Double-layer covalent organic framework composite ion exchange membrane and preparation method thereof
By forming a double-layer covalent organic framework structure on the perfluorosulfonic acid film, the problems of poor ion selectivity and low Coulomb efficiency of the existing film are solved, and higher battery performance and stability are achieved.
Patent Information
- Application Number
- CN202411399932.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing perfluorosulfonic acid film has poor ion selectivity, low Coulombic efficiency, and difficult to effectively block vanadium ions, which limits its application in the field of flow batteries.
Using a double-layer covalent organic frame composite film, the positively charged covalent organic frame amine monomer is adsorbed through the negatively charged perfluorosulfonic acid film, and heated in the aldehyde monomer solution to generate a positively charged ionic co-co. The valent organic frame thin layer structure is then adsorbed negatively charged anionic amine monomer to form a covalent organic frame thin layer structure with double-layer and opposite charges, improving the pore size and proton conduction ability of the membrane.
The balun efficiency, voltage efficiency and capacity retention of the battery are improved, and the vanadium resistance and long-term cycle stability of the membrane are enhanced.
Smart Images

Figure CN118919788A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vanadium battery diaphragms, and in particular to a double-layer covalent organic framework composite ion exchange membrane and a preparation method thereof. Background Art
[0002] As people's demand for energy continues to increase, energy storage equipment plays an increasingly important role in daily life. All-vanadium liquid flow battery is an electrochemical energy storage system that is particularly suitable for long-term, large-scale energy storage. It has the advantages of flexible design, fast response, low cost per kilowatt-hour, recyclable electrolyte, safety and environmental protection, and has gained more and more attention in the energy field.
[0003] The main components of all-vanadium liquid flow batteries include electrolytes, electrodes, and diaphragms. Among them, the diaphragm separates the positive and negative electrolytes and transmits ions, which plays a vital role in the overall performance of all-vanadium liquid flow batteries. At present, most of the ion exchange membranes produced in the industry on a large scale are perfluorosulfonic acid membranes, which have a large number of micellar channels inside, thereby achieving efficient ion exchange and conduction. However, the size of these channels is in the range of several nanometers, which is larger than the size of most ions. Therefore, there are problems such as poor ion selectivity and low coulombic efficiency, and effective modification methods are needed to improve their overall performance.
[0004] Covalent organic framework is a new type of crystalline organic porous polymer material with highly regular pores and periodic structure. It has the characteristics of nanoscale pore size and continuous adjustable, easy functional modification, good chemical stability, etc., and has begun to emerge in the field of separation membranes. However, although the pore size of common two-dimensional covalent organic frameworks is smaller than the micellar channel of perfluorosulfonic acid membrane, most of them are still above 1nm, which is still too large compared to the hydration diameter of vanadium ions. Therefore, it is difficult to achieve effective vanadium ion isolation with a single-layer covalent organic framework film, which hinders its application in the field of liquid flow batteries. Summary of the invention
[0005] The present invention provides a double-layer covalent organic framework composite ion exchange membrane and a preparation method thereof, and prepares a perfluorosulfonic acid ion exchange composite membrane having a double-layer, oppositely charged covalent organic framework thin layer structure. Specifically, a negatively charged perfluorosulfonic acid membrane is used to adsorb a positively charged cationic covalent organic framework amine monomer, and the adsorbed membrane is heated in an aldehyde monomer solution to react to generate a positively charged ionic covalent organic framework thin layer structure. Then, the positive charge of the positively charged covalent organic framework on its surface is used to adsorb a negatively charged anionic amine monomer containing a sulfonic acid group, and after adsorption, the membrane is heated in an aldehyde monomer solution to react to generate a negatively charged ionic covalent organic framework thin layer structure, and finally a three-layer membrane structure of a perfluorosulfonic acid membrane-a positively charged covalent organic framework-a negatively charged covalent organic framework is obtained, that is, a perfluorosulfonic acid ion exchange composite membrane having a double-layer, oppositely charged covalent organic framework thin layer structure. The modified composite ion exchange composite membrane with a double-layer covalent organic framework structure has nanoscale effective pore size and abundant proton conductive groups, thereby improving the coulombic efficiency, voltage efficiency and capacity retention rate of the battery.
[0006] To achieve the above object, the present invention provides the following technical solutions: A method for preparing a double-layer covalent organic framework composite ion exchange membrane comprises the following steps: S1. Dissolving a positively charged amine monomer and a negatively charged amine monomer containing a sulfonic acid group in a solvent, respectively, to prepare a positively charged amine monomer solution and a negatively charged amine monomer solution containing a sulfonic acid group with the same mass fraction of 3 to 15%; dissolving an aldehyde monomer in a solvent, to prepare an aldehyde monomer solution with a mass fraction of 2 to 10%; S2, soaking 0.1-1 parts by weight of the finished perfluorosulfonic acid membrane in 50-200 parts by weight of a positively charged amine monomer solution for 10-30 minutes, taking it out and rinsing it with a solvent, then putting it into 75-300 parts by weight of an aldehyde monomer solution, adding 0.1-1 parts by weight of a catalyst, heating it at 50-75°C for 1-3 hours, and rinsing it with a solvent after the reaction is completed; S3. Soak the membrane in S2 in 75-300 parts by weight of a negatively charged amine monomer solution containing a sulfonic acid group for 30-60 minutes, take it out and rinse it with a solvent, then put it into a solution of 25-100 parts by weight of an aldehyde monomer, add 0.5-2 parts by weight of a catalyst, heat it at 50-75°C for 4-12 hours, rinse it with a solvent after the reaction is completed, and dry it at 60-90°C for 1-3 hours to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
[0007] Preferably, the positively charged amine monomer in step S1 is selected from one of triaminoguanidine hydrochloride, ethidium bromide, phenanthridinium bromide, 2,5-diamino-3-trimethylaminomethoxypyridine hydrochloride and 1,1'-bis(2,4-dinitrophenyl)-4,4'-dichlorobipyridinium.
[0008] Preferably, the negatively charged amine monomer containing a sulfonic acid group in step S1 is selected from one of 2,5-diaminobenzenesulfonic acid, 2,5-diaminophenyl-1,3-disulfonic acid, 2,5-diamino-1,4-benzenedisulfonic acid and 2,2'-benzidine disulfonic acid.
[0009] Preferably, the aldehyde monomer in step S1 is selected from one of trialdehyde phloroglucinol, 2,4,6-tribenzaldehyde-pyridine, 2,4,6-trialdehyde pyran, 2,4,6-trialdehyde-1,3,5-trihydroxypyran and 2,4,6-trialdehyde-1,3,5-triazine.
[0010] Preferably, the solvent is selected from one of methanol, ethanol, mesitylene, dioxane and N-methylpyrrolidone, and the solvent in step S1, step S2 and step S3 is the same.
[0011] Preferably, the catalyst in step S2 and step S3 is selected from one of acetic acid, n-octanoic acid, trichloroacetic acid and scandium trifluoromethanesulfonate.
[0012] A double-layer covalent organic framework composite ion exchange membrane is prepared by adopting the above-mentioned preparation method of a double-layer covalent organic framework composite ion exchange membrane.
[0013] The beneficial effects of the present invention are: 1. The covalent organic framework double-layer structure on the surface of the perfluorosulfonic acid membrane of the present invention reduces the effective screening aperture through the staggered arrangement of the pores, thereby improving the vanadium resistance of the composite membrane and the coulombic efficiency of the vanadium battery; 2. The covalent organic framework thin layer rich in sulfonic acid groups on the surface of the composite membrane of the present invention can improve the proton conductivity of the membrane, thereby improving the voltage efficiency of the vanadium battery; 3. The two layers of two-dimensional covalent organic frameworks with opposite charge properties in the composite membrane prepared by the present invention are tightly combined with the perfluorosulfonic acid membrane through charge attraction, thereby improving the long-term cycle stability of the membrane and the capacity retention rate of the vanadium battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a schematic diagram of the structure of a double-layer covalent organic framework composite ion exchange membrane of the present invention; Figure 2 The powder X-ray diffraction (PXRD) pattern of the covalent organic framework composite film in Example 1 of the present invention; Figure 3The scanning electron microscope (SEM) images of the single-layer composite membrane in step S2 and the double-layer composite membrane in step S3 in Example 2 of the present invention are shown. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0016] A method for preparing a double-layer covalent organic framework composite ion exchange membrane comprises the following steps: S1. Dissolve the positively charged amine monomer and the negatively charged amine monomer containing a sulfonic acid group in a solvent to prepare a positively charged amine monomer solution and a negatively charged amine monomer solution containing a sulfonic acid group with the same mass fraction of 3 to 15%; dissolve the aldehyde monomer in a solvent to prepare an aldehyde monomer solution with a mass fraction of 2 to 10%; the positively charged amine monomer is selected from one of triaminoguanidine hydrochloride, ethidium bromide, methylphenanthridinium bromide, 2,5-diamino-3-trimethylaminomethoxypyridine hydrochloride and 1,1'-bis(2,4-dinitrophenyl)-4,4'-dichlorobipyridinium. ; The negatively charged amine monomer containing a sulfonic acid group is selected from one of 2,5-diaminobenzenesulfonic acid, 2,5-diaminophenyl-1,3-disulfonic acid, 2,5-diamino-1,4-benzenedisulfonic acid and 2,2'-benzidinedisulfonic acid; the aldehyde monomer is selected from one of trialdehyde phloroglucinol, 2,4,6-tribenzaldehyde-pyridine, 2,4,6-trialdehyde pyran, 2,4,6-trialdehyde-1,3,5-trihydroxypyran and 2,4,6-trialdehyde-1,3,5-triazine; the solvent is selected from one of methanol, ethanol, mesitylene, dioxane and N-methylpyrrolidone; S2, soak 0.1-1 parts by weight of the finished perfluorosulfonic acid membrane in 50-200 parts by weight of a positively charged amine monomer solution for 10-30 minutes, take it out and rinse it with a solvent, then put it into 75-300 parts by weight of an aldehyde monomer solution, add 0.1-1 parts by weight of a catalyst, heat it at 50-75°C for 1-3 hours, and rinse it with a solvent after the reaction is completed; the solvent is selected from one of methanol, ethanol, mesitylene, dioxane and N-methylpyrrolidone, and it is the same as that in S1; S3. Soak the membrane in S2 in 75-300 parts by weight of a negatively charged amine monomer solution containing a sulfonic acid group for 30-60 minutes, take it out and rinse it with a solvent, then put it into a solution of 25-100 parts by weight of an aldehyde monomer, add 0.5-2 parts by weight of a catalyst, heat it at 50-75°C for 4-12 hours, rinse it with a solvent after the reaction is completed, and dry it at 60-90°C for 1-3 hours to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure; the catalyst is selected from one of acetic acid, n-octanoic acid, trichloroacetic acid and scandium trifluoromethanesulfonate; the solvent is selected from one of methanol, ethanol, mesitylene, dioxane and N-methylpyrrolidone, and it is the same as that in S1 and S2.
[0017] Embodiment 1: comprises the following steps: S1. Dissolve triaminoguanidine hydrochloride and 2,5-diaminobenzenesulfonic acid in methanol to prepare 3% triaminoguanidine hydrochloride solution and 3% 2,5-diaminobenzenesulfonic acid solution respectively. Dissolve trialdehyde phloroglucinol in methanol to prepare 2% trialdehyde phloroglucinol solution; S2, soak 0.1g of the finished perfluorosulfonic acid membrane in 50g of triaminoguanidine hydrochloride solution for 10min, take it out and rinse it with methanol. Then, put it into 75g of trialdehyde phloroglucinol solution, add 0.1g of acetic acid and heat it at 50℃ for 3h. Rinse it with methanol after the reaction is completed; S3, soak the membrane in S2 in 75g of 2,5-diaminobenzenesulfonic acid solution for 30min. Take it out and rinse it with methanol. Then, put it into 25g of trialdehyde phloroglucinol solution, add 0.5g of acetic acid, and heat it at 50℃ for 4h. After the reaction, rinse it with methanol and dry it at 60℃ for 1h to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
[0018] Embodiment 2: comprises the following steps: S1. Dissolve ethidium bromide and 2,5-diaminophenyl-1,3-disulfonic acid in ethanol to prepare 6% ethidium bromide solution and 6% 2,5-diaminophenyl-1,3-disulfonic acid solution respectively. Dissolve 2,4,6-tribenzaldehyde-pyridine in ethanol to prepare 4% 2,4,6-tribenzaldehyde-pyridine solution; S2. Soak 0.5g of the finished perfluorosulfonic acid membrane in 100g of ethidium bromide solution for 15min, take it out and rinse it with ethanol. Then, put it into 150g of 2,4,6-tribenzaldehyde-pyridine solution, add 0.3g of n-octanoic acid and heat it at 55℃ for 2.5h. Rinse it with ethanol after the reaction is completed; S3, soak the membrane in S2 in 150g of 2,5-diaminophenyl-1,3-disulfonic acid solution for 40min. Take it out and rinse it with ethanol. Then, put it into 50g of 2,4,6-tribenzaldehyde-pyridine solution, add 1g of n-octanoic acid, and heat it at 55℃ for 6h. After the reaction, rinse it with ethanol and dry it at 70℃ for 1.5h to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
[0019] Embodiment 3: comprises the following steps: S1. Dissolve phenanthroline bromide and 2,5-diamino-1,4-benzenedisulfonic acid in mesitylene to prepare phenanthroline bromide solution with a mass fraction of 9% and 2,5-diamino-1,4-benzenedisulfonic acid solution with a mass fraction of 2,5-diamino-1,4-benzenedisulfonic acid respectively. Dissolve 2,4,6-trialdehyde pyran in mesitylene to prepare 2,4,6-trialdehyde pyran solution with a mass fraction of 6%; S2, soak 1g of the finished perfluorosulfonic acid membrane in 150g of bromophenanthridine solution for 30min, take it out and rinse it with mesitylene. Then, put it into 225g of 2,4,6-trialdehyde pyran solution, add 0.5g of trichloroacetic acid and heat it at 60℃ for 2h. After the reaction is completed, rinse it with mesitylene; S3, soak the membrane in S2 in 225g of 2,5-diamino-1,4-benzenedisulfonic acid solution for 45min. Take it out and rinse it with mesitylene. Then, put it into 75g of 2,4,6-trialdehyde pyran solution, add 1.5g of trichloroacetic acid, and heat it at 60℃ for 8h. After the reaction, rinse it with mesitylene and dry it at 80℃ for 2h to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
[0020] Embodiment 4: comprises the following steps: S1. Dissolve 2,5-diamino-3-trimethylaminomethoxypyridine hydrochloride and 2,2'-benzidine disulfonic acid in dioxane to prepare 12% 2,5-diamino-3-trimethylaminomethoxypyridine hydrochloride solution and 12% 2,2'-benzidine disulfonic acid solution. Dissolve 2,4,6-trialdehyde-1,3,5-trihydroxypyran in dioxane to prepare 8% 2,4,6-trialdehyde-1,3,5-trihydroxypyran solution; S2. Soak 1g of the finished perfluorosulfonic acid membrane in 200g of 2,5-diamino-3-trimethylaminomethoxypyridine hydrochloride solution for 25 minutes, take it out and rinse it with dioxane. Then, put it into 300g of 2,4,6-trialdehyde-1,3,5-trihydroxypyran solution, add 0.8g of scandium trifluoromethanesulfonate and heat it at 65°C for 1.5h. Rinse it with dioxane after the reaction is completed; S3, soak the membrane in S2 in 300g of 2,2'-benzidine disulfonic acid solution for 50min. Take it out and rinse it with dioxane. Then, put it into 100g of 2,4,6-trialdehyde-1,3,5-trihydroxypyran solution, add 2g of scandium trifluoromethanesulfonate, and heat it at 65℃ for 10h. After the reaction, rinse it with dioxane and dry it at 85℃ for 2.5h to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
[0021] Embodiment 5: comprises the following steps: S1. Dissolve 1,1'-bis(2,4-dinitrophenyl)-4,4'-dichlorobipyridyl and 2,5-diaminobenzenesulfonic acid in N-methylpyrrolidone to prepare 15% 1,1'-bis(2,4-dinitrophenyl)-4,4'-dichlorobipyridyl solution and 15% 2,5-diaminobenzenesulfonic acid solution. Dissolve 2,4,6-trialdehyde-1,3,5-triazine in N-methylpyrrolidone to prepare a 10% solution. S2. Soak 0.7g of the finished perfluorosulfonic acid membrane in 150g of 1,1'-bis(2,4-dinitrophenyl)-4,4'-dichlorobipyridinium solution for 20min, take it out and rinse it with N-methylpyrrolidone. Then, put it into 225g of 2,4,6-trialdehyde-1,3,5-triazine solution, add 1g of acetic acid and heat it at 75℃ for 1h. After the reaction, rinse it with N-methylpyrrolidone; S3, soak the membrane in S2 in 225g of 2,5-diaminobenzenesulfonic acid solution for 60min. Take it out and rinse it with N-methylpyrrolidone. Then, put it into 80g of 2,4,6-trialdehyde-1,3,5-triazine solution, add 1.5g of acetic acid, and heat it at 75℃ for 12h. After the reaction, rinse it with N-methylpyrrolidone and dry it at 90℃ for 3h to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
[0022] Comparative Example 1: The perfluorosulfonic acid membrane was placed in methanol, 0.1 g of acetic acid was added, and the mixture was heated at 50° C. for 7 h. The membrane was removed and rinsed with methanol, and dried at 60° C. for 1 h to obtain a blank control.
[0023] Comparative Example 2: Step S3 in Example 2 is omitted, that is, a composite ion exchange membrane with a single-layer covalent organic framework structure is prepared.
[0024] 1. Characterization of the structural regularity of the composite membrane: The composite membrane in Example 1 was immersed in N,N-dimethylformamide to dissolve the lower perfluorosulfonic acid membrane layer, and the upper double-layer covalent organic framework layer was collected and washed with ethanol and pure water, dried, and then characterized by powder X-ray diffraction (PXRD) at an angle of 2 to 40°. The test results are as follows: Figure 2 shown.
[0025] 2. Proton conductivity determination: The porous membranes prepared in Examples 1-5 and Comparative Examples 1-3 were tested for proton conductivity using an electrochemical workstation. The membrane was cut into a fixed size (1.2 cm × 1.2 cm), and after recording the thickness, it was placed in a fixture and two silver sheets were pressed on both sides of the membrane. Four electrodes were clamped on the exposed ends of the silver sheet, and the electrodes were connected to the electrochemical workstation. The voltage value was the open circuit voltage, and the frequency range was 100 kHz to 100 Hz. The proton conductivity σ can be calculated using the following formula: σ = L / (R × S) Wherein: R is the resistance of proton conduction; L is the distance between platinum wires; S is the product of the thickness and surface area of the membrane. The test results are shown in Table 1.
[0026] 3. Microscopic morphology characterization: The single-layer composite film of step S2 and the double-layer composite film of step S3 in Example 2 were respectively characterized by cold field emission scanning electron microscopy (SEM). Before the characterization, the samples were subjected to gold spraying treatment to enhance the conductivity for 40 seconds. The characterization results are shown in FIG. Figure 3 shown.
[0027] 4. Battery performance test: The membranes in Examples 1-5 and Comparative Examples 1-2 were assembled into battery stacks for testing, and the coulombic efficiency, voltage efficiency, energy efficiency, and capacity retention after 300 cycles were tested and recorded under the same operating conditions. The test results are shown in Table 1.
[0028] Table 1 Proton conductivity measurement and battery performance test results
[0029] The structure and mechanism of action of the perfluorosulfonic acid composite membrane with double-layer, oppositely charged covalent organic framework thin layer in Examples 1-5 are as follows Figure 1 shown.
[0030] like Figure 2As shown, the PXRD spectrum of the composite film in Example 1 simultaneously shows characteristic peaks of each covalent organic framework in the double-layer structure, and their positions are 4.7°, 10° and 27°, respectively. The peaks at 4.7° and 10° correspond to the (100) crystal planes of the outer and inner covalent organic frameworks, respectively, and the peak at 27° corresponds to the (001) crystal planes of the two layers. Figure 3 As shown, the single-layer composite film of step S2 and the double-layer composite film of step S3 in Example 2 both have defect-free surface morphology. The above two points together indicate that a composite film with a double-layer covalent organic framework structure is successfully prepared, and each layer has good crystallinity and structural regularity, laying a foundation for strengthening the performance of the composite film.
[0031] As can be seen from Table 1, the coulombic efficiency of the composite ion exchange membrane with a single-layer covalent organic framework structure in Comparative Example 2 is slightly improved by about 1% compared with the blank control of Comparative Example 1, but the improvement is far less than that of the composite membrane with a double-layer covalent organic framework structure in Examples 1-5, which can reach 2.4% to 3%. This shows that the covalent organic framework double-layer structure on the surface of the composite membrane prepared by the present invention reduces the effective screening pore size through the staggered arrangement of pores, thereby improving the vanadium resistance of the composite membrane and the coulombic efficiency of the battery.
[0032] The outermost negatively charged covalent organic framework thin layer on the surface of the composite membrane in Examples 1-5 is prepared by selecting a monomer having a sulfonic acid group, so the surface of the composite membrane is rich in proton conductive groups, and has higher proton conductivity and voltage efficiency than the blank membrane in Comparative Example 1; while the covalent organic framework layer on the surface of the composite membrane with a single-layer structure in Comparative Example 2 does not have similar conductive groups, and it covers the sulfonic acid groups of the perfluorosulfonic acid membrane itself, resulting in a decrease in the proton conductivity of the membrane and the battery voltage efficiency. This shows that the covalent organic framework thin layer rich in sulfonic acid groups on the surface of the composite membrane of the present invention can improve the proton conductivity of the membrane, thereby improving the voltage efficiency of the battery.
[0033] After 300 cycles of continuous operation, the capacity retention rates of the double-layer composite membranes in Examples 1-5 were all above 80%, which were significantly higher than those of the blank membrane in Comparative Example 1 and the single-layer composite membrane in Comparative Example 2. This indicates that the two layers of the two-dimensional covalent organic framework with opposite charge properties in the composite membrane prepared by the present invention are tightly combined with the perfluorosulfonic acid membrane through charge attraction, thereby improving the long-term cycle stability of the membrane and the capacity retention rate of the battery.
[0034] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a double-layer covalent organic framework composite ion exchange membrane, characterized in that: The steps include: S1. Dissolving a positively charged amine monomer and a negatively charged amine monomer containing a sulfonic acid group in a solvent respectively, and preparing a positively charged amine monomer solution and a negatively charged amine monomer solution containing a sulfonic acid group with the same mass fraction of 3 to 15% respectively; Dissolving the aldehyde monomer in a solvent to prepare an aldehyde monomer solution with a mass fraction of 2 to 10%; S2, soaking 0.1-1 parts by weight of the finished perfluorosulfonic acid membrane in 50-200 parts by weight of a positively charged amine monomer solution for 10-30 minutes, taking it out and rinsing it with a solvent, then putting it into 75-300 parts by weight of an aldehyde monomer solution, adding 0.1-1 parts by weight of a catalyst, heating it at 50-75°C for 1-3 hours, and rinsing it with a solvent after the reaction is completed; S3. Soak the membrane in S2 in 75-300 parts by weight of a negatively charged amine monomer solution containing a sulfonic acid group for 30-60 minutes, take it out and rinse it with a solvent, then put it into a solution of 25-100 parts by weight of an aldehyde monomer, add 0.5-2 parts by weight of a catalyst, heat it at 50-75°C for 4-12 hours, rinse it with a solvent after the reaction is completed, and dry it at 60-90°C for 1-3 hours to obtain a perfluorosulfonic acid composite membrane with a double-layer, oppositely charged covalent organic framework thin layer structure.
2. The method for preparing a double-layer covalent organic framework composite ion exchange membrane according to claim 1, characterized in that: In the step S1, the positively charged amine monomer is selected from one of triaminoguanidine hydrochloride, ethidium bromide, phenanthridinium bromide, 2,5-diamino-3-trimethylaminomethoxypyridine hydrochloride and 1,1'-bis(2,4-dinitrophenyl)-4,4'-dichlorobipyridinium.
3. The method for preparing a double-layer covalent organic framework composite ion exchange membrane according to claim 1, characterized in that: In the step S1, the negatively charged amine monomer containing a sulfonic acid group is selected from one of 2,5-diaminobenzenesulfonic acid, 2,5-diaminophenyl-1,3-disulfonic acid, 2,5-diamino-1,4-benzenedisulfonic acid and 2,2'-benzidine disulfonic acid.
4. The method for preparing a double-layer covalent organic framework composite ion exchange membrane according to claim 1, characterized in that: In the step S1, the aldehyde monomer is selected from one of trialdehyde phloroglucinol, 2,4,6-tribenzaldehyde-pyridine, 2,4,6-trialdehyde pyran, 2,4,6-trialdehyde-1,3,5-trihydroxypyran and 2,4,6-trialdehyde-1,3,5-triazine.
5. The method for preparing a double-layer covalent organic framework composite ion exchange membrane according to claim 1, characterized in that: The solvent is selected from one of methanol, ethanol, mesitylene, dioxane and N-methylpyrrolidone, and the solvent in step S1, step S2 and step S3 is the same.
6. The method for preparing a double-layer covalent organic framework composite ion exchange membrane according to claim 1, characterized in that: In step S2 and step S3, the catalyst is selected from one of acetic acid, n-octanoic acid, trichloroacetic acid and scandium trifluoromethanesulfonate.
7. A double-layer covalent organic framework composite ion exchange membrane, characterized in that: The composite ion exchange membrane is prepared by the preparation method of a double-layer covalent organic framework composite ion exchange membrane according to any one of claims 1 to 6.
Citation Information
Patent Citations
Ion screening flow battery diaphragm with functional polymer / covalent organic framework interpenetrating shrinkage cavity structure
CN114725418A
Covalent organic framework double-layer positively charged nanofiltration membrane as well as preparation method and application thereof
CN116078192A
Ionic covalent organic framework functionalized modified diaphragm as well as preparation and application thereof
CN116169425A
Preparation method of cationic covalent organic framework modified battery diaphragm
CN118380720A
Covalent organic framework modified high-ion-selectivity permeable membrane as well as preparation method and application thereof
CN118634653A
Cited By
Multistage asymmetric covalent organic framework film and preparation method and application thereof
CN119869241A
Covalent organic framework-polymer hybrid porous membrane as well as preparation method and application thereof
CN120878879A
Covalent organic framework composite membrane as well as preparation method and application thereof
CN120895674A
A covalent organic framework composite membrane and a preparation method and application thereof
CN120895674B