Semiconductor device and method of manufacturing the same
By using a multi-step bias power scheme during magnetron sputtering to form TiN electrodes with varying density and high-k dielectric layers, the interfacial mixing and diffusion problems of metal-insulator metal capacitors are solved, thereby improving the reliability and performance of semiconductor devices.
Patent Information
- Application Number
- CN202410922485.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-13
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
Existing metal-insulator metal capacitors suffer from interfacial mixing and cross-diffusion problems during semiconductor manufacturing, which affect the reliability and performance of the device.
A multi-step bias power scheme is adopted to control the variation of bias power during magnetron sputtering, forming TiN electrodes with varying density and high-k dielectric layers, thereby reducing interface mixing and diffusion.
This improves the reliability and performance of MIM capacitors, reduces the possibility of interface mixing and diffusion, and enhances the consistency of mechanical and electrical properties.
Smart Images

Figure CN118922062A_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present disclosure are generally directed to a semiconductor device and a method for manufacturing the same. Background Art
[0002] Semiconductor devices are used in a wide variety of electronic applications, such as personal computers, cell phones, digital cameras, and other electronic devices. Semiconductor devices are typically manufactured by sequentially depositing insulating or dielectric layers, conductive layers, and semiconducting layers of material on a semiconductor substrate and using lithography to pattern the various material layers to form circuit components and elements on the semiconductor device.
[0003] The semiconductor industry continues to improve the integration density of various electronic components (such as transistors, diodes, resistors, capacitors, etc.) by continuously reducing the minimum feature size, thereby allowing more components to be integrated into a given area. However, as the minimum feature size decreases, additional problems that need to be solved also arise.
[0004] One type of capacitor is a metal-insulator-metal (MIM) capacitor, which has been widely used in mixed signal devices and logic circuits, such as embedded memory and radio frequency devices. Metal-insulator-metal capacitors are used to store charge in various semiconductor devices. Metal-insulator-metal capacitors are formed horizontally on a semiconductor wafer, where two metal plates or electrodes sandwich a dielectric layer parallel to the wafer surface. However, MIM capacitors still have many challenges. Summary of the invention
[0005] The present disclosure provides a method for manufacturing a semiconductor device, the method comprising: forming a first electrode above a substrate, the first electrode having a variable density, the variable density increasing from a first density level at a bottom surface of the first electrode to a second density level, the second density level at a top surface of the first electrode being higher than the first density level; forming a high-K dielectric layer above the first electrode; and forming a second electrode above the high-K dielectric layer, the high-K dielectric layer having a variable density, the variable density increasing from a third density level at a bottom surface of the second electrode bonded to the high-K dielectric layer to a fourth density level, the fourth density level at the top surface of the second electrode being higher than the third density level.
[0006] The present disclosure provides a semiconductor device, comprising: a substrate; a first titanium nitride electrode formed over the substrate, the first titanium nitride electrode having a variable density, the variable density increasing from a first density level at a bottom surface of the first titanium nitride electrode to a second density level, the second density level at a top surface of the first titanium nitride electrode being higher than the first density level; a high-K dielectric layer formed over the first titanium nitride electrode; and a second titanium nitride electrode over the high-K dielectric layer, the variable density increasing from a third density level at a bottom surface of the second titanium nitride electrode bonded to the high-K dielectric layer to a fourth density level, the fourth density level at a top surface of the second titanium nitride electrode being higher than the third density level.
[0007] The present disclosure provides a method for manufacturing a semiconductor device, the method comprising: depositing a first titanium nitride electrode over a substrate by a plasma-based physical vapor deposition technique using a power source to cause magnetron sputtering, wherein the first titanium nitride electrode has a variable density, the variable density increases from a first density level at a bottom surface of the first titanium nitride electrode to a second density level, the second density level at a middle region within the first titanium nitride electrode is higher than the first density level, and increases to a third density level, the third density level at a top surface of the first titanium nitride electrode is higher than the second density level; forming a high-K dielectric layer over the first titanium nitride electrode; and depositing a second titanium nitride electrode over the high-K dielectric layer. A second titanium nitride electrode is deposited by magnetron sputtering, wherein the second titanium nitride electrode has a varying density that increases from a first density level at a bottom surface of the second titanium nitride electrode bonded to a high-K dielectric layer to a second density level, the second density level at an intermediate region within the second titanium nitride electrode being higher than the first density level, and to a third density level, the third density level at a top surface of the second titanium nitride electrode being higher than the second density level; wherein the magnetron sputtering includes systematically increasing a bias power using a bias power schedule to bombard a target material to sputter atoms of the target material, the bias power schedule causing the bias power to increase from a first power level that is high enough to cause sputtering to a higher power level that results in a desired sputtering yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] When with Figure 1 When read together, various aspects of the present disclosure can be best understood from the following detailed description. It is worth noting that, in accordance with standard industry practices, various features are not drawn to scale. In fact, the size of various features can be arbitrarily increased or reduced for clarity of discussion.
[0009] Figure 1 is a schematic diagram illustrating an example portion of a semiconductor device according to various embodiments;
[0010] Figure 2Ais a block diagram illustrating an example process chamber for fabricating an example MIM capacitor according to various embodiments;
[0011] Figure 2B is a cross-sectional view of an example MIM capacitor electrode formed using a multi-step biasing scheme according to various embodiments;
[0012] FIG. 3A to FIG. 3C is a schematic diagram illustrating various bias power schemes that may be applied by a power supply in a process chamber to cause magnetron sputtering to increase sputtering yield according to various embodiments;
[0013] Figure 4 is a schematic diagram illustrating example crystal ratios determined using X-ray diffraction analysis (XRD) on a TiN electrode formed using a single-step biasing power scheme and on a TiN electrode formed using a multi-step biasing power scheme, according to various embodiments;
[0014] Figure 5 is a schematic diagram illustrating an example time dependent dielectric breakdown (TDDB) test result of a capacitor electrode formed using a single-step bias power scheme and a capacitor electrode formed using a multi-step bias power scheme according to some embodiments;
[0015] Figure 6 is a process flow diagram illustrating an example process for forming a MIM capacitor using a multi-step bias power scheme according to some embodiments;
[0016] 7A to 7D FIG. 5 is a cross-sectional view of a semiconductor device at various fabrication stages according to some embodiments.
[0017]
Explanation of symbols
[0018] 100:Semiconductor device
[0019] 102: Base material
[0020] 104: Interconnection structure
[0021] 106,108,110: Insulation layer
[0022] 112,114,116:IMD layer
[0023] 118:Metal Wire
[0024] 120:Through hole
[0025] 122:MIM capacitor
[0026] 124: Insulation layer
[0027] 126:CBM layer
[0028] 128:CTM layer
[0029] 200: Process chamber
[0030] 202: substrate carrier
[0031] 204: Base material
[0032] 206: Anode
[0033] 208: cathode
[0034] 210:Magnet array
[0035] 212: Target raw materials
[0036] 214: High Density Plasma
[0037] 216: Plasma
[0038] 218: Inert gas source
[0039] 220: Ion
[0040] 222: Particles
[0041] 224: Membrane
[0042] 228: Magnetic Field
[0043] 230: Electrode
[0044] 232,234,236,238,240: Area
[0045] 304,306: Bias power
[0046] 502,504,506,508:TDDB value
[0047] 600: Craftsmanship
[0048] 610,620,630,640,650: Blocks
[0049] 701,707: Bottom surface
[0050] 702: Pre-MIM layer
[0051] 703,709: Middle area
[0052] 704,708: Electrode
[0053] 705,711: Top surface
[0054] 706: High K dielectric layer
[0055] DC: Direct current
[0056] θ: angle DETAILED DESCRIPTION
[0057] The following disclosure provides many different embodiments or examples for implementing the different features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the disclosure. Of course, these are merely examples and are not intended to be limiting.
[0058] For the sake of brevity, conventional techniques related to the manufacture of conventional semiconductor devices are not described in detail herein. In addition, the various operations and processes described herein may be incorporated into a more comprehensive procedure or process having additional functions not described in detail herein. Specifically, the various processes in the manufacture of semiconductor devices are well known, and therefore, for the sake of brevity, many conventional processes will be only briefly mentioned or omitted entirely herein without providing conventional process details. It will be readily understood by those skilled in the art after reading this disclosure in its entirety that the structures disclosed herein may be used with a variety of technologies and may be incorporated into a variety of semiconductor devices and products. It should also be noted that the semiconductor device structure includes a variable number of elements, and that a single element shown in the figure may represent a plurality of elements.
[0059] In addition, spatially relative terms, such as "on," "above," "above," "above," "top," "below," "below," "below," "below," "bottom," and the like, are used to facilitate describing the relationship between one element or component and another (or some) elements or components, as illustrated in the accompanying drawings. Spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the drawings. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used herein may be interpreted accordingly. When a spatially relative term (such as the spatially relative terms listed above) is used to describe a first element relative to a second element, the first element may be directly above the other element, or there may be multiple elements or multiple layers between the two.
[0060] In addition, the disclosure may repeat reference numerals and / or letters in various examples. Such repetition is for the purpose of simplicity and clarity and does not in itself limit the relationship between the various embodiments and / or configurations discussed.
[0061] It is worth noting that references in the specification to "one embodiment", "an embodiment", "example embodiment", "exemplary", "example", etc., indicate that the described embodiment may include certain features, structures, or characteristics, but not every embodiment necessarily includes certain features, structures, or characteristics. In addition, such terms do not necessarily refer to the same embodiment. In addition, when a certain feature, structure, or characteristic is described in conjunction with an embodiment, whether or not explicitly described, it will be within the knowledge of those skilled in the art to affect such feature, structure, or characteristic in conjunction with other embodiments.
[0062] It should be understood that the phraseology or terminology herein is for the purpose of description rather than limitation, so that those skilled in the relevant art can interpret the phraseology or terminology of the specification according to the teachings herein.
[0063] The following disclosure provides many different embodiments or examples for implementing different features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the disclosure. Of course, these are merely examples and are not intended to be limiting. For example, in the following description, a first feature is formed on or above a second feature, which may include an embodiment in which the first and second features are directly in contact with each other, and may also include an embodiment in which additional features may be formed between the first and second features so that the first and second features may not be in direct contact. Throughout the description herein, unless otherwise stated, the same reference numerals in different figures represent the same or similar components formed using the same or similar materials and by the same or similar methods.
[0064] Figure 1 A cross-sectional view of an example portion of a semiconductor device 100 including a metal-insulator-metal (MIM) capacitor structure is shown according to various embodiments. The example semiconductor device 100 includes a substrate 102 and an interconnect structure 104 .
[0065] The substrate 102 may be a semiconductor substrate, such as a bulk semiconductor, a semiconductor-on-insulator (SOI) substrate, a semiconductor wafer, etc., which may be doped (e.g., using p-type or n-type dopants) or undoped. Other substrates, such as multilayer or gradient substrates, may also be used. In some embodiments, the semiconductor material of the substrate may include silicon; germanium; a compound semiconductor including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; an alloy semiconductor including SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP; or a combination of the foregoing.
[0066] The substrate 102 may include any number of conductive features and device elements formed in and / or above the semiconductor substrate. The conductive features may include, for example, plugs, interconnects, or wiring lines. The device elements may include, for example, transistors, diodes, or capacitors. For example, the transistor may be a metal oxide semiconductor field effect transistor (MOSFET), a complementary metal oxide semiconductor (CMOS) transistor, a bipolar junction transistor (BJT), a high voltage transistor, a high frequency transistor, a p-channel field effect transistor (PFET) and / or an n-channel field effect transistor (NFET), a diode, or other suitable element. The substrate 102 may also include isolation features (not shown), such as shallow trench isolation (STI) features or local oxidation of silicon (LOCOS) features. The isolation features may define and isolate various device elements.
[0067] The interconnect structure 104 provides routing and electrical connections between device elements formed in and / or above the substrate 102. The interconnect structure 104 may include a plurality of insulating layers (in this example, a first insulating layer 106, a second insulating layer 108, and a third insulating layer 110 are shown). The example first insulating layer 106, the second insulating layer 108, and the third insulating layer 110 include a first inter-metal dielectric (IMD) layer 112, a second IMD layer 114, and a third IMD layer 116, respectively, and one or more conductive features, in this example, including metal lines 118 and / or vias 120 formed in a metallization layer. The conductive features may be electrically connected to active and / or passive devices of the substrate 102 through contacts (not shown).
[0068] In some embodiments, the interconnect structure 104 may be formed using a single damascene process and / or a dual damascene process, a via-first process, or a metal-first process. In one embodiment, an insulating layer and an opening (not shown) may be formed therein using acceptable lithography and etching techniques. The first IMD layer 112, the second IMD layer 114, and the third IMD layer 116, for example, may be or include an oxide film, such as silicon oxide, undoped silicon glass (USG), fluorosilicate glass (FSG), boron doped silicate glass (BSG), phosphosilicate glass (PSG), boron phosphorous-doped silicate glass (BPSG), polyethylene oxide (PEOX), thermal oxide, silicon dioxide (SiO2), or other suitable dielectric materials. One or more of IMD layers 112 , 114 , and 116 may be made of a low dielectric constant (low-k) material, such as a dielectric constant less than about 3.0 or less than about 2.5.
[0069] Conductive material for metal lines 118 and / or vias 120 may be formed in the openings in the IMD layer, such as copper (Cu), aluminum (Al), tungsten (W), nickel, cobalt, silver, combinations thereof, or other suitable materials, and may be formed in the openings using electro-chemical plating processes, chemical vapor deposition (CVD), atomic layer deposition (ALD), physical vapor deposition (PVD), or the like, or combinations thereof. After forming the conductive material, a planarization process such as chemical mechanical polishing (CMP) may be used to remove excess conductive material, thereby leaving conductive features in the openings of the insulating layer. This process may then be repeated to form additional insulating layers and conductive features therein. Figure 1The interconnect structure 104 shown in FIG. 1 is for illustration purposes only. The interconnect structure 104 may include other configurations and may include one or more metal lines and IMD layers.
[0070] The example interconnect structure 104 also includes a MIM capacitor 122 formed above the IMD layer and above the substrate 102. The example MIM capacitor 122 has a sandwich structure in which an insulating layer 124 is formed between a capacitor bottom metal (CBM) layer 126 and a capacitor top metal (CTM) layer 128. In various embodiments, the CBM layer 126 and the CTM layer 128 are formed of a metal, such as titanium nitride (TiN), and the insulating layer 124 is formed of a high dielectric constant (high-K) dielectric material (e.g., having a relative dielectric constant greater than about 3). As used and described herein, high-K dielectric materials include dielectric materials having a high dielectric constant, such as a dielectric constant greater than that of thermal silicon oxide (approximately 3.9). The insulating layer 124 may include a high-K dielectric layer such as hafnium oxide (HfO2). Alternatively, the high-K dielectric layer may include other high-K dielectrics, such as TiO2, HfZrO, Ta2O3, HfSiO4, ZrO2, ZrSiO2, LaO, Al2O, ZrO, TiO, Ta2O5, Y2O3, SrTiO3 (STO), BaTiO3 (BTO), BaZrO, HfZrO, HfLaO, HfSiO, LaSiO, AlSiO, HfTaO, HfTiO, (Ba, Sr)TiO3 (BST), Al2O3, Si3N4, oxynitride (SiON), combinations thereof, or other suitable materials. The dielectric layer of the high-K material may be formed by ALD, physical vapor deposition (PVD), CVD, chemical oxidation, thermal oxidation, and / or other suitable methods.
[0071] In various embodiments, the CBM layer 126 and the CTM layer 128 are formed by PVD using magnetron sputtering. Magnetron sputtering is a deposition technique involving a gaseous plasma that is generated and confined in a space containing the material to be deposited ("target"). The surface of this target is eroded by high-energy ions in the plasma, and the released atoms pass through the vacuum environment and are deposited on the substrate to form a thin film. To initiate the generation of the plasma, a high voltage is applied between a cathode (usually located directly behind the sputtering target) and an anode (usually connected to the PVD chamber as an electrical ground). The electrons present in the sputtering gas are accelerated away from the cathode, causing the electrons to collide with nearby sputtering gas atoms. These collisions cause electrostatic repulsion, thereby "knocking off" electrons from the sputtering gas atoms, resulting in ionization. The positively charged sputtering gas atoms are now accelerated toward the negatively charged cathode, resulting in high-energy collisions with the target surface. Each collision causes atoms on the target surface to be ejected into the vacuum environment with sufficient kinetic energy to reach the surface of the substrate.
[0072] During the manufacture of the MIM capacitor, intermixing and interdiffusion between the TiN from the CTM layer 128 and the high-K material from the insulating layer 124 may occur, which may degrade the reliability of the MIM capacitor. Intermixing involves mixing of the TiN and the high-K material at the interface between the two materials during the deposition of the TiN. Such interfacial mixing may damage the high-K layer and cause poor performance of the device. During the use of the device with the high-K and TiN interface, interdiffusion may occur, in which the material becomes hot during use and causes the two materials at the interface between the two materials to diffuse together. In order to reduce the possibility and negative impact of intermixing and interdiffusion at the interface, and to improve the reliability of the MIM capacitor, and to provide the ability to fine-tune the mechanical properties, electrical properties, uniformity and consistency of the TiN electrode (CBM layer 126 and CTM layer 128), a multi-step bias power scheme may be used to form the CBM layer 126 and the CTM layer 128.
[0073] Figure 2A FIG. 2 is a block diagram illustrating an example process chamber 200 for fabricating an example MIM capacitor, according to various embodiments. Figure 2ASpecific details and features that are apparent to those of ordinary skill in the art are omitted. The example process chamber 200 includes a substrate carrier 202, a substrate 204, an anode 206, a cathode 208, a magnet array 210, a target material raw material 212, a high density plasma 214, a plasma 216 generated by neutralization, an inert gas source (e.g., argon) 218, inert gas ions 220, target material particles 222, and a sputtered film 224. The example process chamber 200 is a PVD process chamber. The target material raw material 212 includes titanium (Ti) located in the process chamber 200. The target material raw material 212 provides a source of Ti atoms that combines with nitrogen to form the TiN electrodes (e.g., CBM layer 126 and CTM layer 128) of the MIM capacitor 122. The substrate carrier 202 is also located in the process chamber 200 and can be an electrostatic chuck that provides a platform for the substrate 204. A substrate 204 is positioned on a substrate stage 202 on which a MIM capacitor, such as the MIM capacitor 122, is fabricated. An inert gas line, such as an argon gas line, is positioned in a sidewall of the process chamber to provide an inert gas source 218 that can be used to initiate a sputtering process to remove Ti atoms from the target raw material 212 during the formation of the TiN electrodes (e.g., the CBM layer 126 and the CTM layer 128).
[0074] In one embodiment, the sputtering process begins when a substrate 204 to be coated is placed in a process chamber 200 containing an inert gas (typically argon) and a negative charge 226 is applied to a target raw material 212 to be deposited on the substrate 204, causing the plasma 216 to emit light.
[0075] In the plasma environment, free electrons flow out of the negatively charged target raw material 212 and collide with the outer electron shells of argon atoms, driving these electrons away due to their like charges. The noble gas atoms become positively charged ions 220, which are attracted to the negatively charged target raw material 212 at a very high speed, and "sputter off" atomic-sized particles 222 from the target raw material 212 due to the collision momentum. These particles 222 pass through the process chamber 200 of the gold coating machine (sputtercoater) and are deposited as a thin film 224 of material on the surface of the substrate 204 to be coated.
[0076] The number of atoms ejected or "sputtered off" from the target raw material 212 or raw material is referred to as the sputtering yield. The sputtering yield can be controlled by the energy and angle of incidence of the bombarding ions 220, the relative masses of the ions and target atoms, and the surface binding energy of the target atoms.
[0077] Because ions 220 are charged particles, magnetic field 228 can be used to control their speed and behavior. Magnetron sputtering deposition uses magnets from magnet array 210 behind negative cathode 208 to capture electrons on negatively charged target raw material 212 so that they are not free to bombard substrate 204, thereby allowing faster deposition rates.
[0078] The bias power applied to the process chamber 200, for example in the form of a DC sputtering power supply, an RF sputtering power supply, a pulsed DC sputtering power supply, an MF sputtering power supply, an AC sputtering power supply, a high power impulse magnetron sputtering (HiPIMS) power supply, etc., can be controlled by a bias scheme to control the sputtering yield. Controlling the sputtering yield can allow for multi-step bias adjustment.
[0079] Figure 2B A cross-sectional view of an example electrode 230 (e.g., a TiN electrode) formed using multi-step attunement is depicted. As used herein, multi-step attunement involves forming an electrode (e.g., a TiN electrode) having a varying density that increases from a first density level at the bottom surface of the electrode to a second density level that is higher than the first density level at a mid-region within the electrode, and to a higher density level that is higher than the second density level at the top surface of the electrode. Figure 2B In the example of FIG. 2 , the electrode 230 has five density levels. In other examples, other numbers of density levels can be formed, such as three or more density levels.
[0080] The example electrode 230 has a first region 232 at a first density level, a second region 234 at a second density level higher than the first density level, a third region 236 at a third density level higher than the second density level, a fourth region 238 at a fourth density level higher than the third density level, and a fifth region 240 at a fifth density level higher than the fourth density level. The example electrode 230 can be formed in a PVD process chamber (e.g., process chamber 200) by plasma-based PVD technology. The PVD process chamber uses a power source (e.g., a DC sputtering power source, an RF sputtering power source, a pulsed DC sputtering power source, a medium frequency sputtering power source, an AC sputtering power source, a high power pulsed magnetron sputtering (HiPIMS) power source) to cause magnetron sputtering, and as the magnetron sputtering continues, the sputtering yield increases.
[0081] In this example, during a first period, when the first region 232 is formed, the bias power applied to the magnetron cathode in the process chamber is at a first level. During a second period, when the second region 234 is formed, the bias power applied to the magnetron cathode in the process chamber is at a second level higher than the first level. During a third period, when the third region 236 is formed, the bias power applied to the magnetron cathode in the process chamber is at a third level higher than the second level. During a fourth period, when the fourth region 238 is formed, the bias power applied to the magnetron cathode in the process chamber is at a fourth level higher than the third level. During a fifth period, when the fifth region 240 is formed, the bias power applied to the magnetron cathode in the process chamber is at a fifth level higher than the fourth level.
[0082] In various embodiments, the bias power may range from 0 watts (W) to 250 watts, and the TiN thickness may range from 0 angstroms. In various embodiments, each thickness region may have a constant bias power or a varying bias power.
[0083] FIG. 3A to FIG. 3C A schematic diagram illustrating how varying bias power levels may be applied by a power supply in a process chamber to cause magnetron sputtering and increase sputtering yield. Figure 3A In the example of , applying a bias power scheme in a process chamber includes: applying a step increase 302 to increase the bias power. This may result in forming an electrode having discrete electrode regions, such as the example electrode 230, having a discrete density level that increases as one moves from the bottom of the electrode to the top of the electrode. Although Figure 3A The examples shown show equal voltage levels being increased over equal time increments, but in other examples the amount of power increase may not be equal in magnitude, and in other examples the time increments may not be equal in magnitude.
[0084] exist Figure 3B In the example of , applying a bias power scheme in a process chamber includes increasing the bias power in a linear manner 304. This may result in forming an electrode having a density level that continuously increases as one moves from the bottom of the electrode to the top of the electrode. Figure 3B The examples show that the slope of the voltage level increase is the same at equal time increments, but in other examples, the slope values of the power increase may not be equal in the same time increment, and in other examples, the time increment values may not be equal.
[0085] exist Figure 3CIn an example of , applying a bias power scheme in a process chamber includes exponentially increasing the bias power 306. This may result in forming an electrode having a density level that increases exponentially as one moves from the bottom of the electrode to the top of the electrode.
[0086] Although in FIG. 3A to FIG. 3C In the example of FIG. 1 , the bias power is shown to be increased in a stepwise, linear, or exponential manner, but in other examples, a combination of two or more of the stepwise, linear, or exponential manners may be used to increase the bias power. Other power schemes may also be used to increase the bias power during the formation of TiN, thereby causing the TiN layer to be deposited with varying densities.
[0087] In various embodiments, the bias power scheme can be controlled to achieve desired mechanical properties, desired electrical properties, desired uniform properties, and / or desired consistent properties of the deposited metal layer (e.g., TiN layer). In various embodiments, the bias power scheme can be controlled to achieve desired mechanical properties, such as a desired density. Higher density can produce a stronger metal layer.
[0088] In various embodiments, the bias power scheme can be controlled to achieve other desired mechanical properties, such as desired microstructural changes in the form of roughness, grain size, etc. In one example embodiment using a single-step bias power scheme (e.g., applying a constant bias power in the process chamber to deposit TiN), the grain size of the deposited TiN is 130.2 angstroms. The center roughness is 13.5±0.1 angstroms, and the edge roughness is 11.9±0.1 angstroms. In contrast, the thickness of the TiN layer using a multi-step bias power scheme (e.g., changing the bias power applied in the process chamber multiple times) is equal to the thickness of the TiN layer deposited using a single-step bias power scheme, and the deposited TiN has a grain size of 118.0 angstroms, a center roughness of 13.6±0.2 angstroms, and an edge roughness of 10.8±0.1 angstroms. Smaller grain sizes can be achieved based on multi-step bias. In addition, the desired roughness can be obtained using a multi-step bias power scheme.
[0089] In various embodiments, the bias power scheme can be controlled to achieve other desired microstructural changes. In one example implementation, a TiN layer is deposited on a high-K layer using a multi-step bias, resulting in a (200 / 111) ratio of the deposited TiN that is different from the (200 / 111) ratio of the deposited TiN when deposited using a single-step bias. Figure 4As shown in FIG. 1 , as measured by X-ray diffraction analysis (XRD), the θ-2θ: (200) / (100) ratio of the TiN electrode formed using a single-step bias voltage is greater than 0.2, while the θ-2θ: (200) / (100) ratio of the TiN electrode formed using a multi-step bias voltage is approximately 0.15. Figure 4 As shown in the figure, as determined using X-ray diffraction analysis (XRD), the grazing incidence X-ray diffraction (GIXRD): (200) / (100) ratio is almost twice that of the TiN electrode formed using a single-step bias (ratio of about 2) compared to the TiN electrode formed using a multi-step bias (ratio of about 1). Therefore, the crystal structure of the TiN layer can be changed using a multi-step bias. XRD is a technique used in materials science to determine the crystal structure of a material. XRD works by irradiating a material with incident X-rays and then measuring the intensity and scattering angle of the X-rays that leave the material.
[0090] Using a multi-step bias power scheme to deposit TiN can maintain a stoichiometric TiN composition (e.g., a Ti:N ratio close to 1:1). In one embodiment, depositing a TiN layer on a high-K layer results in an atomic percentage of Ti in the TiN of 51.59% and an atomic percentage of N in the TiN of 48.41% (determined by EDX line scan). When a TiN layer of the same thickness is deposited using a multi-step bias power scheme, depositing a TiN layer on a high-K layer results in an atomic percentage of Ti in the TiN of 51.18% and an atomic percentage of N in the TiN of 48.82% (determined by EDX line scan).
[0091] In various embodiments, the bias power scheme can be controlled to achieve desired electrical characteristics, such as resistivity or plate resistance. In various embodiments, when patterning a metal layer (e.g., a TiN layer), a lower resistivity or plate resistance can be achieved by applying a higher bias power in the process chamber. A lower bias power can be applied at the lower layers of the metal layer to reduce intermixing and / or interdiffusion, while a higher bias power can be applied at the higher layers of the metal layer to reduce the resistivity or plate resistance.
[0092] In various embodiments, the bias power scheme can be controlled to achieve desired consistent characteristics, such as lower or higher sidewall angle magnitudes. In various embodiments, when patterning a metal layer (e.g., a TiN layer), a lower sidewall angle magnitude can be achieved by applying a higher bias power in the process chamber. A lower bias power can be applied at lower layers of the metal layer to reduce intermixing and / or interdiffusion, while a higher bias power can be applied at higher layers of the metal layer to reduce the sidewall angle magnitude.
[0093] In various embodiments, the bias power scheme may be controlled to achieve desired uniformity characteristics, such as wafer thickness uniformity, thickness range, sheet resistance uniformity, and sheet resistance range.
[0094] In various embodiments, the bias power scheme can be controlled to improve the reliability of the device. In one example implementation, Figure 5 , a time dependent dielectric breakdown (TDDB) test was performed to compare the reliability of a MIM capacitor having a TiN layer formed using a single step bias and a MIM capacitor having a TiN layer formed using a multi-step bias. In this example, the specification requirement is 10 years of use. The reverse direction is defined as a top capacitor plate with a negative voltage applied and a bottom capacitor plate with a positive voltage applied, where electrons move from the top plate to the bottom plate. The TDDB value 502 of the capacitor having a TiN layer formed using a multi-step bias is much better than the TDDB value 504 of the capacitor having a TiN layer formed using a single step bias. Performance is improved due to reduced damage to the top surface of the high-K layer of the capacitor.
[0095] Furthermore, in this example, the forward direction is defined as the top capacitor plate with a positive voltage applied and the bottom capacitor plate with a negative voltage applied, where electrons move from the bottom plate to the top plate. The TDDB value 506 of the capacitor with the TiN layer formed using a multi-step bias is much better than the TDDB value 508 of the capacitor with the TiN layer formed using a single-step bias. The performance is improved due to reduced damage to the top surface of the high-K layer of the capacitor.
[0096] Figure 6 A process flow diagram is depicted of an example process 600 for forming a MIM capacitor using a multi-step bias power scheme. Figure 6 Combination 7A to 7D Describe, 7A to 7D6 is a cross-sectional view of a semiconductor device at various stages of manufacture according to some embodiments of the exemplary process 600 disclosed herein. In some drawings, some reference numbers of elements or features depicted therein may be omitted to avoid obscuring other elements or features; these omissions are for convenience in describing the drawings.
[0097] The process 600 is provided as an example only and is not intended to limit the present disclosure beyond what is expressly recited in the claims. Additional steps may be provided before, during, or after the example process 600, and some of the steps described may be removed, substituted, or deleted for additional embodiments of the example process 600. Additional features may be added to the semiconductor devices depicted in the figures, and some of the features described below may be replaced, modified, or deleted in other embodiments of the semiconductor device.
[0098] It should be understood that some portions of the semiconductor device may be manufactured by typical semiconductor technology manufacturing processes, and therefore only some processes are briefly described herein. In addition, the exemplary semiconductor device may include various other devices and features, such as other types of devices, such as additional transistors, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, and / or other logic devices, etc., which are simplified for better understanding of the concepts disclosed herein. In some embodiments, the exemplary device includes a plurality of semiconductor devices (e.g., transistors) that may be interconnected, including PFETs, NFETs, etc. In addition, it should be noted that the operations of process 600 (including any description given with reference to the accompanying drawings) are merely exemplary and are not intended to limit the content beyond the specific description of the appended claims.
[0099] At block 610, the exemplary process 600 includes providing a substrate. The substrate includes a layer on which an electrode (eg, a TiN electrode) is to be formed. Fig. 7A In an example, in an embodiment after completing block 610, a substrate having a pre-MIM layer 702 is provided, on which an electrode (eg, a TiN electrode) is to be formed.
[0100] At block 620, the exemplary process 600 includes forming a first electrode (e.g., a TiN electrode) over a substrate, the first electrode having a varying density, the varying density increasing from a first density level at a bottom surface of the first electrode to a second density level, the second density level at a middle region within the first electrode being higher than the first density level, and increasing to a third density level, the third density level at a top surface of the first electrode being higher than the second density level. In various embodiments, forming the first electrode includes depositing the first electrode by a plasma-based physical vapor deposition (PVD) technique using a power source (e.g., a DC sputtering power source, an RF sputtering power source, a pulsed DC sputtering power source, a medium frequency sputtering power source, an AC sputtering power source, a high power pulsed magnetron sputtering (HiPIMS) power source), and increasing a sputtering yield resulting from the magnetron sputtering as the magnetron sputtering continues. In various embodiments, magnetron sputtering includes systematically increasing bias power to bombard a target material using a bias power schedule to sputter atoms of the target material, the bias power schedule causing the bias power to increase from a first power level resulting in an initial sputtering yield to a higher power level resulting in a desired sputtering yield, the desired sputtering yield being higher than the initial sputtering yield. In various embodiments, the bias power schedule includes applying one or more of increasing the bias power in a stepwise increase, increasing the bias power in a linear manner, and / or increasing the bias power in an exponential manner.
[0101] In various embodiments, the bias power scheme is controlled to achieve desired mechanical properties, desired electrical properties, desired uniform properties, or desired consistent properties. In various embodiments, the desired mechanical properties may include microstructural changes in the form of density, desired roughness, grain size, crystal arrangement. In various embodiments, the desired electrical properties may include resistivity or plate resistance. In various embodiments, the desired consistent properties may include sidewall angle size. In various embodiments, the desired uniform properties may include wafer thickness uniformity, thickness range, sheet resistance uniformity, and sheet resistance range.
[0102] Reference Figure 7B In an example, after completing block 620, a substrate having a pre-MIM layer 702 is provided, wherein an electrode 704 (e.g., a TiN electrode) is formed on the pre-MIM layer 702. The electrode 704 has a varying density, increasing from a first density level at a bottom surface 701 of the first electrode to a second density level, the second density level at a middle region 703 within the first electrode being higher than the first density level, and increasing to a third density level, the third density level at a top surface 705 of the first electrode being higher than the second density level.
[0103] At block 630, the exemplary process 600 includes forming a high-K dielectric layer over the first electrode. Figure 7CIn an example, in an embodiment after completing block 630, a high-K dielectric layer 706 has been formed over the electrode 704. The high-K dielectric layer 706 may be formed by a suitable deposition technique (eg, PVD).
[0104] At block 640, the example process 600 includes forming a second electrode over the high-K dielectric layer, the high-K dielectric layer having a varying density, the varying density increasing from a fourth density level at a bottom surface of the second electrode bonded to the high-K dielectric layer to a fifth density level, the fifth density level at a middle region of the second electrode being higher than the fourth density level, and increasing to a sixth density level, the sixth density level at a top surface within the second electrode being higher than the fifth density level. In various embodiments, forming the second electrode includes depositing the second electrode by a plasma-based physical vapor deposition (PVD) technique using a power source (e.g., a DC sputtering power source, an RF sputtering power source, a pulsed DC sputtering power source, a medium frequency sputtering power source, an AC sputtering power source, a high power pulsed magnetron sputtering (HiPIMS) power source), and increasing a sputtering yield resulting from the magnetron sputtering as the magnetron sputtering continues. In various embodiments, magnetron sputtering includes systematically increasing bias power to bombard a target material using a bias power schedule to sputter atoms of the target material, the bias power schedule causing the bias power to increase from a first power level resulting in an initial sputtering yield to a higher power level resulting in a desired sputtering yield, the desired sputtering yield being higher than the initial sputtering yield. In various embodiments, the bias power schedule includes applying one or more of increasing the bias power in a stepwise increase, increasing the bias power in a linear manner, and / or increasing the bias power in an exponential manner.
[0105] In various embodiments, the first density level is equal to the fourth density level, the second density level is equal to the fifth density level, and the third density level is equal to the sixth density level. In other embodiments, the first density level is not equal to the fourth density level, the second density level is not equal to the fifth density level, and / or the third density level is not equal to the sixth density level. In various embodiments, the bias power scheme can be controlled to achieve a desired mechanical characteristic, a desired electrical characteristic, a desired uniform characteristic, or a desired consistent characteristic.
[0106] Reference to Fig.7D In an example, in an embodiment after completing block 640, an electrode 708 (e.g., a TiN electrode) is formed over the high-K dielectric layer 706. The electrode 708 has a varying density, increasing from a first density level at a bottom surface 707 of the second electrode to a second density level, the second density level at a middle region 709 within the second electrode being higher than the first density level, and increasing to a third density level, the third density level at a top surface 711 of the second electrode being higher than the second density level.
[0107] At block 650, the example process 600 includes: performing additional manufacturing operations. The semiconductor device may be further processed to form various features and regions known in the art. For example, subsequent processes may form various contacts, vias, wires, and multilayer interconnect features (e.g., metal layers and interlayer dielectrics) on the substrate, configured to connect the various features to form a functional circuit. In this example, the multilayer interconnects may include: vertical interconnects such as vias or contacts, and horizontal interconnects such as metal lines. The various interconnect features may use various conductive materials, including copper, tungsten and / or silicide. In one example, damascene and / or dual damascene processes are used to form a copper-related multilayer interconnect structure. In addition, additional process steps may be implemented before, during, or after process 600, and some of the process steps described above according to various embodiments of process 600 may be replaced or deleted.
[0108] Although the foregoing examples are illustrative of the formation of TiN material / high-K material interfaces in MIM capacitors and MIM capacitors, the foregoing devices, apparatuses, and methods may also be used in conjunction with other material layer interfaces. For example, the multi-level bias power scheme may be used to deposit materials other than TiN. In addition, the multi-level bias power scheme may also be used to deposit TiN materials in other applications, such as VIA structures, interdiffusion barriers, and metal hard masks, where it may be helpful to prevent intermixing and interdiffusion.
[0109] In some aspects, the technology described herein relates to a manufacturing method, comprising: forming a first electrode above a substrate, the first electrode having a variable density, the variable density increasing from a first density level at a bottom surface of the first electrode to a second density level, the second density level at a top surface of the first electrode being higher than the first density level; forming a high-K dielectric layer above the first electrode; and forming a second electrode above the high-K dielectric layer, the high-K dielectric layer having a variable density, the variable density increasing from a third density level at a bottom surface of the second electrode bonded to the high-K dielectric layer to a fourth density level, the fourth density level at a top surface of the second electrode being higher than the third density level.
[0110] In some aspects, the technology described herein relates to a manufacturing method, wherein: forming a first electrode includes: forming the first electrode with a variable density, the variable density increasing from a first density level at a bottom surface of the first electrode to a first intermediate density level, the first intermediate density level at a middle region within the first electrode being higher than the first density level, and increasing to a second density level, the second density level at a top surface of the first electrode being higher than the first intermediate density level; and forming the second electrode includes: forming a second electrode with a variable density, the variable density increasing from a third density level at a bottom surface of the second electrode bonded to a high-K dielectric layer to a second intermediate density level, the second intermediate density level at a middle region within the second electrode being higher than the third density level, and increasing to a fourth density level, the fourth density level at the top surface of the second electrode being higher than the second intermediate density level.
[0111] In some aspects, the technology described herein relates to a manufacturing method in which the first density level is equal to the third density level, the first intermediate density level is equal to the second intermediate density level, and the second density level is equal to the fourth density level.
[0112] In some aspects, the technology described herein relates to a manufacturing method, wherein forming a first electrode and a second electrode further includes: depositing a first titanium nitride (TiN) electrode and a second TiN electrode by a plasma-based physical vapor deposition technique using a power source to cause magnetron sputtering.
[0113] In some aspects, the technology described herein relates to a manufacturing method in which magnetron sputtering includes: systematically increasing the bias power using a bias power scheme to bombard a target material to sputter atoms of the target material, the bias power scheme causing the bias power to increase from a first power level that results in an initial sputtering yield to a higher power level that results in a desired sputtering yield, wherein the desired sputtering yield is higher than the initial sputtering yield.
[0114] In some aspects, the techniques described herein relate to a method of manufacturing in which a bias power scheme includes applying a step increase to increase the bias power.
[0115] In some aspects, the techniques described herein relate to a method of manufacturing in which a bias power scheme includes increasing the bias power in a linear manner.
[0116] In some aspects, the techniques described herein relate to a method of manufacturing in which a bias power scheme includes increasing the bias power in an exponential manner.
[0117] In some aspects, the technology described herein relates to a semiconductor device comprising: a substrate; a first titanium nitride electrode formed over the substrate, the first titanium nitride electrode having a varying density that increases from a first density level at a bottom surface of the first TiN electrode to a second density level, the second density level at a top surface of the first TiN electrode being higher than the first density level; a high-K dielectric layer formed over the first TiN electrode; and a second TiN electrode over the high-K dielectric layer, having a varying density that increases from a third density level at a bottom surface of the second TiN electrode bonded to the high-K dielectric layer to a fourth density level, the fourth density level at a top surface of the second TiN electrode being higher than the third density level.
[0118] In some aspects, the technology described herein relates to a semiconductor device, wherein: a varying density of a first TiN electrode increases from a first density level at a bottom surface of the first TiN electrode to a first intermediate density level, the first intermediate density level at an intermediate region within the first TiN electrode being higher than the first density level, and increases to a second density level, the second density level at a top surface of the first TiN electrode being higher than the first intermediate density level; and a varying density of a second TiN electrode increases from a third density level at a bottom surface of the second TiN electrode to a second intermediate density level, the second intermediate density level at an intermediate region within the second TiN electrode being higher than the third density level, and increases to a fourth density level, the fourth density level at a top surface of the second TiN electrode being higher than the second intermediate density level.
[0119] In some aspects, the techniques described herein relate to a semiconductor device in which a first density level is equal to a third density level, a first intermediate density level is equal to a second intermediate density level, and the second density level is equal to a fourth density level.
[0120] In some aspects, the technology described herein relates to a semiconductor device in which a first TiN electrode and a second TiN electrode are formed by a plasma-based physical vapor deposition (PVD) technique using a power source to cause magnetron sputtering.
[0121] In some aspects, the technology described herein relates to a semiconductor device, wherein a power source for causing magnetron sputtering using a plasma-based physical vapor deposition technique comprises: a DC sputtering power source, an RF sputtering power source, a pulsed DC sputtering power source, a medium frequency sputtering power source, an AC sputtering power source, or a high power pulsed magnetron sputtering power source.
[0122] In some aspects, the technology described herein relates to a semiconductor device in which a first TiN electrode and a second TiN electrode are formed by magnetron sputtering, and a bias power is systematically increased using a bias power scheme to bombard a target material and sputter atoms of the target material, the bias power scheme causing the bias power to increase from a first power level resulting in a first density level and a third density level to a second power level resulting in a second density level and a fourth density level.
[0123] In some aspects, the techniques described herein relate to a semiconductor device in which a bias power scheme includes applying a step increase to increase the bias power.
[0124] In some aspects, the techniques described herein relate to a semiconductor device in which a bias power scheme includes increasing the bias power in a linear manner.
[0125] In some aspects, the technology described herein relates to a manufacturing method, comprising: depositing a first TiN electrode over a substrate, depositing the first TiN electrode by a plasma-based physical vapor deposition technique using a power source to cause magnetron sputtering, wherein the first TiN electrode has a varying density, the varying density increasing from a first density level at a bottom surface of the first TiN electrode to a second density level, the second density level at a middle region within the first TiN electrode being higher than the first density level, and increasing to a third density level, the third density level at a top surface of the first TiN electrode being higher than the second density level; forming a high-K dielectric layer over the first TiN electrode; and depositing a second TiN electrode over the high-K dielectric layer. , depositing a second TiN electrode by magnetron sputtering, wherein the second TiN electrode has a varying density that increases from a first density level at a bottom surface of the second TiN electrode bonded to a high-K dielectric layer to a second density level, the second density level at an intermediate region within the second TiN electrode being higher than the first density level, and to a third density level, the third density level at a top surface of the second TiN electrode being higher than the second density level; wherein the magnetron sputtering includes bombarding a target material with a bias power scheme that systematically increases a bias power to sputter atoms of the target material, the bias power scheme causing the bias power to increase from a first power level that is high enough to cause sputtering to a higher power level that results in a desired sputtering yield.
[0126] In some aspects, the techniques described herein relate to a semiconductor device in which a bias power scheme includes applying a step increase to increase the bias power.
[0127] In some aspects, the techniques described herein relate to a semiconductor device in which a bias power scheme includes increasing the bias power in a linear manner.
[0128] In some aspects, the techniques described herein relate to a semiconductor device in which a bias power scheme includes increasing the bias power in an exponential manner.
[0129] Although the disclosure has presented at least one exemplary embodiment in the aforementioned detailed description, it should be understood that there are a large number of changes in the content. It should also be understood that one or more exemplary embodiments are only examples and are not intended to limit the scope, applicability or configuration of the disclosure in any way. On the contrary, the foregoing detailed description provides a convenient roadmap for implementing the exemplary embodiments of the disclosure for those skilled in the art. It should be understood that various changes can be made to the component functions and arrangements described in the exemplary embodiments without departing from the scope of the attached patent application disclosed.
Claims
1. A method for manufacturing a semiconductor device, characterized in that: The method includes: forming a first electrode over a substrate, the first electrode having a varying density that increases from a first density level at a bottom surface of the first electrode to a second density level, the second density level at a top surface of the first electrode being higher than the first density level; forming a high-K dielectric layer above the first electrode; and A second electrode is formed above the high-K dielectric layer, the high-K dielectric layer having a variable density that increases from a third density level at a bottom surface of the second electrode bonded to the high-K dielectric layer to a fourth density level, the fourth density level at a top surface of the second electrode being higher than the third density level.
2. The manufacturing method according to claim 1, characterized in that: Forming the first electrode comprises: forming the first electrode with a varying density, the varying density increasing from the first density level at the bottom surface of the first electrode to a first intermediate density level, the first intermediate density level at an intermediate region within the first electrode being higher than the first density level, and increasing to the second density level, the second density level at the top surface of the first electrode being higher than the first intermediate density level; and Forming the second electrode comprises: The second electrode is formed to have a variable density, which increases from the third density level at the bottom surface of the second electrode bonded to the high-K dielectric layer to a second intermediate density level, the second intermediate density level at an intermediate region within the second electrode being higher than the third density level, and increases to the fourth density level, the fourth density level at the top surface of the second electrode being higher than the second intermediate density level.
3. The manufacturing method according to claim 2, characterized in that: The first density level is equal to the third density level, the first intermediate density level is equal to the second intermediate density level, and the second density level is equal to the fourth density level.
4. The manufacturing method according to claim 1, characterized in that: Forming the first electrode and the second electrode further comprises: A first titanium nitride electrode and a second titanium nitride electrode are deposited by a plasma-based physical vapor deposition technique using a power source to cause magnetron sputtering.
5. The manufacturing method according to claim 4, characterized in that: The magnetron sputtering includes: The target material is bombarded with a bias power that is systematically increased using a bias power schedule to sputter atoms of the target material, the bias power schedule causing the bias power to increase from a first power level that results in an initial sputtering yield to a higher power level that results in a desired sputtering yield that is higher than the initial sputtering yield.
6. A semiconductor device, characterized in that: Include: a substrate; a first titanium nitride electrode formed above the substrate, the first titanium nitride electrode having a variable density that increases from a first density level at a bottom surface of the first titanium nitride electrode to a second density level, the second density level at a top surface of the first titanium nitride electrode being higher than the first density level; a high-K dielectric layer formed above the first titanium nitride electrode; and A second titanium nitride electrode is located above the high-K dielectric layer and has a variable density that increases from a third density level at a bottom surface of the second titanium nitride electrode bonded to the high-K dielectric layer to a fourth density level, wherein the fourth density level at a top surface of the second titanium nitride electrode is higher than the third density level.
7. The semiconductor device according to claim 6, wherein: The varying density of the first titanium nitride electrode increases from the first density level at the bottom surface of the first titanium nitride electrode to a first intermediate density level, the first intermediate density level at an intermediate region within the first titanium nitride electrode being higher than the first density level, and to the second density level, the second density level at the top surface of the first titanium nitride electrode being higher than the first intermediate density level; and The variable density of the second titanium nitride electrode increases from the third density level at the bottom surface of the second titanium nitride electrode to a second intermediate density level, the second intermediate density level at an intermediate region within the second titanium nitride electrode being higher than the third density level, and increases to the fourth density level, the fourth density level at the top surface of the second titanium nitride electrode being higher than the second intermediate density level.
8. The semiconductor device according to claim 6, wherein: The first titanium nitride electrode and the second titanium nitride electrode are formed by a plasma physical vapor deposition technique using a power source to cause magnetron sputtering.
9. The semiconductor device according to claim 8, wherein: The first titanium nitride electrode and the second titanium nitride electrode are formed by magnetron sputtering, and the bias power is systematically increased using a bias power scheme to bombard the target material and sputter atoms of the target material, the bias power scheme causing the bias power to increase from a first power level resulting in the first density level and the third density level to a second power level resulting in the second density level and the fourth density level.
10. A method for manufacturing a semiconductor device, characterized in that: The method includes: Depositing a first titanium nitride electrode over a substrate by plasma-based physical vapor deposition using a power source to cause magnetron sputtering, wherein the first titanium nitride electrode has a varying density that increases from a first density level at a bottom surface of the first titanium nitride electrode to a second density level, the second density level at an intermediate region within the first titanium nitride electrode being higher than the first density level, and increasing to a third density level, the third density level at a top surface of the first titanium nitride electrode being higher than the second density level; forming a high-K dielectric layer above the first titanium nitride electrode; and Depositing a second titanium nitride electrode over the high-K dielectric layer by magnetron sputtering, wherein the second titanium nitride electrode has a varying density, the varying density increasing from a first density level at a bottom surface of the second titanium nitride electrode bonded to the high-K dielectric layer to a second density level, the second density level at an intermediate region within the second titanium nitride electrode being higher than the first density level, and increasing to a third density level, the third density level at a top surface of the second titanium nitride electrode being higher than the second density level; The magnetron sputtering includes systematically increasing bias power to bombard a target material to sputter atoms of the target material using a bias power schedule that causes the bias power to increase from a first power level high enough to cause sputtering to a higher power level that results in a desired sputtering yield.