, the oxygen flow rate is increased to 1100-1400 sccm, thereby forming a thicker silicon dioxide mask on the back of the TOPCon cell. At high temperatures, the solid solubility of P atoms in SiO2 and Si is very different, and the diffusion rate of phosphorus in silicon is much greater than that in silicon dioxide. Therefore, adding a layer of silicon dioxide mask before phosphorus diffusion can slow down the diffusion rate of P and prevent P diffusion.

[0021] Preferably, in the step five, POCl3 is used for phosphorus diffusion, firstly low-temperature deposition is performed, then staged advancement is performed, POCl3 is used again for source supplement diffusion, and finally a post-oxidation annealing process is performed.

[0022] Preferably, in step 5, POCl3 is used for phosphorus diffusion at a flow rate of

[0023] 1500~1600sccm, first low-temperature deposition, the deposition temperature is 750~850℃, the time is 900~1200s; then advance in stages, first at a temperature of 860~930℃ for 10~20min, then at 800~860℃ for 10~20min; then POCl3 is used for source diffusion again, the flow rate is 1500~1600sccm, the deposition temperature is 830~860℃, the time is 120~180s, and finally an oxidation annealing process is carried out for 1200~1500s, and the temperature is reduced to 720~750℃.

[0024] With the high-temperature advancement process, the phosphorus source deposited on the surface of the silicon wafer in the deposition step is consumed, and the surface concentration decreases. In the step five, the temperature of the heating advancement is increased, and the source is passed again at the end, POCl3 is added for diffusion, and the surface concentration is appropriately increased, thereby improving the crystallization ability, optimizing the bandgap width, achieving the purpose of increasing the opening voltage and improving the efficiency, maintaining a good tunneling layer, and maintaining the original passivation and contact capabilities of the single-layer polysilicon.

[0025] Preferably, in step 6, RCA is used to clean the back oxide layer, the N+ layer generated on the front and edge during phosphorus diffusion, and the front borosilicate glass layer and the front phosphosilicate glass layer are removed; then, aluminum oxide atomic layer deposition is performed on the front to form an aluminum oxide passivation layer; SiN is deposited on the front and back. x , forming a front anti-reflection layer and a back anti-reflection layer; and then forming an ohmic contact by printing electrodes and high-temperature sintering.

[0026] The present invention also provides a TOPCon solar cell obtained by adopting the above preparation method.

[0027] Preferably, the above-mentioned TOPCon solar cell comprises an N-type silicon wafer, wherein a P+ diffusion layer, an aluminum oxide passivation layer, a front anti-reflection layer and a front metal electrode are sequentially arranged on the front side of the N-type silicon wafer, and a first tunneling oxide layer, a blocking polysilicon layer, a second tunneling oxide layer, a doped polysilicon layer, a back anti-reflection layer and a back metal electrode are sequentially arranged on the back side; the front metal electrode penetrates the front anti-reflection layer and the aluminum oxide passivation layer to form an ohmic contact with the P+ diffusion layer; the back metal electrode penetrates the back anti-reflection layer to form an ohmic contact with the doped polysilicon layer.

[0028] The beneficial effects produced by the technical solution of the present invention are as follows:

[0029] (1) By depositing a stacked structure of the first tunneling oxide layer - blocking polysilicon layer - second tunneling oxide layer - doped polysilicon layer on the back of the silicon substrate, the advancement temperature of phosphorus diffusion can be greatly increased, thereby improving the crystallization ability. At the same time, it can avoid the increase in internal expansion caused by high-temperature phosphorus diffusion, maintain a good tunneling effect, maintain the contact passivation ability of the polysilicon layer and the tunneling layer, and ultimately greatly improve the efficiency of the TOPCon battery.

[0030] (2) By adopting the Doe experimental design, the gradient of oxide layers and polysilicon layers with different thicknesses was verified, and the thickness was obtained as follows: first tunneling oxide layer (1-1.5nm) - blocking polysilicon layer (20-40nm) - second tunneling oxide layer (0.3-0.5nm) - doped polysilicon layer (100-130nm), thereby greatly increasing the advancement temperature of phosphorus diffusion and improving the crystallization ability.

[0031] (3) By increasing the oxygen flow rate before phosphorus diffuses, a thicker silicon dioxide mask is formed on the back of the battery, which slows down the diffusion rate of phosphorus and prevents the solubility difference between phosphorus atoms in SiO2 and Si at high temperatures from being too large. The diffusion rate of phosphorus in silicon is also much greater than that in silicon dioxide, which leads to P diffusion.

[0032] (4) By increasing the temperature of the heating process and passing the source again at the end, adding POCl3 for diffusion, the surface concentration is appropriately increased, thereby improving the crystallization ability and optimizing the bandgap width, thereby achieving the purpose of increasing the opening voltage and improving the efficiency, maintaining a good tunneling layer, and maintaining the original passivation and contact capabilities of the single-layer polysilicon. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 It is a schematic diagram of the structure of the TOPCon solar cell in the present invention.

[0035] In the figure, 1. N-type silicon wafer; 2. P+ diffusion layer; 3. aluminum oxide passivation layer; 4. front anti-reflection layer; 5. front metal electrode; 6. first tunneling oxide layer; 7. blocking polysilicon layer; 8. second tunneling oxide layer; 9. doped polysilicon layer; 10. back anti-reflection layer; 11. back metal electrode. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] This implementation method uses a double-layer passivation contact structure on the TOPCon solar cell, and increases the oxygen flow rate before the phosphorus diffusion process to form a thicker silicon dioxide masking film, reduces the phosphorus source flow rate at the beginning of phosphorus diffusion, greatly increases the advancement temperature and improves the crystallization ability, and then performs a source replenishment process after the advancement is completed to increase the phosphorus diffusion surface concentration, and ultimately greatly improve the efficiency of the TOPCon cell. The specific implementation method is as follows:

[0038] like Figure 1 As shown, a method for preparing a TOPCon solar cell with a double-layer passivation contact structure comprises the following steps:

[0039] Step 1, select an n-type silicon substrate 1 and sequentially perform cleaning, texturing, front boron diffusion and etching and alkaline polishing treatments;

[0040] Step 2: Using LPCVD equipment, oxygen is introduced under normal pressure, and the reaction is carried out at a temperature of 600-620° C. for 950-1200 seconds to form a first tunnel oxide layer 6 with a thickness of 1-1.5 nm on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer 7 with a thickness of 20-40 nm is deposited on the surface of the first tunnel oxide layer 6 by reacting at a low pressure of 200-300 mtorr and a temperature of 590-630° C. for 200-400 seconds;

[0041] Step 3: Using LPCVD equipment, oxygen is introduced under normal pressure, and the reaction is carried out at a temperature of 590-630° C. for 200-400 seconds to form a second tunnel oxide layer 8 on the surface of the silicon substrate with a thickness of 0.3-0.5 nm. Subsequently, a doped polysilicon layer 9 with a thickness of 100-130 nm is deposited on the surface of the second tunnel oxide layer 8 by reacting at a low pressure of 200-300 mtorr and a temperature of 590-630° C. for 1000-1400 seconds;

[0042] Step 4: using a low-pressure diffusion deposition device, through low-pressure oxidation, using an oxygen flow rate of 1100 to 1400 sccm, reacting for 200 to 300 seconds, to form a thicker silicon dioxide masking film;

[0043] Step five, use POCl3 for phosphorus diffusion with a flow rate of 1500-1600sccm, first low-temperature deposition, the deposition temperature is 750-850℃, and the time is 900-1200s; then advance in stages, first heat up at a temperature of 860-930℃ for 10-20min, and then cool down at 800-860℃ for 10-20min; then use POCl3 for source diffusion again with a flow rate of 1500-1600sccm, the deposition temperature is 830-860℃, and the time is 120-180s, and finally an oxidation annealing process is performed for 1200-1500s, and the temperature is reduced to 720-750℃.

[0044] Step six, finally, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence to make a battery.

[0045] The present invention also provides a TOPCon solar cell obtained by adopting the above preparation method.

[0046] As a preferred embodiment, the above-mentioned TOPCon solar cell includes an N-type silicon wafer 1, the front side of the N-type silicon wafer is sequentially provided with a P+ diffusion layer 2, an aluminum oxide passivation layer 3, a front anti-reflection layer 4 and a front metal electrode 5, and the back side is sequentially provided with a first tunneling oxide layer 6, a blocking polysilicon layer 7, a second tunneling oxide layer 8, a doped polysilicon layer 9, a back anti-reflection layer 10 and a back metal electrode 11; the front metal electrode 5 penetrates the front anti-reflection layer 4 and the aluminum oxide passivation layer 3 to form an ohmic contact with the P+ diffusion layer 2; the back metal electrode 11 penetrates the back anti-reflection layer 10 to form an ohmic contact with the doped polysilicon layer 9.

[0047] The beneficial effects of the method for preparing a TOPCon solar cell with a double-layer passivation contact structure in the present invention are further reviewed through several groups of embodiments.

[0048] Embodiment 1:

[0049] In this embodiment, a method for preparing a TOPCon solar cell with a double-layer passivation contact structure includes the following steps:

[0050] Step 1: Select an n-type silicon substrate and perform cleaning, texturing, front boron diffusion and etching and alkaline polishing in sequence;

[0051] Step 2: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 620°C for 1200s to form a first tunnel oxide layer with a thickness of 1.5nm on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer with a thickness of 40nm is deposited on the surface of the first tunnel oxide layer by reacting at a low pressure of 300mtorr and a temperature of 630°C for 400s.

[0052] Step 3: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 630°C for 400s to form a second tunnel oxide layer with a thickness of 0.5nm on the surface of the silicon substrate. Subsequently, a doped polysilicon layer with a thickness of 130nm is deposited on the surface of the second tunnel oxide layer by reacting at a low pressure of 300mtorr and a temperature of 630°C for 1400s.

[0053] Step 4: using a low-pressure diffusion deposition device, through low-pressure oxidation, using an oxygen flow rate of 1400 sccm, and reacting for 300 seconds, to form a thicker silicon dioxide masking film;

[0054] Step 5: Phosphorus diffusion is performed using POCl3 at a flow rate of 1600 sccm. Low-temperature deposition is performed first, with a deposition temperature of 850°C for 1200 seconds. The process is then advanced in stages, with a temperature rise at 930°C for 20 minutes, and then a temperature drop at 860°C for 10 minutes. POCl3 is then used for source diffusion again, with a flow rate of 1600 sccm, a deposition temperature of 860°C for 180 seconds, and finally an oxidation annealing process is performed for 1500 seconds, followed by cooling to 750°C.

[0055] Step six, finally, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence to make a battery.

[0056] Comparative Example 1:

[0057] In the preparation method of this comparative example 1, the phosphorus diffusion process in step 5 only includes deposition and oxidation annealing, specifically:

[0058] POCl3 was used as the diffusion source, the flow rate was 1600sccm, the temperature was 850℃, and the time was 35min. Finally, an oxidation annealing process was performed for 1500s and the temperature was lowered to 750℃.

[0059] The other steps are the same as in Example 1.

[0060] Embodiment 2:

[0061] In this embodiment, a method for preparing a TOPCon solar cell with a double-layer passivation contact structure includes the following steps:

[0062] Step 1: Select an n-type silicon substrate and perform cleaning, texturing, front boron diffusion and etching and alkaline polishing in sequence;

[0063] Step 2: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 610°C for 1100s to form a first tunnel oxide layer with a thickness of 1.3nm on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer with a thickness of 30nm is deposited on the surface of the first tunnel oxide layer by reacting at a low pressure of 260mtorr and a temperature of 620°C for 300s.

[0064] Step 3: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 610°C for 300s to form a second tunnel oxide layer with a thickness of 0.4nm on the surface of the silicon substrate. Subsequently, a doped polysilicon layer with a thickness of 120nm is deposited on the surface of the second tunnel oxide layer by reacting at a low pressure of 260mtorr and a temperature of 620°C for 1300s.

[0065] Step 4: low-pressure diffusion deposition equipment is used to form a thicker silicon dioxide masking film by low-pressure oxidation, using an oxygen flow rate of 1300 sccm and reacting for 280 seconds;

[0066] Step 5: Phosphorus diffusion is performed using POCl3 at a flow rate of 1550sccm. Low-temperature deposition is performed first, with a deposition temperature of 830°C for 1100s. The process is then advanced in stages, with a temperature rise at 910°C for 18min, followed by a temperature drop at 840°C for 18min. POCl3 is then used for source supplementation diffusion again, with a flow rate of 1550sccm, a deposition temperature of 850°C for 160s, and finally an oxidation annealing process is performed for 1400s before cooling to 740°C.

[0067] Step six, finally, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence to make a battery.

[0068] Comparative Example 2:

[0069] In the preparation method of this comparative example 2, the phosphorus diffusion process in step 5 only includes deposition, high temperature advancement and oxidation annealing, specifically:

[0070] Using POCl3 as the diffusion source with a flow rate of 1550sccm, low-temperature deposition was first performed at 830°C for 1100s. Then, the process was advanced in stages, first at a temperature of 910°C for 18min, then at a temperature of 840°C for 18min. Finally, an oxidation annealing process was performed for 1400s, followed by cooling to 740°C.

[0071] The other steps are the same as in Example 2.

[0072] Embodiment 3:

[0073] In this embodiment, a method for preparing a TOPCon solar cell with a double-layer passivation contact structure includes the following steps:

[0074] Step 1: Select an n-type silicon substrate and perform cleaning, texturing, front boron diffusion and etching and alkaline polishing in sequence;

[0075] Step 2: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 610°C for 1000s to form a first tunneling oxide layer with a thickness of 1.2nm on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer with a thickness of 30nm is deposited on the surface of the first tunneling oxide layer by reacting at a low pressure of 240mtorr and a temperature of 600°C for 300s.

[0076] Step 3: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 610°C for 300s to form a second tunnel oxide layer with a thickness of 0.4nm on the surface of the silicon substrate. Subsequently, a doped polysilicon layer with a thickness of 110nm is deposited on the surface of the second tunnel oxide layer by reacting at a low pressure of 240mtorr and a temperature of 600°C for 1200s.

[0077] Step 4: low-pressure diffusion deposition equipment is used to form a thicker silicon dioxide masking film by low-pressure oxidation, using an oxygen flow rate of 1200 sccm and reacting for 260 seconds;

[0078] Step 5: Phosphorus diffusion is performed using POCl3 at a flow rate of 1550sccm. Low-temperature deposition is performed first, with a deposition temperature of 800°C for 1000s. The process is then advanced in stages, with a temperature rise at 880°C for 16min, and then a temperature drop at 820°C for 16min. POCl3 is then used for source supplementation diffusion again, with a flow rate of 1550sccm, a deposition temperature of 840°C for 150s, and finally an oxidation annealing process is performed for 1300s, followed by cooling to 730°C.

[0079] Step six, finally, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence to make a battery.

[0080] Comparative Example 3:

[0081] In the preparation method of this comparative example 3, step 4 uses a low-pressure diffusion deposition device, and forms a thicker silicon dioxide masking film by low-pressure oxidation with an oxygen flow rate of 1000 sccm for 260 seconds. The other steps are the same as those in Example 3.

[0082] Embodiment 4:

[0083] In this embodiment, a method for preparing a TOPCon solar cell with a double-layer passivation contact structure includes the following steps:

[0084] Step 1: Select an n-type silicon substrate and perform cleaning, texturing, front boron diffusion and etching and alkaline polishing in sequence;

[0085] Step 2: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 600°C for 950s to form a first tunnel oxide layer with a thickness of 1nm on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer with a thickness of 20nm is deposited on the surface of the first tunnel oxide layer by reacting at a low pressure of 200mtorr and a temperature of 590°C for 200s.

[0086] Step 3: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 590°C for 200s to form a second tunnel oxide layer with a thickness of 0.3nm on the surface of the silicon substrate. Subsequently, a doped polysilicon layer with a thickness of 100nm is deposited on the surface of the second tunnel oxide layer by reacting at a low pressure of 200mtorr and a temperature of 590°C for 1000s.

[0087] Step 4: using a low-pressure diffusion deposition device, through low-pressure oxidation, using an oxygen flow rate of 1100 sccm, and reacting for 200 seconds, to form a thicker silicon dioxide masking film;

[0088] Step 5: Phosphorus diffusion is performed using POCl3 at a flow rate of 1500sccm. Low-temperature deposition is performed first, with a deposition temperature of 750°C for 900s. The process is then advanced in stages, with a temperature rise at 860°C for 10min, and then a temperature drop at 800°C for 20min. POCl3 is then used for source diffusion again, with a flow rate of 1500sccm, a deposition temperature of 830°C for 120s, and finally an oxidation annealing process is performed for 1200s, followed by cooling to 720°C.

[0089] Step six, finally, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence to make a battery.

[0090] Comparative Example 4:

[0091] In the preparation method of this comparative example 4, step 4 uses a low-pressure diffusion deposition device, and forms a thicker silicon dioxide masking film by low-pressure oxidation, using an oxygen flow rate of 1500 sccm, and reacting for 200 seconds. The other steps are the same as those of Example 4.

[0092] The TOPCon solar cells obtained in the above four groups of embodiments and comparative examples were tested for performance, and the results are as follows:

[0093] Table 1 TOPCon solar cell performance test results of Examples 1 to 4 and Comparative Examples 1 to 4

[0094]

[0095]

[0096] It can be seen from Table 1 that the TOPCon solar cells prepared in Examples 1 to 4 of the present application adopt a double-layer passivation contact structure + increase in oxygen flow before phosphorus diffusion + optimization of source quantity and advancement temperature process for phosphorus diffusion + re-source replenishment, respectively, compared with their comparative examples 1 to 4, the voltage, current and photoelectric conversion efficiency of the battery are improved, and the advancement temperature of phosphorus diffusion can be greatly increased to improve the crystallization ability.

[0097] Embodiment 5:

[0098] In this embodiment, a method for preparing a TOPCon solar cell with a double-layer passivation contact structure includes the following steps:

[0099] Step 1: Select an n-type silicon substrate and perform cleaning, texturing, front boron diffusion and etching and alkaline polishing in sequence;

[0100] Step 2: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 610°C for 1100s to form a first tunnel oxide layer with a thickness of 1.3nm on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer with a thickness of 30nm is deposited on the surface of the first tunnel oxide layer by reacting at a low pressure of 240mtorr and a temperature of 600°C for 300s.

[0101] Step 3: Using LPCVD equipment, oxygen is introduced under normal pressure and reacted at 600°C for 300s to form a second tunnel oxide layer with a thickness of 0.4nm on the surface of the silicon substrate. Subsequently, a doped polysilicon layer with a thickness of 120nm is deposited on the surface of the second tunnel oxide layer by reacting at a low pressure of 240mtorr and a temperature of 600°C for 1200s.

[0102] Step 4: using a low-pressure diffusion deposition device, through low-pressure oxidation, using an oxygen flow rate of 1400 sccm, and reacting for 300 seconds, to form a thicker silicon dioxide masking film;

[0103] Step 5: Phosphorus diffusion is performed using POCl3 at a flow rate of 1550sccm. Low-temperature deposition is performed first at a deposition temperature of 830°C for 1000s. The process is then advanced in stages, first at a temperature of 930°C for 20min, then at a temperature of 860°C for 20min. POCl3 is then used for source diffusion again at a flow rate of 1550sccm, a deposition temperature of 850°C for 180s, and finally an oxidation annealing process is performed for 1500s before cooling to 750°C.

[0104] Step six, finally, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence to make a battery.

[0105] Comparative Example 5:

[0106] In the preparation method of this comparative example 5, step 2 and step 3 form a first tunneling oxide layer (0.8nm) - a blocking polysilicon layer (18nm) - a second tunneling oxide layer (0.4nm) - a doped polysilicon layer (120nm), and the other steps are the same as those in Example 5.

[0107] Comparative Example 6:

[0108] The preparation method in this comparative example 6 is the same as that in Example 5 except that step 2 and step 3 form the first tunneling oxide layer (1.8nm) - blocking polysilicon layer (45nm) - second tunneling oxide layer (0.4nm) - doped polysilicon layer (120nm).

[0109] Comparative Example 7:

[0110] The preparation method in this comparative example 7 is the same as that in Example 5 except that step 2 and step 3 form the first tunneling oxide layer (1.3nm) - blocking polysilicon layer (30nm) - second tunneling oxide layer (0.2nm) - doped polysilicon layer (90nm).

[0111] Comparative Example 8:

[0112] The preparation method in this comparative example 8 is the same as that in Example 5 except that step 2 and step 3 form the first tunneling oxide layer (1.3nm) - blocking polysilicon layer (30nm) - second tunneling oxide layer (0.6nm) - doped polysilicon layer (140nm).

[0113] The TOPCon solar cells obtained in the above-mentioned Example 5 and Comparative Examples 5 to 8 were subjected to performance tests, and the results are as follows:

[0114] Table 2 TOPCon solar cell performance test results of Example 5 and Comparative Examples 5 to 8

[0115]

[0116] It can be seen from Table 2 that the TOPCon solar cell prepared in Example 5 of the present application adopts a double-layer passivation contact structure with a thickness of a first tunneling oxide layer (1-1.5 nm) - a blocking polysilicon layer (20-40 nm) - a second tunneling oxide layer (0.3-0.5 nm) - a doped polysilicon layer (100-130 nm). Compared with comparative examples 5 to 8, the voltage, current and photoelectric conversion efficiency of the battery are also improved.

[0117] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a TOPCon solar cell with a double-layer passivation contact structure, characterized in that: The steps include: Step 1: Clean and texturize the silicon substrate, diffuse boron on the front side, and perform etching and alkaline polishing treatment in sequence; Step 2, depositing a first tunneling oxide layer and a blocking polysilicon layer on the back side of the processed silicon substrate; Step 3, depositing a second tunneling oxide layer and a doped polysilicon layer again on the deposited blocking polysilicon layer; Step 4, increasing the oxygen flow rate to form a silicon dioxide film mask on the back side; Step 5: back phosphorus diffusion; Step six, cleaning, passivation treatment, screen printing and high-temperature sintering are carried out in sequence.

2. The method for preparing a TOPCon solar cell according to claim 1, characterized in that: In step 2, LPCVD equipment is used to introduce oxygen under normal pressure and react at a temperature of 600-620°C for 950-1200s to form a first tunneling oxide layer on the surface of the silicon substrate. Subsequently, a barrier polysilicon layer is deposited on the surface of the first tunneling oxide layer at a low pressure of 200-300mtorr and a temperature of 590-630°C for 200-400s.

3. The method for preparing a TOPCon solar cell according to claim 1 or 2, characterized in that: The thickness of the first tunneling oxide layer is 1-1.5 nm, and the thickness of the blocking polysilicon layer is 20-40 nm.

4. The method for preparing a TOPCon solar cell according to claim 1, characterized in that: In step three, LPCVD equipment is used to introduce oxygen under normal pressure and react at a temperature of 590-630°C for 200-400 seconds to form a second tunneling oxide layer on the surface of the silicon substrate. Subsequently, a doped polysilicon layer is deposited on the surface of the second tunneling oxide layer at a low pressure of 200-300 mtorr and a temperature of 590-630°C for 1000-1400 seconds.

5. The method for preparing a TOPCon solar cell according to claim 1 or 4, characterized in that: The thickness of the second tunneling oxide layer is 0.3-0.5 nm, and the thickness of the doped polysilicon layer is 100-130 nm.

6. The method for preparing a TOPCon solar cell according to claim 1, characterized in that: In step 4, a low-pressure diffusion deposition device is used, an oxygen flow rate of 1100 to 1400 sccm is used, and the reaction time is 200 to 300 seconds to form a silicon dioxide masking film.

7. The method for preparing a TOPCon solar cell according to claim 1, characterized in that: In step five, POCl3 is used for phosphorus diffusion, first low-temperature deposition, then staged advancement, POCl3 is used again for source diffusion, and finally a post-oxidation annealing process is performed.

8. The method for preparing a TOPCon solar cell according to claim 7, characterized in that: In the step five, POCl3 is used for phosphorus diffusion with a flow rate of 1500-1600sccm, and low-temperature deposition is first performed at a deposition temperature of 750-850°C for 900-1200s; then it is advanced in stages, first at a temperature of 860-930°C for 10-20min, and then at a temperature of 800-860°C for 10-20min; then POCl3 is used for source diffusion again with a flow rate of 1500-1600sccm, a deposition temperature of 830-860°C for 120-180s, and finally an oxidation annealing process is performed for 1200-1500s, and the temperature is reduced to 720-750°C.

9. A TOPCon solar cell, characterized in that: The method is prepared according to any one of claims 1 to 8.

10. The TOPCon solar cell according to claim 9, characterized in that: The silicon wafer comprises a P+ diffusion layer, an aluminum oxide passivation layer, a front anti-reflection layer and a front metal electrode, which are sequentially arranged on the front side of the silicon wafer, and a first tunneling oxide layer, a blocking polysilicon layer, a second tunneling oxide layer, a doped polysilicon layer, a back anti-reflection layer and a back metal electrode, which are sequentially arranged on the back side of the silicon wafer; The front metal electrode penetrates the front anti-reflection layer, the aluminum oxide passivation layer and the P+ diffusion layer to form an ohmic contact; the back metal electrode penetrates the back anti-reflection layer and the doped polysilicon layer to form an ohmic contact.

Citation Information

Patent Citations

  • TOPCon battery phosphorus diffusion process

    CN113808927A

  • Diffusion process for improving high sheet resistance uniformity of solar cell

    CN115863156A

  • Tunnel oxide passivation contact solar cell and preparation method thereof

    CN116799073A

  • Solar cell and preparation method thereof

    CN117594699A

  • Battery back surface structure and double-sided TOPCon solar battery

    CN216980577U