Multilayer film
By using metallocene-catalyzed multimodal polyethylene copolymers in multilayer films and copolymers of ethylene and C3-C8α-olefins in multilayer films, the problems in recirculation and performance of existing multilayer films are solved, and mechanical and sealing are achieved Improvement of performance and maintenance of optical performance, suitable for packaging of food and medical products.
Patent Information
- Application Number
- CN202380027511.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-16
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-08
AI Technical Summary
Existing multilayer films have difficulties in recycling, while poor material performance, especially in mechanical and sealing properties, and a single material solution is lacking.
A multilayer film structure consisting of metallocene-catalyzed multimodal polyethylene copolymer (MMCP) and copolymers of ethylene with C3-C8α-olefins, including surface, core and sealing layers, through specific component ratios and processes Methods to improve the mechanical and sealing properties of the membrane.
实现了多层膜的易于再循环,并在机械和密封性能上显著提升,同时保持可接受的光学性能,适用于食品和医疗产品的包装材料。
Smart Images

Figure BDA0005042070640000101 
Figure BDA0005042070640000111 
Figure BDA0005042070640000112
Abstract
Description
[0001] The present invention relates to a multilayer film comprising a skin layer (SKL), a core layer (CL) and a sealing layer (SL), wherein the sealing layer (SL) comprises (a) 15 to 85 wt.-% of a specific metallocene-catalyzed multimodal polyethylene copolymer (MMCP), based on the total weight of the sealing layer (SL) and (b) 15 to 85 wt.-% of a specific plastomer, based on the total weight of the sealing layer (SL), wherein components (a) and (b) add up to a maximum of 100 wt.-%. The present invention also relates to the use of the multilayer film as a packaging material, preferably for food and / or medical products.
[0002] Polyethylene is widely used in various fields of daily life, such as packaging, due to its excellent cost-effectiveness. Due to different needs, multilayer products with different types of materials are now used, which meets the needs on the one hand, but the disadvantage is that such products are difficult to recycle. From the perspective of recycling, a single material solution would be preferred. At the same time, the performance of the material should not be reduced.
[0003] Single-material solutions are known in the prior art.
[0004] EP 0 575 465 A1 relates to a heat-sealable composition suitable for films and film structures, comprising: (a) 30 to 70% by weight of a low melting point polymer, the polymer comprising a density of 0.88 g / cm 3 Up to 0.915g / cm 3 , an ethylene-based copolymer having a melt index of 1.5 dg / min to 7.5 dg / min, a molecular weight distribution of no more than 3.5 and a composition distribution breadth index of greater than 70%; and (b) 70 to 30 weight percent of a propylene-based polymer different from (a), the polymer having 88 mol% to 100 mol% propylene and 12 mol% to 0 mol% of an α-olefin other than propylene.
[0005] WO 2012 / 061168 A1 relates to a sealant composition, a method for preparing the same, an article made therefrom, and a method for forming such an article. The sealant composition according to the invention comprises: (a) 70 to 99.5 wt% of an ethylene / α-olefin interpolymer composition based on the total weight of the sealant composition, wherein the ethylene / α-olefin interpolymer composition comprises an ethylene / α-olefin interpolymer composition, wherein the ethylene / α-olefin interpolymer composition has a comonomer distribution constant (CDC) in the range of 15 to 250, a Cd / D ratio in the range of 0.875 to 0.963 g / cm 3%, a density in the range of 0.2 to 20 g / 10 min, a melt index (I2) in the range of 0.2 to 20 g / 10 min, and a long chain branching frequency in the range of 0.02 to 3 long chain branches (LCB) / 1000C; (b) 0.5 to 30 wt% of a propylene / α-olefin interpolymer composition, wherein the propylene / α-olefin interpolymer composition comprises a propylene / α-olefin copolymer or a propylene / ethylene / butene terpolymer, wherein the propylene / α-olefin copolymer has a crystallinity in the range of 1 wt% to 30 wt%, a heat of fusion in the range of 2 J / g to 50 J / g, and a DSC melting point in the range of 25°C to 110°C.
[0006] US2021 / 0324185 A1 relates to a polyolefin composition containing one or more high-density polyethylene (HDPE) and linear low-density polyethylene (LLDPE) and a method for forming the same. The polyolefin composition comprises about 40% to about 60% by weight of HDPE and about 40% to about 60% by weight of LLDPE, based on the weight of the polyolefin composition. The HDPE has a molecular weight greater than 0.93 g / cm 3 The density of LLDPE is greater than 0.915 g / cm 3 The polyolefin composition has a density of about 0.91 g / cm 3 or greater, a density of about 0.5 dg / min to about 6 dg / min, and a Tw1-Tw2 value of about -25°C or less.
[0007] WO 2021 / 204799 A1 relates to a film comprising a sealing layer, the sealing layer comprising polyethylene A, the polyethylene A comprising a portion derived from ethylene and a portion derived from an α-olefin containing 4 to 10 carbon atoms, the polyethylene A having a molecular weight of ≥870 and ≤920 kg / m 3 , preferably ≥900 and ≤920kg / m 3 The density determined according to ASTM D792 (2013), wherein the polyethylene A has: a portion of material eluted in analytical temperature rising elution fractionation (a-TREF) at a temperature of ≤30.0°C, ≥5.0 wt% and ≤15.0 wt%, preferably ≥7.5 wt% and ≤12.5 wt%, relative to the total weight of the polyethylene; and two different peaks in the a-TREF curve within the elution temperature range of 50.0 to 90.0°C, wherein the elution temperature difference between the two peaks is ≤17.5°C, preferably ≤15.0°C.
[0008] Starting from this, it was an object of the present invention to provide a multilayer film which is not only easy to recycle but also has very good mechanical and sealing properties and acceptable optical properties.
[0009] These objects have been solved by a multilayer film according to claim 1, comprising
[0010] The skin layer (SKL), the core layer (CL) and the sealing layer (SL); the sealing layer (SL) includes
[0011] (a) 15 to 85 wt.-%, based on the total weight of the sealing layer (SL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP) consisting of
[0012] (i) 35.0 to 70.0 wt% of an ethylene-1-butene polymer component (A), based on the total weight of the MMCP; and
[0013] (ii) 50.0 to 65.0 wt% of an ethylene-1-hexene polymer component (B), based on the total weight of the MMCP; wherein
[0014] The ethylene-1-butene polymer component (A) has
[0015] ·920 to 960 kg / m 3 Density within the range (ASTM D792);
[0016] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 3.0 to 300.0 g / 10 min;
[0017] · a 1-butene content in the range of 0.1 to 3.0 mol% based on the ethylene-1-butene polymer component (A); and
[0018] The ethylene-1-hexene polymer component (B) has
[0019] 880 to 920 kg / m 3 Density within the range (ASTM D792);
[0020] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.001 to 1.0 g / 10 min;
[0021] · a 1-hexene content in the range of 2.5 to 10.0 mol% based on the ethylene-1-hexene polymer compound (B); and
[0022] Metallocene-catalyzed multimodal polyethylene copolymers (MMCPs) have
[0023] ·910 to 930 kg / m 3 Density within the range (ASTM D792);
[0024] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 2.0 g / 10 min;
[0025] as well as
[0026] MFR in the range of 22 to 70 21 (190℃, 21.6kg, ISO 1133) and MFR2
[0027] (190℃, 2.16kg, ISO 1133) ratio, MFR 21 / MFR2; and
[0028] (b) 15 to 85 wt. % of a plastomer, based on the total weight of the sealing layer (SL), which is a copolymer of ethylene and a C3-C8 α-olefin; having
[0029] 870 to 900 kg / m 3 Density within the range (ASTM D792);
[0030] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 10.0 g / 10 min;
[0031] as well as
[0032] - a melting point in the range of 65 to 80°C (measured by DSC as described in the specification); and; wherein the weight ratios of components (a) and (b) add up to at most 100 wt%.
[0033] Advantageous embodiments of the multilayer film according to the invention are specified in dependent claims 2 to 14. The invention also relates to the use of the film according to the invention according to claim 15 as packaging material.
[0034] definition
[0035] Metallocene-catalyzed (linear low density) polyethylene is defined in the present invention as a (linear low density) polyethylene copolymer produced in the presence of a metallocene catalyst.
[0036] Ziegler-Natta catalyzed linear low density polyethylene is defined in the present invention as a (linear low density) polyethylene copolymer produced in the presence of a Ziegler-Natta catalyst.
[0037] For the purposes of the present invention, a metallocene-catalyzed (linear low density) polyethylene consisting of an ethylene-1-butene polymer component (A) and an ethylene-1-hexene polymer component (B) refers to a polymer produced in at least a two-stage sequential polymerization process, wherein the first component (A) is first produced and then, in a subsequent polymerization step, component (B) is produced in the presence of component (A) to produce a metallocene-catalyzed (linear low density) polyethylene or vice versa, i.e., component (B) is first produced and then, in a subsequent polymerization step, component (A) is produced in the presence of component (B) to produce a metallocene-catalyzed (linear low density) polyethylene.
[0038] In the context of multimodal metallocene-catalyzed (linear low density) polyethylene, the term "multimodal" refers herein to the multimodality with respect to the melt flow rate (MFR) of at least the ethylene polymer components (A) and (B), i.e. the ethylene polymer components (A) and (B) have different MFR values. The multimodal metallocene-catalyzed (linear low density) polyethylene may have additional multimodality between the ethylene polymer components (A) and (B) with respect to one or more other properties (such as density, comonomer type and / or comonomer content), which will be described below.
[0039] Low density polyethylene (LDPE) is defined in the present invention as a low density polyethylene copolymer, which is preferably produced in a high pressure process.
[0040] Ethylene homopolymers are polymers consisting essentially of ethylene monomer units. Due to impurities, especially in industrial polymerization processes, ethylene homopolymers may contain up to 1.0 mol% of comonomer units, preferably up to 0.5 mol% of comonomer units, most preferably up to 0.01 mol% of comonomer units.
[0041] In the context of the present invention, a single material film may be a film that uses primarily one polymer (eg polyethylene) but not other polymers in significant amounts. However, in the case where the film is based on polyethylene, different polyethylenes may be present.
[0042] Where the term "comprising" is used in the present description and claims, it does not exclude other, not specifically stated, elements of major or minor functional importance. For the purposes of the present invention, the term "consisting of" is considered to be a preferred embodiment of the term "comprising". If a group is defined hereinafter as comprising at least a certain number of embodiments, this is also to be understood as disclosing the group, which preferably consists only of these embodiments.
[0043] Whenever the terms "including" or "having" are used, these terms are meant to be equivalent to "comprising" as defined above.
[0044] When an indefinite or definite article is used when referring to a singular noun, for example "a", "an" or "the", this includes a plural of that noun unless otherwise stated.
[0045] Metallocene-catalyzed multimodal polyethylene copolymers (MMCP)
[0046] The sealing layer of the multilayer film according to the invention comprises a specific metallocene-catalyzed multimodal polyethylene copolymer (MMCP). The other layers may also comprise said copolymer (MMCP).
[0047] The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) consists of (i) 35.0 to 50.0 wt% of an ethylene-1-butene polymer component (A) and (ii) 50.0 to 65.0 wt% of an ethylene-1-hexene polymer component (B).
[0048] The ethylene-1-butene polymer component (A) has a molecular weight of 920 to 960 kg / m 3 The present invention relates to a polymer having a density (ASTM D792) in the range of 0.1 to 0.5 g / 10 min, a MFR2 (190° C., 2.16 kg, ISO 1133) in the range of 3.0 to 300.0 g / 10 min, and a 1-butene content in the range of 0.1 to 3.0 mol % based on the ethylene-1-butene polymer component (A).
[0049] The ethylene-1-hexene polymer component (B) has a molecular weight of 880 to 920 kg / m 3 range, a density (ASTM D792) within a range of 0.001 to 1.0 g / 10 min, an MFR2 (190° C., 2.16 kg, ISO 1133) within a range of 0.001 to 1.0 g / 10 min, and a 1-hexene content within a range of 2.5 to 10.0 mol % based on the ethylene-1-hexene polymer compound (B).
[0050] The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has a molecular weight of 910 to 930 kg / m 3 Density in the range (ASTM D792), MFR2 in the range of 0.1 to 2.0 g / 10 min (190°C, 2.16 kg, ISO 1133) and MFR in the range of 22 to 70 21 Ratio of MFR (190℃, 21.6kg, ISO 1133) to MFR2 (190℃, 21.6kg, ISO 1133), MFR 21 / MFR2.
[0051] In a preferred embodiment of the present invention, the ethylene-1-butene polymer component (A) consists of ethylene polymer fractions (A-1) and (A-2).
[0052] In case the ethylene-1-butene polymer component (A) consists of ethylene polymer fractions (A-1) and (A-2), the MFR2 of the ethylene polymer fractions (A-1) and (A-2) may be the same as or different from each other.
[0053] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer parts (A-1) and (A-2) is in the range of 3.0 to 300.0 g / 10 min, preferably 100 to 150.0 g / 10 min, more preferably 110 to 130 g / 10 min or 115 to 125 g / 10 min.
[0054] In a preferred embodiment the MFR2 of ethylene polymer components (A) and (B) are different from each other.
[0055] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer component (A) is in the range of 3.0 to 300 g / 10 min, preferably 3.5 to 250 g / 10 min, more preferably 4.0 to 200 g / 10 min, even more preferably 4.5 to 150 g / 10 min or 120 to 130 g / 10 min.
[0056] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer component (B) is in the range of 0.001 to 1.0 g / 10 min, preferably 0.005 to 0.8 g / 10 min, more preferably 0.008 to 0.6 g / 10 min, even more preferably 0.01 to 0.3 g / 10 min.
[0057] The MFR2 (190°C, 2.16 kg, ISO 1133) of the multimodal copolymer (MMCP) is in the range of 0.1 to 2.0 g / 10 min, preferably 0.2 to 1.7 g / 10 min, more preferably 0.5 to 1.5 g / 10 min, even more preferably 0.6 to 0.8 g / 10 min.
[0058] Of course, in addition to the multimodality with respect to (i.e. the difference between) the MFR2 of the ethylene polymer components (A) and (B), the multimodal PE of the present invention may also be multimodal, for example with respect to one or both of two other properties: multimodality with respect to (i.e. the difference between) the densities of the ethylene polymer components (A) and (B).
[0059] Preferably, the multimodal copolymer (MMCP) is further multimodal with respect to the comonomer content of the ethylene polymer components (A) and (B).
[0060] The comonomer type of polymer fractions (A-1) and (A-2) is the same, so both fractions have 1-butene as a comonomer.
[0061] The comonomer content of components (A) and (B) can be measured or, in a preferred case, in a so-called multi-stage process, one component is first produced and then the other component is produced in the presence of the first component, then the comonomer content of the first produced component, e.g. component (A), can be measured and the comonomer content of the other component, e.g. component (B), can be calculated according to the following equation:
[0062] The comonomer content in component B (mol% or weight%) = (the comonomer content in the final product (mol% or weight%) - (the weight fraction of component A) * Comonomer content in component A (mol% or weight%)) / (weight fraction of component B).
[0063] MFR of multimodal copolymers (MMCP) 21 The ratio of MFR (190℃, 21.6kg, ISO 1133) to MFR2 (190℃, 2.16kg, ISO1133), MFR 21 / MFR2 is in the range of 22 to 70, preferably 23 to 50, more preferably 25 to 48, even more preferably 28 to 46.
[0064] The total amount of 1-butene is preferably in the range of 0.1 to 1.0 mol%, more preferably 0.2 to 0.8 mol%, even more preferably 0.3 to 0.7 mol%, based on the multimodal polymer (MMCP).
[0065] The total amount of 1-hexene based on the multimodal polymer (MMCP) is preferably in the range of 1.5 to 8.0 mol%, more preferably 2.0 to 6.0 mol%, even more preferably 2.2 to 4.0 mol%.
[0066] The total amount (mol%) of 1-butene present in the ethylene-1-butene polymer component (A) is 0.1 to 3.0 mol%, preferably 0.3 to 2.6 mol%, more preferably 0.5 to 2.0 mol%, even more preferably 0.6 to 1.8 mol%, based on the ethylene-1-butene polymer component (A).
[0067] The total amount (mol%) of 1-hexene present in the ethylene-1-hexene polymer component (B) is 2.5 to 10.0 mol%, preferably 3.0 to 8.0 mol%, more preferably 3.5 to 6.0 mol%, based on the ethylene-1-hexene polymer component (B).
[0068] Even more preferably, the multimodal polymer (MMCP) of the present invention is further multimodal with respect to the density difference between ethylene polymer component (A) and ethylene polymer component (B). Preferably, the density of ethylene polymer component (A) is different from, preferably higher than, the density of ethylene polymer component (B).
[0069] The density of the ethylene polymer component (A) is 920 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 and / or the density of the ethylene polymer component (B) is in the range of 880 to 920 kg / m 3 , preferably 885 to 915 kg / m 3 , more preferably 890 to 910 kg / m 3 within the range.
[0070] The density of the polymer parts (A-1) and (A-2) is 925 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 , most preferably 935 to 945 kg / m 3 within the range.
[0071] The densities of the polymer parts (A-1) and (A-2) may be the same as or may be different from each other.
[0072] The metallocene-catalyzed multimodal copolymer (MMCP) is preferably a linear low density polyethylene (LLDPE) which has a well-known meaning.
[0073] The multimodal copolymer (MMCP) has a density of 910 to 930 kg / m 3 , preferably 912 to 925 kg / m 3 , more preferably 915 to 920 kg / m 3 within the range.
[0074] More preferably, the multimodal copolymer (MMCP) is multimodal (i.e. there is a difference between them) at least with respect to MFR2, the comonomer content and the density of the ethylene polymer components (A) and (B) is multimodal (i.e. there is a difference between them), as defined above, below or in the claims, the claims including any preferred ranges or embodiments of the polymer composition.
[0075] Furthermore, the multimodal copolymer (MMCP) may also have a molecular weight distribution (Mw / Mn) determined by GPC in the range of at least 3.5 to 7.2, preferably in the range of 4.0 to 7.0, more preferably in the range of 4.5 to 6.8.
[0076] Furthermore, the ratio of the soluble fraction at 35°C of the multimodal copolymer (MMCP) determined by cross fractionation chromatography (CFC) as described in the experimental part to the density of the multimodal polyethylene copolymer (MMCP), SF@35°C / density MMCP , below 0.007, preferably below 0.006, more preferably below 0.005, for example in the range of 0.001 to below 0.007, preferably 0.001 to below 0.006, more preferably 0.001 to below 0.005.
[0077] The amount of the soluble fraction is in the range of 0.5 to 6.0 wt%, preferably 0.8 to 5.0 wt%, more preferably 1.0 to 4.0 wt%, based on the total multimodal polyethylene copolymer (MMCP).
[0078] In one embodiment of the invention the multimodal polyethylene copolymer (MMCP) is further characterized in that the ratio of the molecular weight (Mw) of the low crystalline fraction (LCF) to the molecular weight (Mw) of the high crystalline fraction (HCF), Mw(Tp(LCF) / Mw(Tp(HCF), determined as described in the experimental part, is in the range of >1.3 to 10.0, preferably in the range of 2.0 to 8.0, more preferably in the range of 2.2 to 6.0, and / or the ratio of the half peak width (LCF) / (98-Tp(LCF)) is in the range of 0.10 to 1.50, preferably in the range of 0.15 to 1.2, more preferably in the range of 0.20 to 1.0, and / or
[0079] The difference of Mw(LCF)-Mw(HCF) is at least 31,000 and at most 200,000 g / mol, preferably 50,000 to 180,000 g / mol, more preferably 80,000 to 150,000 g / mol.
[0080] Preferably, the multimodal polyethylene copolymer (MMCP) is additionally characterised by at least 2 of the above mentioned parameters, more preferably by all 3 of the above mentioned parameters.
[0081] Definition of High Crystalline Fraction (HCF) and Low Crystalline Fraction (LCF):
[0082] High crystalline fraction (HCF) is the amount (in wt%) of the polymer fraction with a crystallization temperature above 90°C,
[0083] It mainly contains one or more homopolymeric polyethylene chains with a very low branching content.
[0084] The low crystalline fraction (LCF) is then the amount (in % by weight) of the polymer fraction having a crystallization temperature of 30 to below 90°C.
[0085] Within the scope of the present invention, the first and second ethylene polymer parts (A-1 and A-2) of the ethylene polymer component (A) are present in a weight ratio of 4:1 to 1:4, such as 3:1 to 1:3, or 2:1 to 1:2, or 1:1.
[0086] The ethylene polymer component (A) is present in an amount of 35.0 to 50.0 wt.-%, preferably in an amount of 36.0 to 48.0 wt.-%, even more preferably in an amount of 38.0 to 45.0 wt.-%, based on the multimodal copolymer (MMCP).
[0087] Accordingly, the ethylene polymer component (B) is present in an amount of 50.0 to 65.0 wt.-%, preferably in an amount of 52.0 to 64.0 wt.-%, more preferably in an amount of 55.0 to 62.0 wt.-%, based on the multimodal copolymer (MMCP).
[0088] The metallocene-catalyzed multimodal copolymer (MMCP) can be produced in a two-stage process, which preferably comprises a slurry reactor (loop reactor), wherein the slurry (loop) reactor is connected in series with a gas phase reactor (GPR), whereby ethylene polymer component (A) is produced in the loop reactor and ethylene polymer component (B) is produced in the GPR in the presence of ethylene polymer component (A) to produce the multimodal copolymer (MMCP).
[0089] In case the ethylene component (A) of the multimodal copolymer (MMCP) consists of ethylene polymer fractions (A-1) and (A-2), the multimodal copolymer (MMCP) may be produced in a three-stage process, which preferably comprises a first slurry reactor (loop reactor 1), wherein the first slurry loop reactor is connected in series to a further slurry reactor (loop reactor 2) such that the first ethylene polymer fraction (A-1) produced in the loop reactor 1 is fed to the loop reactor 2, where the second ethylene polymer fraction (A-2) is produced in the presence of the first fraction (A-1). Thus, the loop reactor 2 is connected in series to a gas phase reactor (GPR) such that the first ethylene polymer fraction (A) leaving the second slurry reactor is fed to the GPR, to produce a trimodal polyethylene copolymer. In this case, the reaction conditions in the two slurry reactors are selected such that products different in MFR and / or density are produced in the two slurry reactors.
[0090] Such processes are described in particular in WO 2016 / 198273 A1, WO 2021 / 009189 A1, WO 2021 / 009190 A1, WO 2021 / 009191 A1 and WO 2021 / 009192. Full details on how to prepare suitable metallocene-catalyzed multimodal copolymers (MMCPs) can be found in these references.
[0091] Metallocene-catalyzed multimodal copolymers (MMCPs) are produced by using a metallocene catalyst. The metallocene catalyst preferably comprises a metallocene complex and a cocatalyst. The metallocene compound or complex is also referred to herein as an organometallic compound (C).
[0092] The organometallic compound (C) comprises a transition metal (M) from Groups 3 to 10 of the Periodic Table of Elements (IUPAC 2007) or from the actinides or lanthanides.
[0093] According to the present invention, the term "organometallic compound (C)" includes any metallocene or non-metallocene compound of a transition metal, which carries at least one organic (coordinating) ligand and exhibits catalytic activity alone or together with a cocatalyst. Transition metal compounds are well known in the art, and the present invention encompasses compounds of metals from Groups 3 to 10, e.g. Groups 3 to 7, or Groups 3 to 6, e.g. Groups 4 to 6, of the Periodic Table (IUPAC 2007), as well as lanthanides or actinides.
[0094] In one embodiment, the organometallic compound (C) has the following formula (I):
[0095]
[0096] Wherein each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 - alkoxy, phenyl or benzyl;
[0097] Each Het is independently a monocyclic heteroaromatic group containing at least one heteroatom selected from O or S;
[0098] L is -R'2Si-, wherein each R' is independently a C substituted with an alkoxy group having 1 to 10 carbon atoms. 1-20 -Hydrocarbon or C 1-10 -alkyl;
[0099] M is Ti, Zr or Hf;
[0100] Each R 1 Same or different, is C 1-6 -alkyl or C 1-6 - alkoxy;
[0101] Each n is 1 to 2;
[0102] Each R 2 Same or different, is C 1-6 -alkyl, C 1-6 -alkoxy or -Si(R)3 group;
[0103] Each R is optionally replaced by 1 to 3 C 1-6-alkyl substituted C 1-10 - alkyl or phenyl; and
[0104] Each p is from 0 to 1.
[0105] Preferably, the compound of formula (I) has the structure
[0106]
[0107] Wherein each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 - alkoxy, phenyl or benzyl;
[0108] L is Me2Si-;
[0109] Each R 1 Same or different and C 1-6 - alkyl, for example methyl or tert-butyl;
[0110] Each n is 1 to 2;
[0111] R 2 is -Si(R)3alkyl; each p is 1;
[0112] Each R is C 1-6 -alkyl or phenyl.
[0113] Highly preferred complexes of formula (I) are
[0114]
[0115]
[0116] Most preferably, the complex dimethylsilanediylbis-[2-(5-trimethylsilylfuran-2-yl)-4,5-dimethylcyclopentadien-1-yl]zirconium dichloride is used.
[0117] More preferably, the ethylene polymer components (A) and (B) of the multimodal copolymer (MMCP) are prepared using, ie in the presence of, the same metallocene catalyst.
[0118] To form the catalyst, a cocatalyst, also called an activator, well known in the art is used. Cocatalysts containing Al or B are well known and can be used here. Preferably, an aluminoxane (such as MAO) or a boron-based cocatalyst (such as a borate) is used.
[0119] In contrast to Ziegler Natta catalysis, polyethylene copolymers produced using single-site catalysis have characteristics that distinguish them from Ziegler Natta materials. In particular, the comonomer distribution is more uniform. This can be shown using TREF or Crystaf techniques. Catalyst residues can also indicate the catalyst used. Ziegler Natta catalysts do not contain group (IV) metals such as Zr or Hf.
[0120] Plastic body
[0121] The sealing layer of the multilayer film according to the invention comprises a specific plastomer. Other layers may also comprise said plastomer.
[0122] The sealing layer comprises 15 to 85 wt% of a plastomer based on the total weight of the sealing layer (SL), the plastomer being a copolymer of ethylene and a C3-C8 α-olefin; having a molecular weight of 870 to 900 kg / m 3 range (ASTM D792), MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 10.0 g / 10 min; and a melting point in the range of 65 to 80°C (measured by DSC as described in the specification).
[0123] According to a preferred embodiment of the present invention, the plastomer is a copolymer of ethylene and 1-octene and has one or more of the following characteristics:
[0124] 1-octene content in the range of 18 to 45 wt. %, preferably in the range of 20 to 30 wt. %, based on the total weight of the copolymer; and / or
[0125] Density (ASTM D792) 870 to 890 kg / m 3 In the range of 880 to 886 kg / m 3 within the scope; and / or
[0126] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 5.0 g / 10 min, preferably in the range of 0.5 to 1.5 g / 10 min; and / or
[0127] - Melting point (measured by DSC as described in the specification) in the range of 68 to 77°C, preferably in the range of 71 to 75°C.
[0128] Plastomers according to the invention are commercially available, for example under the trade name Queo (eg Queo 8201) from Borealis.
[0129] Alternatively, suitable vinyl plastomers can be prepared by known methods in a one-stage or two-stage polymerization process including solution polymerization, slurry polymerization, gas phase polymerization or a combination thereof in the presence of a suitable catalyst known to those skilled in the art (such as a vanadium oxide catalyst or a single-site catalyst, such as a metallocene or a constrained geometry catalyst).
[0130] Preferably, the ethylene-based plastomer is prepared by a one-stage or two-stage solution polymerization process, in particular by a high temperature solution polymerization process at a temperature above 100°C.
[0131] Such a process is essentially based on polymerizing monomers and suitable comonomers in a liquid hydrocarbon solvent in which the resulting polymer is soluble. The polymerization is carried out at a temperature above the melting point of the polymer, resulting in a polymer solution. This solution is flashed in order to separate the polymer from the unreacted monomers and the solvent. The solvent is then recovered in the process and recycled.
[0132] The plastomers of the present invention are ideally formed using metallocene-type catalysts. Known solution technologies suitable for use in the process of the present invention are Borceed TM technology.
[0133] Multilayer film
[0134] A preferred embodiment of the multilayer film according to the invention provides that the thickness of the skin layer (SKL) of the multilayer film is in the range of 1 to 100 μm, preferably in the range of 5 to 80 μm, more preferably in the range of 10 to 15 μm.
[0135] According to another preferred embodiment of the present invention, the thickness (CL) of the core layer of the multilayer film is in the range of 10 to 200 μm, preferably in the range of 20 to 80 μm, more preferably in the range of 30 to 45 μm.
[0136] In another preferred embodiment according to the present invention, the thickness of the sealing layer of the multilayer film is in the range of 1 to 50 μm, preferably in the range of 5 to 25 μm, more preferably in the range of 10 to 15 μm.
[0137] In another preferred embodiment according to the present invention, the thickness of the multilayer film is in the range of 12 to 350 μm, preferably in the range of 40 to 150 μm, more preferably in the range of 50 to 70 μm.
[0138] According to another preferred embodiment of the present invention, the multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL).
[0139] The skin layer (SKL) preferably comprises 80 to 95 wt.-%, more preferably 82 to 93 wt.-%, still more preferably 88 to 92 wt.-% of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), based on the total weight of the skin layer (SKL); and 5 to 20 wt.-%, preferably 7 to 18 wt.-%, more preferably 8 to 12 wt.-% of a LDPE having a density of 910 to 930 kg / m 3 , preferably 920 to 925 kg / m 3 The MFR2 (190°C, 2.16 kg, ISO 1133) is in the range of 0.5 to 4.0 g / 10 min, preferably in the range of 0.5 to 1.0 g / 10 min.
[0140] The core layer (CL) preferably comprises 10 to 35 wt%, more preferably 15 to 30 wt%, still more preferably 18 to 25 wt%, based on the total weight of the core layer (CL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP); and 65 to 90 wt%, preferably 70 to 85 wt%, more preferably 75 to 82 wt%, based on the total weight of the core layer (CL), of a Ziegler-Natta-catalyzed linear low density polyethylene, preferably a multimodal α-olefin terpolymer and preferably having a molecular weight in the range of 920 to 970 kg / m 3 , preferably 930 to 938 kg / m 3 and a density in the range of 0.1 to 2.5 g / 10 min, preferably in the range of 0.5 to 1.2 g / 10 min (190° C., 2.16 kg, ISO 1133).
[0141] According to another preferred embodiment of the present invention, the skin layer (SKL), the core layer (CL) and the sealing layer (SL) comprise a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), preferably, the multilayer film consists of a polyethylene-based polymer. It goes without saying that the core layer (CL) is located between the skin layer (SKL) and the sealing layer (SL).
[0142] According to another preferred embodiment of the present invention, the content of MMCP (a) in the sealing layer (SL) is in the range of 20 to 40 wt.% or 60 to 80 wt.%, preferably in the range of 25 to 35 wt.% or 65 to 75 wt.%, more preferably in the range of 28 to 32 wt.% or 68 to 72 wt.%, based on the total weight of the sealing layer; and / or the content of plastomer (b) in the sealing layer (SL) is in the range of 20 to 40 wt.% or 60 to 80 wt.%, preferably in the range of 25 to 35 wt.% or 65 to 75 wt.%, more preferably in the range of 28 to 32 wt.% or 68 to 72 wt.%, based on the total weight of the sealing layer.
[0143] According to another preferred embodiment of the present invention, the multilayer film has an MD tensile modulus (ISO 527-3) in the range of 150 to 300 MPa, preferably in the range of 250 to 290 MPa; and / or a TD tensile modulus (ISO 527-3) in the range of 150 to 400 MPa, preferably in the range of 300 to 350 MPa; and / or a dart drop strength (ISO 7765-1) in the range of 500 to 2000 g, preferably in the range of 1100 to 1700 g, more preferably in the range of 1500 to 1600 g, even more preferably in the range of 500 to 1550 g.
[0144] In another preferred embodiment according to the present invention, the multilayer film has a haze (ASTM D1003-00) in the range of 5% to 15%, preferably in the range of 10% to 13%; and / or a seal initiation temperature determined as described in the specification in the range of 50 to 85°C, preferably in the range of 55 to 73°C, more preferably in the range of 56 to 72°C; and / or a hot tack force determined as described in the specification in the range of 4 to 12N, preferably in the range of 5 to 8N; and / or a hot tack temperature determined as described in the specification in the range of 60 to 90°C, preferably in the range of 65 to 88°C.
[0145] The polymers used in the multilayer articles according to the invention may contain additives and fillers in amounts which are customary in the field of film applications. Examples of such additives are, inter alia, antioxidants, processing stabilizers, UV stabilizers, pigments, fillers, antistatic additives, antiblocking agents, nucleating agents, acid scavengers and polymer processing aids (PPAs).
[0146] It should be understood herein that any additive and / or filler may optionally be added in the form of a so-called masterbatch comprising the respective additive(s) and a carrier polymer. In this case, the carrier polymer is not calculated in the polymer component of the metallocene-catalyzed multimodal polyethylene copolymer (MMCP), but in the amount of the respective additive, based on the total amount of the polymer composition (100 wt %).
[0147] method
[0148] Another aspect of the invention relates to a method for producing a multilayer article.
[0149] The multilayer films according to the invention are generally produced by conventional processes in which the layers of the film are coextruded.
[0150] The different polymer components in any layer of the film are usually intimately mixed before the layer is formed, for example using a twin screw extruder, preferably a counter-rotating extruder or a co-rotating extruder. The blend is then converted into a coextruded film.
[0151] Generally, the multilayer film according to the invention can be produced by a blown film or cast film process, preferably by a blown film process.
[0152] To make such films, at least three polymer melt streams are simultaneously extruded (ie, coextruded) through, for example, a multi-channel tubular, annular or circular die to form a tube which is inflated, expanded and / or cooled with air to form the film. The manufacture of blown films is a well-known process.
[0153] Blown (co)extrusion may be carried out at a temperature of 150 to 230°C, more preferably 160 to 225°C, and cooled by blowing gas (typically air) at a temperature of 10 to 40°C, more preferably 12 to 16°C, to provide a frost line height of 0.5 to 4 times, more preferably 1 to 2 times, the die diameter.
[0154] The blow up ratio (BUR) should generally be in the range of 1.5 to 3.5, preferably 2.0 to 3.0, more preferably 2.1 to 2.8.
[0155] use
[0156] Another aspect of the present invention relates to the use of the multilayer film as packaging material, preferably for food and / or medical products.
[0157] The invention will now be described with reference to the following non-limiting examples.
[0158] Experimental Section
[0159] A. Test Method
[0160] Unless otherwise defined, the following definitions of terms and determination methods apply to the above general description of the invention as well as to the following examples.
[0161] Melt flow rate:
[0162] The melt flow rate (MFR) is determined according to ISO 1133 - Thermoplastics - Determination of melt mass-flow rate (MFR) and melt volume-flow rate (MVR) - Part 1: Standard method and is expressed in g / 10 min. The MFR is an indication of the flowability of the polymer and therefore of its processability. The higher the melt flow rate, the lower the viscosity of the polymer. The MFR of polyethylene is determined at 190°C. The MFR can be determined at different loads, for example 2.16 kg (MFR2), 5 kg (MFR5) or 21.6 kg (MFR 21 ).
[0163] Calculation of MFR2 of component B and part (A-2)
[0164] logA=x·logB+(1-x)·logC
[0165]
[0166] For component B:
[0167] B = MFR2 of component (A)
[0168] C = MFR2 of component (B)
[0169] A = Final MFR2 of the multimodal polyethylene copolymer (MMCP) (blend)
[0170] X = weight fraction of component (A)
[0171] For part (A-2):
[0172] B = MFR2 of the first part (A-1)
[0173] C = MFR2 of the second part (A-2)
[0174] A = Final MFR2 of cyclic polymer (= component (A)) (mixture)
[0175] X = weight fraction of the first part (A-1).
[0176] density
[0177] The density of the polymer is measured in kg / m according to ASTM; D792, method B (density at 23°C by balance) on compression molded specimens prepared according to EN ISO 1872-2. 3 .
[0178] DSC analysis, melting temperature (T m ) and crystallization temperature (T c )
[0179] Data can be measured with a TA Instruments Q2000 Differential Scanning Calorimetry (DSC) on 5 to 7 mg samples.DSC is run according to ISO 11357 / Part 3 / Method C2 in the temperature range of -30 to +225°C with a scan rate of 10°C / min in a hot / cold / hot cycle.
[0180] Crystallization temperature (T c ) and crystallization enthalpy (H c ) is determined by the cooling step, while the melting temperature (T m ) and melting enthalpy (H m ) is determined by the second heating step.
[0181] Dart Drop Intensity (DDI): Determination of impact resistance by free falling dart method
[0182] DDI was measured according to ISO 7765-1:1988 / Method A on films produced as shown below. This test method covers the determination of the energy that will cause film failure under specified conditions of impact by a dart falling freely from a specified height, which will cause 50% of the test specimens to fail (Step Method A). A uniform increment of the missile mass was used during the test, and after each specimen test, the missile weight was reduced or increased by a uniform increment depending on the observed result (failure or no failure) of the specimen.
[0183] Standard conditions:
[0184] Adjustment time: >96h
[0185] Test temperature: 23℃
[0186] Dart head material: phenolic resin
[0187] Dart diameter: 38mm
[0188] Drop height: 660mm
[0189] result:
[0190] Impact failure weight - 50% [g]
[0191] Tensile modulus (TM)
[0192] The tensile modulus (MPa) of film samples (prepared as described below) was measured in the machine direction (MD) and / or transverse direction (TD) according to ISO 527-3 with a film thickness of 60 μm and a crosshead speed of 1 mm / min.
[0193] Haze
[0194] The haze was measured according to ASTM D 1003-00 on the blown films as described below.
[0195] Sealing start temperature (SIT); Sealing end temperature (SET), Sealing range
[0196] This method determines the sealing temperature range (sealing range) of polyethylene films, in particular blown films or cast films. The sealing temperature range is the temperature range over which the film can be sealed according to the conditions given below.
[0197] The lower limit (heat seal initiation temperature (SIT)) is the sealing temperature at which a seal strength of ≥ 5 N is achieved. The upper limit (seal end temperature (SET)) is reached when the film sticks to the sealing device.
[0198] The measurements were performed according to a slightly modified ASTM F1921-12, where the test parameters sealing pressure, cooling time and test speed were modified. The force / temperature curve was continued until thermal failure of the membrane.
[0199] The sealing range was determined on a J&B Universal Sealer Model 4000 on a 60 μm thick blown film, using the following additional parameters:
[0200] Adjustment time: >96h
[0201] Sample width: 25mm
[0202] Sealing pressure: 0.4N / mm 2 (PE)
[0203] Sealing time: 1 second
[0204] Delay time: 30 seconds
[0205] Sealing jaws size: 50x5 mm
[0206] Sealing jaws shape: flat
[0207] Sealing jaw coating: Niptef
[0208] Sealing temperature: ambient temperature -240℃
[0209] Sealing temperature interval: 5°C
[0210] Starting temperature: 50℃
[0211] Grip separation rate: 42 mm / sec
[0212] Hot Tack Temperature (HTT) and Hot Tack Force (HTF)
[0213] HTT (lowest temperature to obtain maximum hot tack) and HTF (maximum hot tack) were measured on three-layer blown films with a thickness of 60 μm according to ASTM F 1921 method B with the following settings:
[0214] Q-name Instrument: Hot Tack-Seal Tester
[0215] Model: J&B model 4000MB
[0216] Sealing strip length: 50[mm]
[0217] Sealing strip width: 5[mm]
[0218] Sealing strip shape: flat
[0219] Sealing pressure: 0.15N / mm 2
[0220] Sealing time: 1s
[0221] Sealing strip coating:
[0222] Roughness of coated seal strip 1[μm]
[0223] Film sample width: 25mm
[0224] Cooling time: 0.2s
[0225] Peeling speed: 200mm / s
[0226] Starting temperature: 50℃
[0227] End temperature: burn-through and / or shrinkage
[0228] Increment: 5℃
[0229] All film samples were prepared in a standard atmosphere for conditioning and testing at 23°C (±2°C) and 50% (±10%) relative humidity. The minimum conditioning time for the samples in the standard atmosphere before testing was at least 40 hours. The minimum standing time between extrusion of the film samples and the start of testing was at least 88 hours. The hot tack measurement determines the strength of the heat seal formed in the film and is performed immediately after the seal is completed and before it cools to ambient temperature.
[0230] The HTF is measured as a function of temperature within a temperature range and with temperature increments as described above. The number of test specimens per temperature is at least 3. The HTF is evaluated as the maximum force (maximum peak value) at failure mode "peeling".
[0231] Comonomer content - quantification of microstructure by NMR spectroscopy
[0232] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers.
[0233] A Bruker Avance III 400 MHz NMR spectrometer was used to analyze the 1 H and 13 C was operated at 500.13 and 125.76 MHz and quantitative data were recorded in the molten state. 13 C{ 1 H}NMR spectra. All spectra were obtained using 13The spectra were recorded at 150 °C using a C-optimized 7 mm magic angle spinning (MAS) probe head with nitrogen used for all pneumatics. Approximately 200 mg of material was loaded into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification {klimke06, parkinson07, castignolles09}. Standard single pulse excitation was used, utilizing NOE {pollard04, klimke06} with a short recycle delay of 3 s and an RS-HEPT decoupling scheme {fillip05, griffin07}. A total of 1024 (1k) transients were acquired for each spectrum.
[0234] Quantitative 13 C{ 1 H} NMR spectra were processed, integrated, and the relevant quantitative properties were determined from the integration. All chemical shifts were internally referenced to the bulk methylene signal (δ+) at 30.00 ppm.
[0235] The amount of ethylene is quantified using the integration of the methylene (δ+) sites at 30.00 ppm and taking into account the number of reported sites per monomer:
[0236] E=I δ+ / 2
[0237] Correction for the presence of isolated comonomer units is based on the number of isolated comonomer units present:
[0238] E total = E + (3 * B+2 * H) / 2
[0239] where B and H are defined for their respective comonomers. Corrections are made in a similar manner when there is continuous and discontinuous comonomer incorporation.
[0240] Characteristic signals corresponding to the incorporation of 1-butene were observed and the comonomer fraction was calculated as the fraction of 1-butene in the polymer relative to all monomers in the polymer:
[0241] fB total = (B total / (E total + B total + H total)
[0242] The amount of isolated 1-butene incorporated into the EEBEE sequence was quantified using the integration of the *B2 site at 39.8 ppm and taking into account the number of reporter sites per comonomer:
[0243] B=I *B2
[0244] If present, the amount of continuously incorporated 1-butene in the EEBBEE sequence was quantified using the integration of the ααB2B2 site at 39.4 ppm and taking into account the number of reported sites for each comonomer:
[0245] BB=2 * IααB2B2
[0246] If present, the amount of non-reporting sites per comonomer:
[0247] HEH=2 * IββB4B4
[0248] No HHH sequence was observed. The total 1-hexene content was calculated based on the sum of isolated, continuous and discontinuously incorporated 1-hexene:
[0249] Total H = H + HH + HEH
[0250] The total mole fraction of 1-hexene in the polymer was then calculated as:
[0251] fH=H total / (E total+B total+H total)
[0252] The mole percentage of comonomer incorporation is calculated from the mole fraction:
[0253] B [mol%] = 100 * f
[0254] H [mol%] = 100 * f
[0255] The weight percent of comonomer incorporation is calculated from the mole fraction:
[0256] B [wt%] = 100 * (fB * 56.11) / ((fB * 56.11)+(fH * 84.16)+((1-
[0257] (fB+fH)) * 28.05))
[0258] H [wt%] = 100 * (fH * 84.16) / ((fB * 56.11)+(fH * 84.16)+((1-
[0259] (fB+fH)) * 28.05))
[0260] References:
[0261] Klimke,K.,Parkinson,M.,Piel,C.,Kaminsky,W.,Spiess,H.W.,Wilhelm,M.,Macromol.Chem.Phys.2006;207:382.Parkinson,M.,Klimke,K.,Spiess,H.W.,Wilhelm,M.,Macromol.Chem.Phys.2007;208:2128.
[0262] Pollard,M.,Klimke,K.,Graf,R.,Spiess,H.W.,Wilhelm,M.,Sperber,O.,Piel,C.,Kaminsky,W.,Macromolecules 2004;37:813.
[0263] Filip,X.,Tripon,C.,Filip,C.,J.Mag.Resn.2005,176,239.
[0264] Griffin,J.M.,Tripon,C.,Samoson,A.,Filip,C.,and Brown,S.P.,Mag.Res.inChem.2007 45,S1,S198.
[0265] Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer50(2009)2373.
[0266] Busico,V.,Cipullo,R.,Prog.Polym.Sci.26(2001)443.
[0267] Busico,V.,Cipullo,R.,Monaco,G.,Vacatello,M.,Segre,A.L.,Macromoleucles30(1997)6251.
[0268] Zhou,Z.,Kuemmerle,R.,Qiu,X.,Redwine,D.,Cong,R.,Taha,A.,Baugh,D.Winniford,B.,J.Mag.Reson.187(2007)225.
[0269] Busico,V.,Carbonniere,P.,Cipullo,R.,Pellecchia,R.,Severn,J.,Talarico,G.,Macromol.Rapid Commun.2007,28,1128.
[0270] Resconi,L.,Cavallo,L.,Fait,A.,Pimontesi,F.,Chem.Rev.2000,100,1253.
[0271] Molecular weight, molecular weight distribution (M n 、M w , MWD)
[0272] Average molecular weight (M z 、M w and M n ), molecular weight distribution (MWD) and its polydispersity index PDI = M w / M n (where M n is the number average molecular weight, M w The width described by the weight average molecular weight (MW) obtained from GPC-LS was calculated by gel permeation chromatography (GPC) according to ASTM D 6474-12 using the following formula:
[0273]
[0274]
[0275]
[0276] For a constant elution volume interval ΔV i , where A i and M i and elution volume V i The associated chromatographic peak slice area and the polyolefin molecular weight (MW), where N equals the number of data points obtained from the chromatogram between the integration limits.
[0277] A high temperature GPC instrument equipped with an infrared (IR) detector (IR4 or IR5 from PolymerChar (Valencia, Spain)) or a differential refractometer (RI) from Agilent Technologies, equipped with 3x Agilent-PLgel Olexis and 1x Agilent-PLgel Olexis Guard columns was used. 1,2,4-Trichlorobenzene (TCB) stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol was used as solvent and mobile phase. The chromatographic system was operated at 160°C with a constant flow rate of 1 mL / min. 200 μL of sample solution was injected for each analysis. Data collection was performed using Agilent Cirrus software version 3.3 or PolymerChar GPC-IR control software.
[0278] The column set was calibrated using universal calibration with 19 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. The PS standards were dissolved at room temperature for several hours. The conversion of polystyrene peak molecular weight to polyolefin molecular weight was accomplished by using the Mark Houwink equation and the following Mark Houwink constants:
[0279] K PS =19x 10 -3 mL / g, α PS =0.655
[0280] K PE =39x 10 -3 mL / g, α PE =0.725
[0281] A third order polynomial fit was used to fit the calibration data.For PE, all samples were prepared in the concentration range of 0.5-1 mg / ml and dissolved at 160°C for 3 hours with continuous gentle shaking.
[0282] Determination of chemical heterogeneity by cross fractionation chromatography (CFC)
[0283] The chemical composition distribution at a certain elution temperature (polymer crystallinity in solution) as well as the determination of the molecular weight distribution and the corresponding molecular weight averages (Mn, Mw and Mv) were determined by fully automated cross-fractionation chromatography (CFC) as described in Ortin A., Monrabal B., Sancho-Tello J., Macromol. Symp., 2007, 257, 13-28.
[0284] Cross-fractionation chromatography (TREF xSEC) was performed using a CFC instrument (PolymerChar, Valencia, Spain). A four-band IR5 infrared detector (PolymerChar, Valencia, Spain) was used to monitor concentration. About 40 mg of polymer sample was dissolved in 25 ml of TCB for 150 min in a stainless steel container at 150 ° C. After the sample was completely dissolved, an aliquot of 0.5 ml was loaded into a TREF column and stabilized at 110 ° C for 60 min. By applying a constant cooling rate of 0.1 ° C / min, the polymer was crystallized and dropped to a temperature of 30 ° C. The following temperature steps were used for discontinuous elution: (35, 40, 45, 50, 53, 56, 59, 62, 64, 66, 69, 72, 76, 79, 82, 85, 89, 91, 93, 95, 97, 100, 110 and 120).
[0285] In the second dimension, GPC analysis used 3PL Olexis columns and 1x Olexis Guard columns from Agilent (Church Stretton, UK) as stationary phases. 1,2,4-Trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol) was applied as eluent at a constant flow rate of 1 mL / min at 150°C. The column set was calibrated using universal calibration (according to ISO 16014-2:2003) with at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. The following Mark Houwink constants were used to convert PS molecular weights to PE molecular weight equivalents.
[0286] K PS =19x 10 -3 mL / g, α PS =0.655
[0287] K PE =39x 10 -3 mL / g, α PE =0.725
[0288] A third order polynomial fit was used to fit the calibration data. Data processing was performed using software provided by PolymerChar and the CFC instrument.
[0289] Soluble part SF@35℃
[0290] The soluble fraction SF@35°C is the polymer fraction eluted at 35°C.
[0291] M w (Tp(LCF, M w(Tp(HCF), half peak width Tp(LCF), half peak width Tp(HCF)
[0292] In order to determine the weight average molecular weight at the maximum peak of the low crystalline part (Mw(Tp(LCF)) or the weight average molecular weight at the maximum peak of the high crystalline part (Mw(Tp(HCF)) and the half peak widths of Tp(LCF) and Tp(HCF) in the first step, an a-TREF curve is obtained from the above CFC analysis,
[0293] The peak maximum of the high crystalline fraction (HCF) peak (Tp(HCF)) and the peak maximum of the low crystalline fraction (LCF) peak (Tp(LCF)) are determined from the a-TREF curve. The elution temperature of Tp(HCF) is higher than that of Tp(LCF) but lower than 99° C. Generally, the high crystalline fraction is in the range of 90° C. to 99° C., and the low crystalline fraction is a polymer fraction eluted from 35° C. to 90° C.
[0294] The half-peak width of HCF and LCF is defined as the elution temperature difference between the front temperature and the back temperature at half the maximum peak height of Tp(LCF) or Tp(HCF), respectively. If the peaks are not well separated, the corresponding front temperature at half the maximum is taken from 35°C forward, while the back temperature at half the maximum is taken from 100°C backward. If LCF is well separated from HCF, the back temperature is taken after HCF.
[0295] In the next step, the Mw at the elution temperatures Tp(LCF) and Tp(HCF) is determined. Thus, the Mw at Tp(LCF) (Mw(Tp(LCD)) is calculated by linear interpolation between the Mw values measured by GPC at elution temperatures above Tp(LCF) and below Tp(LCF). This is achieved by using the "TREND" function in Excel. The same procedure is performed to determine the Mw at Tp(HCF).
[0296] Based on the determined Mw(Tp(LCF), Mw(Tp(HCF), half-peak width(LCF), half-peak width(HCF) and Tp(LCF), the following parameters can be directly calculated:
[0297] -M w (Tp(LCF) / M w (Tp(HCF)
[0298] -M w (TP(LCF))-M w (Difference of TP(HCF) (g / mol) = M w (TP(LCF)-M w (TP(HCF)[g / mol]
[0299] - Half peak width (LCF) / (98°C - Tp (LCF)).
[0300] B. Materials used
[0301] FT5236 is a low density polyethylene (MFR2 (190°C / 2.16kg): 0.75g / 10min, density: 923kg / m 3 , T m 112°C, produced by Tubular Technology) and contains anti-blocking agents, antioxidants and slip additives.
[0302] FX1001 is a product available from Borealis AG as BorShape TM FX1001 purchased multimodal α-olefin terpolymer (MFR5 (190℃ / 5kg): 0.9g / 10min, density: 931kg / m 3 , T m 127°C, produced with a Ziegler-Natta catalyst) and contains an antioxidant.
[0303] Queo0201 is a product available from Borealis AG as Queo TM 0201 Single-modal vinyl 1-octene plastomer (MFR2 (190℃ / 2.16kg): 1.1g / 10min, density: 902kg / m 3 , T m 97°C, produced in a solution polymerization process using a metallocene catalyst, C8 content: 16.1 wt% based on the total weight of the copolymer = 4.6 mol%) and containing a processing stabilizer.
[0304] Queo8201 is a product available from Borealis AG as Queo TM 0201 Single-modal vinyl 1-octene plastomer (MFR2 (190℃ / 2.16kg): 1.1g / 10min, density: 883kg / m 3 , T m 73°C, produced in a solution polymerization process using a metallocene catalyst, C8 content: 26.3 wt% based on the total weight of the copolymer = 8.2 mol%) and containing a processing stabilizer.
[0305] Anteo TM FK1820: A bimodal ethylene / 1-butene / 1-hexene terpolymer commercially available from Borouge with a density of 918 kg / m 3, MFR2 is 1.5g / 10min.
[0306] MMCP is a multimodal copolymer prepared as follows.
[0307] Catalyst preparation (CAT)
[0308] SiO2 loading:
[0309] 10 kg of silica (PQ Corporation ES757, calcined at 600°C) was added from a feed bucket and inerted in the reactor until the O2 level reached less than 2 ppm.
[0310] Preparation of MAO / tol / MC:
[0311] At 25°C (oil circulation temperature) and 95rpm stirring, a 30 wt% MAO toluene solution (14.1kg) was added from a balance to another reactor, followed by toluene (4.0kg). After the addition of toluene, the stirring speed was increased from 95rpm to >200rpm, with a stirring time of 30 minutes. 477g of metallocene racemic-dimethylsilanediylbis{2-(5-(trimethylsilyl)furan-2-yl)-4,5-dimethylcyclopentadiene-1-yl}zirconium dichloride was added from a metal cylinder, followed by 4kg of toluene rinse (total toluene was 8.0kg). The reactor stirring speed was changed to 95rpm for MC feeding, returned to 200rpm and continued for 3h reaction time. After the reaction time, the MAO / tol / MC solution was transferred to a feed container.
[0312] Preparation of catalyst:
[0313] The reactor temperature was set to 10°C (oil circulation temperature) and stirring was adjusted to 40 rpm during the addition of MAO / tol / MC. MAO / tol / MC solution (22.2 kg) was added over 205 minutes, followed by a stirring time of 60 minutes (oil circulation temperature was set to 25°C). After stirring, the "dry mix" was stabilized at 25°C (oil circulation temperature) for 12 hours with a stirring speed of 0 rpm. The reactor was rotated 20° (back and forth) and stirred several times per hour at a speed of 5 rpm.
[0314] After stabilization, the catalyst was dried at 60°C (oil circulation temperature) for 2 hours under a 2 kg / h nitrogen flow, followed by 13 hours under vacuum (same nitrogen flow rate, stirring at 5 rpm). The dried catalyst was sampled and the HC content was measured using a Sartorius moisture analyzer (model MA45) in a glove box using thermogravimetry. The target HC level was <2% (actual 1.3%).
[0315] polymerization:
[0316] The polymerization was carried out in a Borstar pilot plant with a 3-reactor set-up (Loop 1 - Loop 2 - GPR) and a prepolymerization loop reactor according to the conditions given in Table 1.
[0317] Table 1: Polymerization conditions
[0318]
[0319] The polymer (MMCP) was mixed with 2400 ppm of Irganox B561 (available from BASF SE), 270 ppm of Dynamar FX5922 (available from 3M), compounded and extruded into pellets using a JSW extruder under nitrogen atmosphere to give a SEI of 230 kWh / kg and a melt temperature of 250° C. Table 2 summarizes some properties of the MMCP.
[0320] Table 2: Properties of multimodal copolymers
[0321] characteristic unit MMCP <![CDATA[MFR2]]> g / 10min 0.63 <![CDATA[MFR 21 ]]> g / 10min 28.5 <![CDATA[MFR 21 / MFR2]]> - 43.8 density <![CDATA[kg / m 3 ]]> 916.7 C4 mol% 0.6 C6 mol% 2.9 C4 weight% 1.2 C6 weight% 8.2 <![CDATA[M n ]]> g / mol 16000 <![CDATA[M w ]]> g / mol 103000 <![CDATA[M w / M n ]]> - 6.5 Tp(LCF) ℃ 54.5 Half peak width (LCF) ℃ 12.7 Mw(Tp(LCF) / Mw(Tp(HCF)* - 4.96 Difference Mw(TP(LCF))-Mw(TP(HCF)* g / mol 136000 Half peak width (LCF) / (98-Tp(LCF)* - 0.29 <![CDATA[SF@35℃ / Density P > - 0.003 SF@35℃ weight% 2.85
[0322] C. Fabrication of three-layer membrane
[0323] 3-layer films with a total thickness of 60 μm and the composition shown in Table 3 were produced on a Collin 3-layer lab line (melt temperature: 210° C., BUR 1:2.5, absorption speed: 7 m / min).
[0324] D. Results
[0325] Table 3: Composition and properties of the three-layer membrane
[0326]
[0327] Weight % is based on the weight of the entire film
[0328] E. Discussion of Results
[0329] All produced 3-layer films have the same skin layers (except CE3 with FK1820 instead of MMCP) and core layers. The sealing layers of the films according to the invention (IE1 and IE2) contain a blend of a specific metallocene-catalyzed multimodal polyethylene copolymer (MMCP) and a specific plastomer, while the sealing layers of the films according to the comparative examples (CE1 and CE2) contain the same metallocene-catalyzed multimodal polyethylene copolymer (MMCP) and a blend of different plastomers, or only MMCP, CE3 contains FK1820 instead of MMCP and a blend of different plastomers. The use of different plastomers (CE2 and CE3) results in a significant reduction in the toughness of the film. Furthermore, the use of specific plastomers according to the invention allows obtaining films with improved sealing properties.
[0330] Furthermore, the use of specific MMCPs can improve sealing performance and toughness compared to commercial metallocene-catalyzed FK1820.
Claims
1. A multilayer film comprising a skin layer (SKL), a core layer (CL) and a sealing layer (SL); wherein the sealing layer (SL) comprises (a) 15 to 85 wt.-%, based on the total weight of the sealing layer (SL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP) consisting of (i) 35.0 to 50.0 wt% of an ethylene-1-butene polymer component based on the total weight of the MMCP (A); and (ii) 50.0 to 65.0 wt% of an ethylene-1-hexene polymer component based on the total weight of the MMCP (B); The ethylene-1-butene polymer component (A) has ·920 to 960 kg / m 3 Density within the range (ASTM D792); MFR in the range of 3.0 to 300.0 g / 10min 2 (190℃, 2.16kg, ISO 1133); · a 1-butene content in the range of 0.1 to 3.0 mol% based on the ethylene-1-butene polymer component (A); and The ethylene-1-hexene polymer component (B) has 880 to 920 kg / m 3 Density within the range (ASTM D792); MFR in the range of 0.001 to 1.0 g / 10 min 2 (190℃, 2.16kg, ISO 1133); · a 1-hexene content in the range of 2.5 to 10.0 mol% based on the ethylene-1-hexene polymer compound (B); and The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has ·910 to 930 kg / m 3 Density within the range (ASTM D792); MFR in the range of 0.1 to 2.0 g / 10min 2 (190°C, 2.16kg, ISO 1133); and MFR in the range of 22 to 70 21 (190℃, 21.6kg, ISO 1133) and MFR 2 Ratio MFR (190℃, 2.16kg, ISO1133) 21 / MFR 2 ;and (b) 15 to 85 wt. % of a plastomer, based on the total weight of the sealing layer (SL), which is a copolymer of ethylene and a C3-C8 alpha olefin; having 870 to 900 kg / m 3 Density within the range (ASTM D792); MFR in the range of 0.1 to 10.0 g / 10min 2 (190°C, 2.16kg, ISO 1133); and a melting point in the range of 65 to 80°C (measured by DSC as described in the specification); and; The weight proportions of components (a) and (b) add up to 100% by weight.
2. The multilayer film according to claim 1, It is characterized in that The plastomer (b) is a copolymer of ethylene and 1-octene and has one or more of the following characteristics: 1-octene content in the range of 18 to 45 wt. %, based on the total weight of the copolymer, Preferably in the range of 20 to 30 wt. %; and / or Density (ASTM D792) 870 to 890 kg / m 3 In the range of 880 to 886 kg / m 3 within the scope; and / or MFR 2 (190°C, 2.16kg, ISO 1133) in the range of 0.1 to 5.0g / 10min, Preferably in the range of 0.5 to 1.5 g / 10 min; and / or - Melting point (measured by DSC as described in the specification) in the range of 68 to 77°C, preferably in the range of 71 to 75°C.
3. The multilayer film according to claim 1 or 2, It is characterized in that The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has a ratio of the soluble fraction at 35°C to the density of the MMCP, SF@35°C / density, determined by cross fractionation chromatography (CFC) as described in the experimental section, of less than 0.
007. MMCP , wherein the amount of the soluble portion at 35° C. is in the range of 0.5 to 6.0 wt % based on the total weight of the MMCP.
4. The multilayer film according to any one of the preceding claims, It is characterized in that The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has The molecular weight of the low crystalline fraction (LCF) determined as described in the experimental part (M) in the range of >1.3 to 10.0 w ) and the molecular weight of the high crystalline fraction (HCF) (M w ) ratio, M w (Tp(LCF) / M w (Tp(HCF), and / or a width at half height ratio (LCF) / (98-Tp(LCF)) in the range of 0.10 to 1.50, and / or • A difference of Mw(LCF)-Mw(HCF) of at least 31,000 and at most 200,000 g / mol.
5. The multilayer film according to any one of the preceding claims, It is characterized in that The ethylene-1-butene polymer component (A) of the metallocene-catalyzed multimodal polyethylene copolymer (MMCP) (a) consists of an ethylene polymer fraction (A-1) and an ethylene polymer fraction (A-2); wherein The ethylene polymer portion (A-1) preferably has 925 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 Density within the range (ASTM D792); and / or MFR in the range of 3.0 to 300.0 g / 10 min, preferably 100 to 150 g / 10 min, more preferably 115 to 125 g / 10 min 2 (190°C, 2.16 kg, ISO 1133), and / or The ethylene polymer portion (A-2) preferably has 925 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 Density within the range (ASTM D792), and / or MFR in the range of 3.0 to 300.0 g / 10 min, preferably 100 to 150 g / 10 min, more preferably 115 to 125 g / 10 min 2 (190℃, 2.16kg, ISO 1133).
6. The multilayer film according to any one of the preceding claims, It is characterized in that Metallocene-catalyzed multimodal copolymers (MMCP) (a) have Based on the multimodal polymer (MMCP) in the range of 0.1 to 1.0 mol%, preferably 0.2 to 0.8 mol%, More preferably the total amount of 1-butene is in the range of 0.3 to 0.7 mol%; and / or Based on the multimodal polymer (MMCP) in the range of 1.5 to 8.0 mol%, preferably 2.0 to 6.0 mol%, More preferably a total amount of 1-hexene in the range of 2.2 to 4.0 mol%; and / or 35 to 50 wt %, preferably 36 to 48 wt %, more preferably 38 to 45 wt % of the ethylene-1-butene polymer component (A) based on the total weight of the MMCP; and / or 50 to 65 wt %, preferably 52 to 64 wt %, more preferably 55 to 62 wt % of the ethylene-1-hexene polymer component (B) based on the total weight of the MMCP.
7. The multilayer film according to any one of the preceding claims, It is characterized in that The metallocene-catalyzed multimodal copolymer (MMCP) (a) is produced in the presence of a metallocene complex of formula (I): Wherein each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 -alkoxy, phenyl or benzyl; each Het is independently a monocyclic heteroaromatic group containing at least one heteroatom selected from O or S; L is -R' 2 Si-, wherein each R' is independently a C substituted by an alkoxy group having 1 to 10 carbon atoms 1-20 -Hydrocarbon or C 1-10 -alkyl; M is Ti, Zr or Hf; Each R 1 Same or different, is C 1-6 -alkyl or C 1-6 - alkoxy; Each n is 1 to 2; Each R 2 Same or different, is C 1-6 -alkyl, C 1-6 -alkoxy or -Si(R) 3 Group; Each R is optionally replaced by 1 to 3 C 1-6 -alkyl substituted C 1-10 - alkyl or phenyl; and Each p is from 0 to 1.
8. The multilayer film according to any one of the preceding claims, It is characterized in that The thickness of the skin layer (SKL) of the multilayer film is in the range of 1 to 100 μm, preferably in the range of 5 to 80 μm, more preferably in the range of 10 to 15 μm; and / or The thickness of the core layer (CL) of the multilayer film is in the range of 10 to 200 μm, preferably in the range of 20 to 80 μm, more preferably in the range of 30 to 45 μm; and / or The sealing layer (SL) of the multilayer film has a thickness in the range of 1 to 50 μm, preferably in the range of 5 to 25 μm, more preferably in the range of 10 to 15 μm; and / or The thickness of the multilayer film is in the range of 12 to 350 μm, preferably in the range of 40 to 150 μm, more preferably in the range of 50 to 70 μm.
9. The multilayer film according to any one of the preceding claims, It is characterized in that The multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL); and / or The surface layer (SKL) comprises 80 to 95 wt%, more preferably 82 to 93 wt%, more preferably 88 to 92 wt%, based on the total weight of the skin layer (SKL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP); and 5 to 20 wt%, preferably 7 to 18 wt%, more preferably 8 to 12 wt%, based on the total weight of the skin layer (SKL), of LDPE having a molecular weight of 910 to 930 kg / m 3 , preferably 920 to 925 kg / m 3 The density (ASTM D792) is within the range of 0.5 to 4.0 g / 10 min, preferably 0.5 to 1.0 g / 10 min. 2 (190℃, 2.16kg, ISO 1133).
10. The multilayer film according to any one of the preceding claims, It is characterized in that The multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL); and / or The core layer (CL) comprises 10 to 35 wt%, more preferably 15 to 30 wt%, more preferably 18 to 25 wt%, based on the total weight of the core layer (CL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP); and 65 to 90 wt%, preferably 70 to 85 wt%, more preferably 75 to 82 wt%, based on the total weight of the core layer (CL), of a Ziegler-Natta catalyzed linear low density polyethylene, preferably a multimodal α-olefin terpolymer, preferably having a molecular weight in the range of 920 to 970 kg / m 3 , more preferably 930 to 938 kg / m 3 The density (ASTM D792) is within the range of 0.1 to 2.5 g / 10 min, preferably 0.5 to 1.2 g / 10 min. 2 (190℃, 2.16kg, ISO 1133).
11. The multilayer film according to any one of the preceding claims, It is characterized in that The skin layer (SKL), the core layer (CL) and the seal layer (SL) comprise a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), and preferably, the multilayer film consists of a polyethylene-based polymer.
12. The multilayer film according to any one of the preceding claims, It is characterized in that The content of MMCP (a) in the sealing layer (SL) is in the range of 20 to 40 wt. % or 60 to 80 wt. %, preferably in the range of 25 to 35 wt. % or 65 to 75 wt. %, more preferably in the range of 28 to 32 wt. % or 68 to 72 wt. %, based on the total weight of the sealing layer; and / or The content of the plastomer (b) in the sealing layer (SL) is in the range of 20 to 40 wt % or 60 to 80 wt %, preferably in the range of 25 to 35 wt % or 65 to 75 wt %, more preferably in the range of 28 to 32 wt % or 68 to 72 wt %, based on the total weight of the sealing layer.
13. The multilayer film according to any one of the preceding claims, It is characterized in that The multilayer film has a longitudinal tensile modulus (ISO 527-3) in the range of 150 to 300 MPa, preferably 250 to 290 MPa; and / or a transverse tensile modulus in the range of 150 to 400 MPa, preferably in the range of 300 to 350 MPa (ISO 527-3); and / or • Dart drop strength (ISO 7765-1) in the range of 500 to 2000 g, preferably in the range of 1100 to 1700 g, more preferably in the range of 1500 to 1600 g, more preferably in the range of 1500 to 1550 g.
14. The multilayer film according to any one of the preceding claims, It is characterized in that The multilayer film has A haze (ASTM D1003-00) in the range of 5 to 15%, preferably in the range of 10 to 13%; and / or a sealing initiation temperature determined as described in the description in the range of 50 to 85°C, preferably in the range of 55 to 73°C, more preferably in the range of 56 to 72°C; and / or A hot tack force determined as described in the description in the range of 4 to 12 N, preferably in the range of 5 to 8 N; and / or - A hot sticking temperature determined as described in the specification in the range of 60 to 90°C, preferably in the range of 65 to 88°C.
15. Use of the multilayer film according to any of the preceding claims as packaging material, preferably for food and / or medical products.
Citation Information
Patent Citations
Heat sealable blend of very low density polyethylene or plastomer with polypropylene based polymers and heat sealable film and articles made thereof
EP0575465A1
Polyethylene compositions with improved sealing performance and tear strength
US20210324185A1
A sealant composition, method of producing the same
WO2012061168A1
Multimodal copolymer of ethylene and at least two alpha-olefin comonomers and final articles made thereof
WO2016198273A1
Process for producing a polymer composition
WO2021009189A1