Bismuth oxide-containing phosphate glass with high refractive index and high dispersion

By optimizing the combination of components such as P2O5, Bi2O3, TiO2, Nb2O5 in phosphate glass, the problem of improving the glass formation ability and optical properties of high refractive index and low density glass is solved, and the effect of high transmittance and low optical dispersion is achieved. , suitable for optical devices.

CN118922387APending Publication Date: 2024-11-08CORNING INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202380028408.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to improve the glass-forming capacity and optical properties of phosphate glass while maintaining high refractive index and low density, especially in terms of high transmittance and low optical dispersion in visible light and near UV ranges.

Method used

Through the combination of specific compositions, including P2O5, Bi2O3, TiO2, Nb2O5, Li2O, Na2O, WO3 and other components, the specific mole percentage range and chemical formula conditions are met to optimize the refractive index and density parameters of the glass and achieve high refractive index. and low density phosphate glass.

Benefits of technology

It realizes that while maintaining high refractive index and low density, the glass formation ability and optical properties of glass are improved, and meet the needs of high transmittance and low optical dispersion, and is suitable for optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922387A_ABST
    Figure CN118922387A_ABST
Patent Text Reader

Abstract

The glass composition contains phosphorus oxide (P2O5), niobium oxide (Nb2O5), titanium dioxide (TiO2), and bismuth oxide (Bi2O3) as base components, and may optionally include barium oxide (BaO), calcium oxide (CaO), potassium oxide (K2O), lithium oxide (Li2O), sodium oxide (Na2O), tungsten oxide (WO3), boron oxide (B2O3), and other components. The glass can be characterized by a high refractive index at 587.56 nm at a relatively low density at room temperature.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 323,648, filed on March 25, 2022, the contents of which are the basis of this application and are incorporated herein by reference in their entirety. Technical Field

[0002] The present disclosure generally relates to phosphate glasses having a high refractive index and a low density. In addition, the present disclosure relates to glasses having a high optical dispersion. Background Art

[0003] Glass is used in various optical devices (e.g., augmented reality devices, virtual reality devices, mixed reality devices, glasses, etc.). The desirable properties of this type of glass generally include high refractive index and low density. Additional desirable properties may include high transmittance and / or low optical dispersion in the visible and near ultraviolet (near UV) ranges of the electromagnetic spectrum. It may be challenging to find a glass having a desired combination of these properties and that can be formed from a composition having good glass forming ability. For example, in general, as the refractive index of the glass increases, the density also tends to increase. Substances (e.g., TiO2 and Nb2O5) are generally added to increase the refractive index of the glass without increasing the density of the glass. However, these materials generally absorb blue and UV light, and may undesirably reduce the transmittance of the glass in this spectral interval. Generally, attempts to maintain low density, increase the refractive index of the glass, and not reduce the transmittance in the blue and UV regions of the spectrum may result in a reduction in the glass forming ability of the material. For example, crystallization and / or liquid-liquid phase separation may occur during the cooling of the glass melt using cooling rates that are generally acceptable in the industry. Typically, a decrease in glass-forming ability is manifested as an increase in the amount of certain substances (eg, ZrO2, Y2O3, Sc2O3, BeO, etc.).

[0004] Depending on the glass formers used, low density and high refractive index glasses generally belong to one of two types of chemical systems: (a) borosilicate or borosilicate glasses, in which SiO2 and / or B2O3 are the primary glass formers, and (b) phosphate glasses, in which P2O5 is the primary glass former. Glasses that rely on other oxides as primary glass formers (e.g., GeO2, TeO2, Bi2O3, and V2O5) may be difficult to use due to cost, glass forming ability, optical properties, and / or production requirements.

[0005] Phosphate glasses are characterized by a high refractive index and low density, however, the production of phosphate glasses can be challenging due to the risk of PO volatilization from the melt and / or incompatibility with platinum. In addition, phosphate glasses are often very dark in color and may require additional bleaching steps to provide a glass with the desired transmittance properties. Furthermore, phosphate glasses exhibiting a high refractive index also tend to have increased optical dispersion, which can be useful in some applications.

[0006] In view of these considerations, there is a need for phosphate glasses having a high refractive index and a low density (optionally combined with high transmission in the visible and near UV ranges, and / or made from compositions that provide good glass forming ability). Summary of the invention

[0007] According to an embodiment of the present disclosure, a glass comprises a plurality of components, wherein the glass has a composition of components comprising 15.9 mol% or more and 50.0 mol% or less of P2O5, 4.5 mol% or more and 50.0 mol% or less of Bi2O3, 0.0 mol% or more and 50.0 mol% or less of TiO2, 0.0 mol% or more and 50.0 mol% or less of Nb2O5, 0.0 mol% or more and 25.0 mol% or less of Li2O, 0.0 mol% or more and 25.0 mol% or less of K2O, 0.0 mol% or more and 20.0 mol% or less of Na2O, 0.0 mol% or more and 6.0 mol% or more of Na2O, WO3, greater than or equal to 0.0 mol% and less than or equal to 1.0 mol% V2O5, greater than or equal to 25.0 mol% and less than or equal to 70.0 mol% of the sum of TiO2+Nb2O5, greater than or equal to 0.5 mol% and less than or equal to 30.0 mol% of Alk2O, greater than or equal to 0.5 mol% and less than or equal to 30.0 mol% of RO, greater than or equal to 0.0 mol% and less than or equal to 25.0 mol% of the sum of GeO2+TeO2, and may optionally contain Al2O3, wherein the composition of the components satisfies the following condition: Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol%]≥-8.0, wherein Alk2O is the sum of alkali metal oxides, and RO is the sum of divalent metal oxides.

[0008] According to another embodiment of the present disclosure, a glass comprises a plurality of components, wherein the glass has a composition of components comprising greater than or equal to 23.0 mol% and less than or equal to 35.0 mol% of P2O5, greater than or equal to 4.5 mol% and less than or equal to 35.0 mol% of Bi2O3, greater than or equal to 0.5 mol% and less than or equal to 55.0 mol% of Nb2O5, greater than or equal to 0.5 mol% and less than or equal to 55.0 mol% of TiO2, greater than or equal to 0.3 mol % and less than or equal to 20.0 mol % of Li2O, and may optionally contain one or more components selected from BaO, K2O, CaO, Na2O, SrO, WO3, B2O3, SiO2, ZnO, ZrO2, MgO, Al2O3, TeO2, PbO, GeO2, Tl2O, Ag2O, CdO, Cs2O, Ga2O3, La2O3, MoO3, Ta2O5 and V2O5, and the glass satisfies the following conditions: P n -(1.14+0.192*P d )>0.000, where P n The refractive index n at 587.56 nm is predicted from the glass composition in terms of mole % of the components according to formula (I). d Parameters:

[0009] P n =1.865-0.0052736*P2O5+0.0071201*Nb2O5+0.0031659*TiO2-0.0008032*

[0010] BaO-0.0047736*K2O-0.00076807*CaO-0.0027991*Na2O-0.0016514*Li2O-0.000 69646*SrO+0.0032628*WO3+0.007519*Bi2O3-0.0040698*B2O3-0.0035951*SiO2- 0.00067102*ZnO+0.0022313*ZrO2-0.0019531*MgO-0.003506*Al2O3+0.0019216 *TeO2+0.0025766*PbO-0.0018844*GeO2+0.0065444*Tl2O+0.0052048*Ag2O, (I),

[0011] And P d The density d at room temperature is predicted from the glass composition in terms of mole % of the components according to formula (II). RT Parameters:

[0012] P d=4.45-0.020780*Al2O3-0.020918*B2O3+0.014152*BaO+0.061008*Bi2O3

[0013] -0.0067411*CaO+0.013529*CdO+0.012560*Cs2O+0.0028892*Ga2O3-0.0057012*GeO2-0.017838*K 2O+0.046524*La2O3-0.013919*Li2O-0.010279*MgO-0.0064231*MoO3-0.012983*Na2O+0.0083294* Nb2O5-0.028926*P2O5+0.031742*PbO-0.019022*SiO2+0.0045214*SrO+0.050158*Ta2O5+0.00884 86*TeO2-0.0063053*TiO2-0.018941*V2O5+0.027483*WO3-0.0010277*ZnO+0.0100487*ZrO2, (II).

[0014] Those skilled in the art will understand and appreciate these and other aspects, objects and features of the present disclosure upon studying the following specification, claims and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a graph illustrating the refractive index n for some comparative glasses and some exemplary glasses according to embodiments of the present disclosure. d The refractive index parameter P calculated by formula (I) n A diagram of the relationship between .

[0016] Figure 2 is a graph showing the density d of some comparative glasses and some exemplary glasses according to embodiments of the present disclosure. RT The density parameter P calculated by formula (II) d A diagram of the relationship between .

[0017] Figure 3 is a graph illustrating exemplary cooling schedules according to a “15 minute test” condition and a “2.5 minute test” condition for some exemplary glasses according to an embodiment of the present disclosure.

[0018] Figure 4 FIG. 1 is a graph showing density parameters P for some comparative glasses and some exemplary glasses according to an embodiment of the present disclosure. d and the refractive index parameter P n A diagram of the relationship between .

[0019] Figure 5 is a graph showing the density d at room temperature for some comparative glasses and some exemplary glasses according to embodiments of the present disclosure. RT and the refractive index n at 587.56nm d A diagram of the relationship between . DETAILED DESCRIPTION

[0020] In the following embodiments, for the purpose of explanation rather than limitation, exemplary embodiments of the disclosure details are described to provide a thorough understanding of the various principles of the present disclosure. However, those skilled in the art who benefit from the present disclosure should understand that the present disclosure can be practiced in other embodiments different from the specific details shown herein. In addition, the description of known devices, methods and materials can be omitted to avoid blurring the description of the various principles of the present disclosure. Finally, similar element symbols represent similar elements in any applicable place.

[0021] Unless otherwise expressly stated, any method described herein is not to be construed as requiring that its steps be performed in a specific order. Therefore, in the event that a method claim does not actually recite the order of its steps or does not specifically state in the claim or description that the steps are limited to a specific order, the order is not to be inferred in any way in any respect. This applies to any possible non-expressive basis for description, including but not limited to logical themes for arrangement or operational flow; general meaning derived from grammatical organization or punctuation; the number or type of embodiments described in the specification.

[0022] As used herein, the term "and / or" when used with a list of two or more items means that any one of the listed items may be used alone, or any combination of two or more of the listed items may be used. For example, if a composition is described as containing components A, B, and / or C, the composition may contain only A; only B; only C; a combination of A and B; a combination of A and C; a combination of B and C; or a combination of A, B, and C.

[0023] Those skilled in the art and those who make or use the present disclosure will appreciate modifications of the present disclosure. Therefore, it should be understood that the embodiments shown in the drawings and described above are for illustrative purposes only and are not intended to limit the scope of the present disclosure defined by the appended claims interpreted according to the principles of patent law (including the doctrine of equivalents).

[0024] As used herein, the term "about" means that amounts, dimensions, formulas, parameters, and other quantities and characteristics are not exact and need not be exact, but can be approximated and / or larger or smaller as needed to reflect tolerances, conversion factors, rounding, measurement errors, and the like, as well as other factors known to those skilled in the art. When the term "about" is used to describe a value or endpoint of a range, the disclosure should be understood to include the specific value or endpoint referred to. Regardless of whether the value or endpoint of a range in the specification is stated as "about", the value or endpoint of the range is intended to include two embodiments: one modified by "about" and one not modified by "about". It can be further understood that each endpoint of the range is clearly related to the other endpoint and is independent of the other endpoint.

[0025] The term "component" refers to a material or compound included in a batch composition for forming glass. Components include oxides (including but not limited to those represented by formulas (I) and (II) and in the claims). Representative components include B2O3, P2O5, Al2O3, CuO, Cu2O, RO, R2O, SnO2, MnO2, RE m O n , SiO2, Ta2O5, ZnO, WO3, Nb2O5, TiO2, ZrO2, Bi2O3, TeO2, etc. Other representative components include halogens (e.g., F, Br, Cl). Whenever a component is included as a term in a mathematical expression or formula, it should be understood that the component refers to the amount of the component in the batch composition of the glass in mol %. For example, the expression "B2O3+P2O5" refers to the sum of the amount of B2O3 in mol % and the amount of P2O5 in mol % in the batch composition of the glass. A mathematical expression or formula is any expression or formula that includes a mathematical operator (e.g., "+", "-", "*", " / ", "min", or "max").

[0026] Unless otherwise indicated, the amounts or contents of components in glass compositions are expressed herein in units of mol % (mole percent).

[0027] The term "formed from" may mean one or more of comprising, consisting essentially of, or consisting of. For example, a component formed from a particular material may comprise the particular material, consist essentially of the particular material, or consist of the particular material.

[0028] The terms "free" and "substantially free" are used interchangeably herein to refer to the amount of and / or absence of a particular component in a glass composition that was not intentionally added to the glass composition. It is understood that the glass composition may contain trace amounts of less than 0.10 mol% of a particular constituent component as a contaminant or impurity.

[0029] As used herein, when used to describe a particular constituent component in a glass composition, the term "impurity" refers to a constituent component that is not intentionally added to the glass composition and is present in an amount of less than 0.10 mol%. The impurity component may be inadvertently added to the glass composition during processing of the glass composition, as an impurity in another constituent component, and / or may be inadvertently added by migration of the impurity component into the composition.

[0030] Unless otherwise indicated, the term "glass" is used to refer to glass made from the glass compositions disclosed herein.

[0031] The symbol "*" when used in any formula herein indicates multiplication.

[0032] Temperatures are expressed herein in degrees Celsius.

[0033] Density is expressed in g / cm 3 It is expressed as a unit.

[0034] Viscosity is expressed herein in units of P (poise).

[0035] The term "glass former" is used herein to refer to components that, when present alone in a glass composition (ie, without components other than impurities), are capable of forming glass upon cooling of a melt at a rate of no greater than about 300°C / min.

[0036] As used herein, the term "modifier" refers to an oxide of a monovalent or divalent metal (i.e., RO or RO, where "R" represents a cation). Modifiers can be added to glass compositions to alter the atomic structure of the melt and the resulting glass. In some embodiments, the modifier can change the coordination number of the cations present in the glass former (e.g., boron in B2O3), which can result in the formation of a more polymeric atomic network and, therefore, can provide better glass formation.

[0037] As used herein, the term "RO" refers to the total content of divalent metal oxides, the term "RO" refers to the total content of monovalent metal oxides, and the term "AlkO" refers to the total content of alkali metal oxides. For example, the term R2O includes alkali metal oxides (AlkO) in addition to other monovalent metal oxides (e.g., Ag2O, Tl2O, and Hg2O). As described below, in the present disclosure, rare earth metal oxides are referred to herein by their normalized formula (RE2O3), wherein the rare earth metal has a redox state of "+3", and therefore the rare earth metal oxides are not included in the term RO.

[0038] As used herein, the term "rare earth metal" refers to the metals listed in the IUPAC periodic table of elements, lanthanum, and yttrium and scandium. As used herein, the term "rare earth metal oxide" is used to refer to oxides of rare earth metals in different redox states (e.g., "+3" for lanthanum in La2O3, "+4" for cerium in CeO2, "+2" for europium in EuO, etc.). Generally speaking, the redox state of the rare earth metal in the oxide glass may vary, and more specifically, the redox state may change during melting depending on the batch composition and / or the redox conditions in the furnace in which the glass is melted and / or hot processed (e.g., annealed). Unless otherwise stated, rare earth metal oxides are referred to herein by their standardized equations, wherein the rare earth metal has a redox state of "+3". Therefore, in the event that a rare earth metal having a redox state other than "+3" is added to a glass composition batch, the glass composition is recalculated by adding or removing some oxygen to maintain stoichiometry. For example, when CeO2 (cerium in the redox state "+4") is used as a batch component, the resulting glass composition is recalculated assuming that two moles of CeO2 are equal to one mole of Ce2O3, and the resulting glass composition is presented in terms of Ce2O3. m O n " is used to refer to the total content of rare earth metal oxides in all redox states present, while the term "RE2O3" is used to refer to the total content of rare earth metal oxides in the "+3" redox state, also designated as "trivalent equivalent".

[0039] Unless otherwise indicated, all batch compositions are expressed in mole percent (mol %). It will be appreciated by those skilled in the art that various melt compositions (e.g., fluorine, alkali metals, boron, etc.) may have varying degrees of volatility (e.g., a function of vapor pressure, melting time, and / or melting temperature). Therefore, compared to the batch compositions provided herein, when measuring the final product, the term "about" associated with these compositions is intended to include values ​​within about 0.2 mol %. Based on the above considerations, it is expected that the composition between the final product and the batch composition is substantially equal.

[0040] The measured density values ​​of the glasses reported herein are in g / cm2 at room temperature using the Archimedes method in water. 3 The measurement is carried out in units of 0.001 g / cm 3 As used herein, density measurements at room temperature (designated as d RT) is expressed as being measured at 20°C or 25°C and includes measurements that can be taken at temperatures ranging from 20°C to 25°C. It is understood that room temperature can vary between about 20°C to about 25°C, however, for the purposes of this disclosure, the variation in density within the temperature range of 20°C to 25°C is expected to be less than 0.001 g / cm 3 , and are therefore not expected to affect the room temperature density measurements described in this paper.

[0041] As used herein, good glass forming ability refers to the resistance of a melt to devitrification as the material cools. Glass forming ability can be measured by determining the critical cooling rate of a melt. The term "critical cooling rate" or "v cr "Critical cooling rate" is used herein to refer to the minimum cooling rate at which a melt of a given composition forms a glass free of crystals visible under an optical microscope at 500x magnification. The critical cooling rate can be used to measure the glass-forming ability of a composition (i.e., the ability of a melt of a given glass composition to form glass upon cooling). Generally speaking, the lower the critical cooling rate, the better the glass-forming ability.

[0042] The term “liquidus temperature” (T liq ) is used herein to refer to the temperature above which the glass composition is completely liquid and the constituent components of the glass have not crystallized. The liquidus temperature values ​​reported herein are obtained by measuring the sample using DSC or by isothermal holding of the sample wrapped in platinum foil. For the samples measured using DSC, the powder sample is heated to 1250°C at 10 K / min. The end of the endothermic event corresponding to the melting of the crystallization is considered to be the liquidus temperature. For the second technique (isotactic holding), a glass block (approximately 1 cm 3 ) were wrapped in platinum foil to avoid volatilization and placed in an oven at a given temperature for 17 hours. The glass blocks were then observed under an optical microscope to check for crystallization.

[0043] Unless otherwise stated, the refractive index values ​​described herein are measured at room temperature. The refractive index values ​​of the glass samples were measured using a Metricon 2010 prism coupler refractometer with an error of about ±0.0002. Using Metricon, the refractive index of the glass samples was measured at two or more wavelengths of about 406nm, 473nm, 532nm, 633nm, 828nm and 1064nm. The measured correlation characterizes the dispersion and is then fitted using the Cauchy's law equation or the Sellmeier equation to allow calculation of the refractive index of the sample at a given wavelength of interest between the measured wavelengths. The term "refractive index n d ” is used herein to refer to the refractive index calculated as described above at a wavelength of 587.56 nm corresponding to the wavelength of the helium d-line. The term “refractive index nC " is used herein to refer to the refractive index calculated as described above at a wavelength of 656.3 nm. The term "refractive index n F " is used herein to refer to the refractive index calculated as described above at a wavelength of 486.1 nm. The term "refractive index n g ” is used herein to refer to the refractive index calculated as described above at a wavelength of 435.8 nm.

[0044] As used herein, unless otherwise specified, the term "high refractive index" or "high index" refers to a glass having a refractive index value greater than, or equal to, at least 1.80. Where indicated, the term "high refractive index" or "high index" refers to a glass having a refractive index value greater than, or equal to, at least 1.85, greater than, or equal to, 1.90, or greater than, or equal to, 1.95, or greater than, or equal to, 2.00.

[0045] The terms "dispersion" and "optical dispersion" are used interchangeably and refer to the difference or ratio of the refractive index of a glass sample at a predetermined wavelength. One numerical measure of optical dispersion as described herein is the Abbe number which can be calculated by the following formula: x =(n x -1) / (n F -n C ), where "x" in the present disclosure represents one of the commonly used wavelengths (e.g., 587.56 nm [d segment] or 589.3 nm [D segment]), n x is the refractive index at this wavelength, and n F and n C It is the refractive index at wavelengths of 486.1nm (F segment) and 656.3nm (C segment). d and ν D The numerical differences are very small, mainly between ±0.1% and ±0.2%. As described herein, the dispersion of a glass sample is characterized by the Abbe number (ν) which characterizes the relationship between the refractive index of the sample at three different wavelengths according to the following formula: d ) means: d =(n d -1) / (n F -n C ), where n d is the calculated refractive index at 587.56 nm (d segment), n F is the calculated refractive index at 486.1 nm, and n C is the calculated refractive index at 656.3 nm. A higher Abbe number corresponds to a lower optical dispersion.

[0046] The value of the Abbe number corresponding to "high dispersion" or "low dispersion" may vary depending on the refractive index for which the Abbe number is calculated. In some cases, the Abbe number corresponding to "low dispersion" for a high refractive index glass may be lower than the Abbe number corresponding to "low dispersion" for a low refractive index glass. In other words, as the calculated refractive index value increases, the value of the Abbe number corresponding to low dispersion decreases. The same applies to "high dispersion".

[0047] Glass transition temperature (T g ) were measured by differential scanning calorimetry (DSC) at a heating rate of 10 K / min after cooling in air.

[0048] The glass composition may include phosphorus oxide (P2O5). The glass composition in the embodiments described herein contains phosphorus oxide (P2O5) as the main glass former. A larger amount of P2O5 results in a larger viscosity value at a given temperature, preventing the melt from crystallizing upon cooling, and thus improving the glass forming ability of the melt (i.e., reducing the critical cooling rate of the melt). However, P2O5 significantly reduces the refractive index. Therefore, the content of P2O5 in the high refractive index glass is limited. In an embodiment, the amount of phosphorus oxide (P2O5) contained in the glass composition may be greater than or equal to 15.9 mol% and less than or equal to 50.0 mol%, as well as all ranges and sub-ranges between the foregoing values. In some embodiments, the glass composition may include PO in an amount greater than or equal to 15.9 mol%, greater than or equal to 17.5 mol%, greater than or equal to 18.0 mol%, greater than or equal to 20.0 mol%, greater than or equal to 23.0 mol%, greater than or equal to 23.5 mol%, greater than or equal to 24.05 mol%, greater than or equal to 24.5 mol%, greater than or equal to 35.0 mol%, greater than or equal to 40.0 mol%, or greater than or equal to 45.0 mol%. In some other embodiments, the glass composition may include PO in an amount less than or equal to 50.0 mol%, less than or equal to 45.0 mol%, less than or equal to 40.0 mol%, less than or equal to 35.0 mol%, less than or equal to 28.0 mol%, less than or equal to 27.5 mol%, less than or equal to 25.5 mol%, less than or equal to 25.0 mol%, or less than or equal to 20.0 mol%. In some more embodiments, the glass composition may include P2O5 in an amount greater than or equal to 15.9 mol% and less than or equal to 50.0 mol%, greater than or equal to 17.5 mol% and less than or equal to 27.5 mol%, greater than or equal to 18.0 mol% and less than or equal to 28.0 mol%, greater than or equal to 23.0 mol% and less than or equal to 35.0 mol%, greater than or equal to 23.5 mol% and less than or equal to 25.5 mol%, greater than or equal to 24.05 mol% and less than or equal to 25.05 mol%, greater than or equal to 24.2 mol% and less than or equal to 25.0 mol%, greater than or equal to 24.48 mol% and less than or equal to 25.5 mol%, greater than or equal to 25.05 mol%, greater than or equal to 25.0 mol%, greater than or equal to 25.0 mol%, greater than or equal to 25.48 mol% and less than or equal to 25.5 mol%, greater than or equal to 25.0 ... Less than or equal to 24.99 mol%, greater than or equal to 15.9 mol% and less than or equal to 20.0 mol%, greater than or equal to 17.5 mol% and less than or equal to 50.0 mol%, greater than or equal to 20.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 23.0 mol% and less than or equal to 50.0 mol%, greater than or equal to 23.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 23.5 mol% and less than or equal to 50.0 mol%, greater than or equal to 23.5 mol% and less than or equal to 25.0 mol%, greater than or equal to 24.05 mol% and less than or equal to 25.0 mol%.

[0049] The glass composition may include germanium oxide (GeO2). Germanium oxide (GeO2) provides a high ratio of refractive index to density and does not reduce visible light transmittance. Germanium oxide is a glass-forming oxide. However, germanium oxide is expensive, so the content of germanium oxide should be limited, or the glass composition may not contain GeO2. In an embodiment, the amount of germanium oxide (GeO2) included in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the amount of GeO2 included in the glass composition may be greater than or equal to 0.0 mol%, greater than or equal to 5.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 19.0 mol%, greater than or equal to 20.0 mol%, greater than or equal to 21.0 mol%, or greater than or equal to 23.0 mol%. In some other embodiments, the glass composition may include GeO2 in an amount less than or equal to 25.0 mol%, less than or equal to 23.0 mol%, less than or equal to 21.0 mol%, less than or equal to 20.0 mol%, less than or equal to 19.0 mol%, less than or equal to 10.0 mol%, or less than or equal to 5.0 mol%. In some more embodiments, the glass composition may include GeO2 in an amount greater than or equal to 0.0 mol% and less than or equal to 5.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 19.0 mol%, greater than or equal to 19.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 19.0 mol% and less than or equal to 20.0 mol%, greater than or equal to 20.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 20.0 mol% and less than or equal to 21.0 mol%.

[0050] The glass composition may include boron oxide (B2O3). According to some embodiments of the present disclosure, boron oxide may act as a glass former. As a glass former, B2O3 may increase liquidus viscosity and thus inhibit crystallization. However, adding B2O3 to the glass composition may cause liquid-liquid phase separation, which may cause devitrification and / or a reduction in visible light transmittance of the resulting glass. In addition, adding B2O3 to a high refractive index glass may reduce the refractive index. Therefore, the amount of boron oxide is limited, or the glass may be substantially free of B2O3. In an embodiment, the amount of boron oxide (B2O3) contained in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, as well as all ranges and sub-ranges between the foregoing values. In some embodiments, the amount of B2O3 contained in the glass composition may be greater than or equal to 0.0 mol%, or greater than or equal to 5.0 mol%. In some other embodiments, the glass composition may include B2O3 in an amount less than or equal to 10.0 mol%, less than or equal to 10.0 mol%, less than or equal to 8.0 mol%, or less than or equal to 5.0 mol%. In some more embodiments, the glass composition may include B2O3 in an amount greater than or equal to 0.0 mol% and less than or equal to 15.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 8.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 5.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 15.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 8.0 mol%.

[0051] The glass composition may include an alkali metal oxide (Alk2O). Alkali metal oxides (Li2O, Na2O, K2O, Rb2O, and Cs2O) may help incorporate a high refractive index component (e.g., TiO2, Nb2O5, or WO3) into the glass structure at a given density. Most commonly, Li2O, Na2O, and / or K2O are used for this purpose. Of these three oxides, K2O generally has the greatest effect on the solubility of the high refractive index component; however, the addition of K2O itself may reduce the refractive index. Li2O generally provides the greatest ratio of refractive index to density among the alkali metal oxides, but has the least effect on the solubility of the high refractive index component. Sodium oxide (Na2O) generally provides an intermediate effect between Li2O and K2O. However, the exact effect of these oxides on glass forming ability is difficult to predict, and the desired ratios between these oxides may be different in different embodiments. More specifically, in some embodiments, it is desirable to add all three oxides (Li2O, Na2O, and K2O) or two of them together with each other. In addition, in some embodiments, a monovalent metal oxide (RO) is used together with a divalent metal oxide (RO) to improve the glass forming ability of the glass, and a higher refractive index can be achieved at a given density. Therefore, in some embodiments of the present disclosure, the total content of alkali metal oxides can be limited.

[0052] In some embodiments, the glass composition may include an alkali metal oxide Alk2O in an amount greater than or equal to 0.5 mol%, greater than or equal to 10.0 mol%, or greater than or equal to 20.0 mol%. In some other embodiments, the glass composition may include an alkali metal oxide Alk2O in an amount less than or equal to 30.0 mol%, less than or equal to 20.0 mol%, or less than or equal to 10.0 mol%. In some more embodiments, the glass composition may include an alkali metal oxide Alk2O in an amount greater than or equal to 0.5 mol% and less than or equal to 30.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 10.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 30.0 mol%, or greater than or equal to 10.0 mol% and less than or equal to 20.0 mol%.

[0053] The glass composition may include potassium oxide (KO). Potassium oxide may increase the solubility of high refractive index components (e.g., TiO2 and Nb2O5) to a greater extent than other monovalent and divalent metal oxides. However, potassium oxide itself provides the lowest refractive index among alkali metal oxides. Therefore, at high concentrations of KO, it may be difficult to achieve a high refractive index. Therefore, the amount of KO in the glass of the present disclosure is limited, or the glass may be substantially free of KO. In an embodiment, the glass composition may include potassium oxide (KO) in an amount greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the glass composition may include KO in an amount greater than or equal to 0.0 mol%, greater than or equal to 2.0 mol%, greater than or equal to 5.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 19.0 mol%, greater than or equal to 20.0 mol%, greater than or equal to 21.0 mol%, or greater than or equal to 23.0 mol%. In some other embodiments, the glass composition may include K2O in an amount less than or equal to 25.0 mol%, less than or equal to 23.0 mol%, less than or equal to 21.0 mol%, less than or equal to 20.0 mol%, less than or equal to 19.0 mol%, less than or equal to 10.0 mol%, less than or equal to 8.0 mol%, less than or equal to 7.5 mol%, or less than or equal to 5.0 mol%. In some more embodiments, the glass composition may include K2O in an amount greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 7.5 mol%, greater than or equal to 2.06 mol% and less than or equal to 7.5 mol%, greater than or equal to 5.0 mol% and less than or equal to 7.5 mol%, greater than or equal to 10.0 mol% and less than or equal to 19.0 mol%, greater than or equal to 19.0 mol% and less than or equal to 20.0 mol%.

[0054] The glass composition may include lithium oxide (Li2O). Among the known monovalent metal oxides, lithium oxide provides the highest ratio of glass refractive index to density. In addition, in some embodiments, Li2O can help increase the solubility of Nb2O5 and TiO2, and additionally increase the refractive index at a given density. In addition, lithium oxide can accelerate the process of bleaching glass. However, the addition of Li2O (even in sufficiently small concentrations) may reduce the glass forming ability of the glass, causing crystallization or liquid-liquid phase separation of the glass-forming melt when cooling. Therefore, the amount of Li2O is limited. In some embodiments, the glass may be substantially free of Li2O. In an embodiment, the amount of lithium oxide (Li2O) included in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the glass composition may include Li2O in an amount greater than or equal to 0.0 mol%, greater than or equal to 0.1 mol%, greater than or equal to 0.3 mol%, greater than or equal to 5.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 19.0 mol%, greater than or equal to 20.0 mol%, greater than or equal to 21.0 mol%, or greater than or equal to 23.0 mol%. In some other embodiments, the glass composition may include Li2O in an amount less than or equal to 25.0 mol%, less than or equal to 23.0 mol%, less than or equal to 21.0 mol%, less than or equal to 20.0 mol%, less than or equal to 19.0 mol%, less than or equal to 10.0 mol%, less than or equal to 7.5 mol%, less than or equal to 6.5 mol%, less than or equal to 5.75 mol%, less than or equal to 5.0 mol%, or less than or equal to 2.1 mol%. In some more embodiments, the glass composition may include Li2O in an amount greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 7.5 mol%, greater than or equal to 0.0 mol% and less than or equal to 6.5 mol%, greater than or equal to 0.0 mol% and less than or equal to 5.75 mol%, greater than or equal to 0.3 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.42 mol%. and less than or equal to 2.08 mol %, greater than or equal to 0.0 mol % and less than or equal to 2.1 mol %, greater than or equal to 0.1 mol % and less than or equal to 2.1 mol %, greater than or equal to 0.3 mol % and less than or equal to 2.1 mol %, greater than or equal to 5.0 mol % and less than or equal to 25.0 mol %, greater than or equal to 5.0 mol % and less than or equal to 5.75 mol %, greater than or equal to 10.0 mol % and less than or equal to 19.0 mol %, greater than or equal to 19.0 mol % and less than or equal to 20.0 mol %.

[0055] The glass composition may include sodium oxide (Na2O). In high refractive index glasses, Na2O acts similarly to K2O to improve the solubility of high refractive index components (e.g., TiO2, Nb2O5, WO3, and others), but at the same time, Na2O itself reduces the refractive index of the glass. In most cases, it is found that the effect of Na2O on the solubility of high refractive index components is slightly lower than the corresponding effect of K2O. However, Na2O provides a lower thermal expansion coefficient than K2O, which can reduce the thermal stress formed when cooling the glass product, thereby improving the quality of the product. In an embodiment, the glass composition may include sodium oxide (Na2O) in an amount greater than or equal to 0.0 mol% and less than or equal to 20.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the glass composition may include Na2O in an amount greater than or equal to 0.0 mol%, greater than or equal to 5.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 14.0 mol%, greater than or equal to 16.0 mol%, or greater than or equal to 18.0 mol%. In some other embodiments, the glass composition may include Na2O in an amount less than or equal to 20.0 mol%, less than or equal to 18.0 mol%, less than or equal to 16.0 mol%, less than or equal to 14.0 mol%, less than or equal to 10.0 mol%, less than or equal to 7.5 mol%, less than or equal to 6.5 mol%, less than or equal to 5.75 mol%, or less than or equal to 5.0 mol%. In some more embodiments, the glass composition may include Na2O in an amount greater than or equal to 0.0 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 7.5 mol%, greater than or equal to 0.0 mol% and less than or equal to 6.5 mol%, greater than or equal to 0.0 mol% and less than or equal to 5.75 mol%, greater than or equal to 0.03 mol% and less than or equal to 4.97 mol%, greater than or equal to 0.0 mol% and less than or equal to 5.0 mol%.

[0056] Glass compositions may include divalent metal oxides (RO). Divalent metal oxides (e.g., alkaline earth metal oxides (BeO, MgO, CaO, SrO, and BaO), zinc oxide (ZnO), cadmium oxide (CdO), lead oxide (PbO), and others) (when present in glass) provide a higher refractive index than most monovalent oxides. Some divalent metal oxides (e.g., CaO, SrO, and ZnO) also provide a relatively low density, thereby increasing the ratio of refractive index to density, and thus increasing the effectiveness of the optical glass. In addition, divalent metal oxides can help increase the solubility of high refractive index components (e.g., TiO2, Nb2O5, and WO3), resulting in a further increase in refractive index at a given density. However, when added in large amounts, divalent metal oxides may cause crystallization or liquid-liquid phase separation of refractory minerals in the melt, thereby reducing the glass forming ability of the glass. Therefore, the amount of divalent metal oxides in the glass compositions of the present disclosure is limited.

[0057] In some embodiments, the glass composition may include the divalent metal oxide RO in an amount greater than or equal to 0.3 mol%, greater than or equal to 0.5 mol%, greater than or equal to 10.0 mol%, or greater than or equal to 20.0 mol%. In some other embodiments, the glass composition may include the divalent metal oxide RO in an amount less than or equal to 30.0 mol%, less than or equal to 20.0 mol%, or less than or equal to 10.0 mol%. In some more embodiments, the glass composition may include a divalent metal oxide RO in an amount greater than or equal to 0.3 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 30.0 mol%, greater than or equal to 0.3 mol% and less than or equal to 30.0 mol%, greater than or equal to 0.3 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 10.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 30.0 mol%, or greater than or equal to 10.0 mol% and less than or equal to 20.0 mol%.

[0058] The glass composition may include barium oxide (BaO). Barium oxide may increase the solubility of high refractive index components (e.g., TiO2 and Nb2O5), resulting in an increase in the refractive index at a given density. However, barium is a heavy element, and large additions may increase the density of the glass. In addition, at high concentrations, crystallization of minerals (e.g., barium titanate (BaTiO3), barium niobate (BaNb2O6), barium orthophosphate (Ba3P2O8), and others) may result. Therefore, the amount of BaO in the glass is limited, or the glass may be substantially free of BaO. In an embodiment, the amount of barium oxide (BaO) included in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 20.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the amount of BaO included in the glass composition may be greater than or equal to 0.0 mol%, greater than or equal to 1.75 mol%, greater than or equal to 3.0 mol%, or greater than or equal to 10.0 mol%. In some other embodiments, the glass composition may include BaO in an amount less than or equal to 20.0 mol%, less than or equal to 10.0 mol%, less than or equal to 9.0 mol%, or less than or equal to 8.0 mol%. In some more embodiments, the glass composition may include BaO in an amount greater than or equal to 0.0 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 9.0 mol%, greater than or equal to 1.75 mol% and less than or equal to 8.0 mol%, greater than or equal to 2.59 mol% and less than or equal to 8.99 mol%, greater than or equal to 0.0 mol% and less than or equal to 8.0 mol%, greater than or equal to 1.75 mol% and less than or equal to 20.0 mol%, greater than or equal to 3.0 mol% and less than or equal to 20.0 mol%, greater than or equal to 3.0 mol% and less than or equal to 8.0 mol%.

[0059] The glass composition may include calcium oxide (CaO). Among the known monovalent and divalent metal oxides, calcium oxide provides the highest ratio of refractive index to density. In addition, in some embodiments, CaO can help increase the solubility of Nb2O5 and TiO2, and additionally increase the refractive index at a given density. However, if the amount of CaO in the glass is too high, it may cause crystallization of refractory materials (e.g., calcium titanate (CaTiO3, CaTi2O5, etc.), calcium niobate (CaNb2O6), calcium metasilicate (CaSiO3) and others). This effect may reduce the viscosity at the liquidus temperature, thereby increasing the critical cooling rate, and may cause crystallization of the melt when cooling. Therefore, the amount of CaO is limited. In an embodiment, the amount of calcium oxide (CaO) included in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 17.0 mol%, and all ranges and sub-ranges between the aforementioned values. In some embodiments, the glass composition may include CaO in an amount greater than or equal to 0.0 mol%, greater than or equal to 1.0 mol%, or greater than or equal to 10.0 mol%. In some other embodiments, the glass composition may include CaO in an amount less than or equal to 17.0 mol%, less than or equal to 10.0 mol%, or less than or equal to 9.0 mol%. In some more embodiments, the glass composition may include CaO in an amount greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 9.0 mol%, greater than or equal to 0.97 mol% and less than or equal to 8.99 mol%, greater than or equal to 0.0 mol% and less than or equal to 17.0 mol%, greater than or equal to 1.0 mol% and less than or equal to 17.0 mol%, greater than or equal to 1.0 mol% and less than or equal to 9.0 mol%.

[0060] The glass composition may include vanadium oxide (V2O5). Among all oxides, vanadium oxide provides the highest ratio of refractive index to density. However, vanadium oxide may cause undesirable dark or even black colors, and may also cause ecological problems. For these reasons, the content of vanadium oxide in the glass is limited, or the glass composition may not contain V2O5. In an embodiment, the amount of vanadium oxide (V2O5) contained in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 5.0 mol%, and all ranges and sub-ranges between the aforementioned values. In some other embodiments, the amount of V2O5 contained in the glass composition may be less than or equal to 5.0 mol%, less than or equal to 2.5 mol%, or less than or equal to 1.0 mol%. In some more embodiments, the amount of V2O5 contained in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 1.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 5.0 mol%.

[0061] The glass composition may include tungsten oxide (WO3). WO3 provides a high refractive index without significantly increasing the density or causing undesirable coloring. However, at a high content of WO3, the liquidus temperature tends to increase, while the viscosity at the liquidus temperature decreases, making it difficult to avoid crystallization of the melt during cooling. Therefore, the content of tungsten oxide should be limited, or the glass composition may be free of WO3. In an embodiment, the amount of tungsten oxide (WO3) contained in the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the amount of WO3 contained in the glass composition may be greater than or equal to 0.0 mol%, greater than or equal to 3.93 mol%, greater than or equal to 5.0 mol%, greater than or equal to 7.0 mol%, greater than or equal to 8.0 mol%, or greater than or equal to 9.0 mol%. In some other embodiments, the glass composition may include WO3 in an amount less than or equal to 10.0 mol%, less than or equal to 9.0 mol%, less than or equal to 8.0 mol%, less than or equal to 7.5 mol%, less than or equal to 7.0 mol%, less than or equal to 6.5 mol%, less than or equal to 6.0 mol%, less than or equal to 5.0 mol%, or less than or equal to 4.8 mol%. In some more embodiments, the glass composition may include WO3 in an amount greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 7.5 mol%, greater than or equal to 0.0 mol% and less than or equal to 6.5 mol%, greater than or equal to 0.0 mol% and less than or equal to 6.0 mol%, greater than or equal to 3.93 mol% and less than or equal to 4.8 mol%, greater than or equal to 0.0 mol% and less than or equal to 4.8 mol%, greater than or equal to 5.0 mol% and less than or equal to 6.0 mol%, greater than or equal to 8.0 mol% and less than or equal to 9.0 mol%.

[0062] The glass composition may include bismuth oxide (Bi2O3). Bi2O3 provides a very high refractive index, but leads to an increase in density. However, it may also reduce the viscosity of the melt at high temperatures, which may cause crystallization of the melt when it is cooled. This effect is particularly significant at high contents of Bi2O3. Therefore, the content of bismuth oxide should be limited. In an embodiment, the amount of bismuth oxide (Bi2O3) included in the glass composition may be greater than or equal to 4.0 mol% and less than or equal to 50.0 mol%, and all ranges and sub-ranges between the foregoing values. In some embodiments, the amount of Bi2O3 included in the glass composition may be greater than or equal to 4.0 mol%, greater than or equal to 4.5 mol%, greater than or equal to 5.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 25.0 mol%, greater than or equal to 35.0 mol%, greater than or equal to 40.0 mol%, or greater than or equal to 45.0 mol%. In some other embodiments, the glass composition may include Bi2O3 in an amount of less than or equal to 50.0 mol%, less than or equal to 45.0 mol%, less than or equal to 40.0 mol%, less than or equal to 35.0 mol%, less than or equal to 30.0 mol%, less than or equal to 25.0 mol%, less than or equal to 23.0 mol%, or less than or equal to 10.0 mol%. In some more embodiments, the glass composition may include Bi2O3 in an amount of greater than or equal to 4.0 mol% and less than or equal to 30.0 mol%, greater than or equal to 4.5 mol% and less than or equal to 50.0 mol%, greater than or equal to 4.5 mol% and less than or equal to 35.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 30.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 5.0 mol% and less than or equal to 23.0 mol%, or less than or equal to 10.0 mol%. % and less than or equal to 23.0 mol %, greater than or equal to 4.0 mol % and less than or equal to 50.0 mol %, greater than or equal to 4.5 mol % and less than or equal to 10.0 mol %, greater than or equal to 10.0 mol % and less than or equal to 50.0 mol %, greater than or equal to 10.0 mol % and less than or equal to 23.0 mol %, greater than or equal to 25.0 mol % and less than or equal to 50.0 mol %, greater than or equal to 25.0 mol % and less than or equal to 30.0 mol %.

[0063] The glass composition may include titanium dioxide (TiO2). High refractive index glass typically includes substances (e.g., TiO2 and Nb2O5) that absorb at least a portion of visible light (specifically at wavelengths in the blue and near UV regions). In an embodiment of the present disclosure, the transmittance of the glass may be characterized for different wavelengths in the range of about 300 nm to 2300 nm. High transmittance in the visible and near UV ranges (blue region) is particularly desirable in some applications. Achieving high transmittance in the blue region in high refractive index glass can be challenging. High-grade TiO2 and / or Nb2O5 that increase the refractive index, which are typically used in glass, tend to reduce transmittance in the near UV region and shift the UV cutoff wavelength to a higher wavelength. Therefore, the amount of TiO2 is limited, or the glass composition may be substantially free of TiO2. In an embodiment, the amount of titanium dioxide (TiO2) included in the glass composition may be greater than or equal to 0.0 mol % and less than or equal to 55.0 mol %, as well as all ranges and sub-ranges between the aforementioned values. In some embodiments, the glass composition may include TiO2 in an amount greater than or equal to 0.0 mol%, greater than or equal to 0.3 mol%, greater than or equal to 0.5 mol%, greater than or equal to 7.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 13.0 mol%, greater than or equal to 14.0 mol%, greater than or equal to 25.0 mol%, greater than or equal to 40.0 mol%, greater than or equal to 45.0 mol%, or greater than or equal to 50.0 mol%. In some other embodiments, the glass composition may include TiO2 in an amount less than or equal to 55.0 mol%, less than or equal to 50.0 mol%, less than or equal to 45.0 mol%, less than or equal to 40.0 mol%, less than or equal to 36.0 mol%, less than or equal to 33.0 mol%, less than or equal to 30.0 mol%, less than or equal to 25.0 mol%, or less than or equal to 10.0 mol%.In some more embodiments, the glass composition may include TiO2 in an amount greater than or equal to 0.0 mol% and less than or equal to 50.0 mol%, greater than or equal to 0.3 mol% and less than or equal to 40.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 55.0 mol%, greater than or equal to 7.0 mol% and less than or equal to 40.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 36.0 mol%, greater than or equal to 13.0 mol% and less than or equal to 33.0 mol%, greater than or equal to 13.7 mol% and less than or equal to 30.23 mol%, greater than or equal to 0.0 mol%. % and less than or equal to 55.0 mol %, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol %, greater than or equal to 0.3 mol % and less than or equal to 10.0 mol %, greater than or equal to 0.5 mol % and less than or equal to 10.0 mol %, greater than or equal to 7.0 mol % and less than or equal to 55.0 mol %, greater than or equal to 7.0 mol % and less than or equal to 10.0 mol %, greater than or equal to 10.0 mol % and less than or equal to 25.0 mol %, greater than or equal to 13.0 mol % and less than or equal to 25.0 mol %, greater than or equal to 14.0 mol % and less than or equal to 25.0 mol %.

[0064] The glass composition may include niobium oxide (Nb2O5). Similar to titanium dioxide, niobium oxide may be used to increase the refractive index of the glass while maintaining a low density. However, niobium oxide may introduce a yellow tint to the glass that cannot be bleached as titanium dioxide does, and may result in a decrease in transmittance (more particularly in the blue and UV ranges). Similar to titanium dioxide, niobium oxide may result in crystallization and / or phase separation of the melt. In some embodiments, the glass may be substantially free of Nb2O5. In an embodiment, the glass composition may include niobium oxide (Nb2O5) in an amount greater than or equal to 0.0 mol% and less than or equal to 55.0 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may include Nb2O5 in an amount greater than or equal to 0.0 mol%, greater than or equal to 0.5 mol%, greater than or equal to 7.0 mol%, greater than or equal to 10.0 mol%, greater than or equal to 14.0 mol%, greater than or equal to 16.5 mol%, greater than or equal to 19.0 mol%, greater than or equal to 25.0 mol%, greater than or equal to 40.0 mol%, greater than or equal to 45.0 mol%, or greater than or equal to 50.0 mol%. In some other embodiments, the glass composition may include Nb2O5 in an amount less than or equal to 55.0 mol%, less than or equal to 50.0 mol%, less than or equal to 45.0 mol%, less than or equal to 40.0 mol%, less than or equal to 33.0 mol%, less than or equal to 30.5 mol%, less than or equal to 29.0 mol%, less than or equal to 25.0 mol%, or less than or equal to 10.0 mol%. In some more embodiments, the glass composition may include Nb2O5 in an amount greater than or equal to 0.0 mol% and less than or equal to 50.0 mol%, greater than or equal to 0.5 mol% and less than or equal to 55.0 mol%, greater than or equal to 7.0 mol% and less than or equal to 40.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 40.0 mol%, greater than or equal to 14.0 mol% and less than or equal to 33.0 mol%, greater than or equal to 16.5 mol% and less than or equal to 30.5 mol%, greater than or equal to 18.83 mol% and less than or equal to 28.82 mol%, greater than or equal to 0.0 mol%. % and less than or equal to 55.0 mol %, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol %, greater than or equal to 0.5 mol % and less than or equal to 10.0 mol %, greater than or equal to 7.0 mol % and less than or equal to 55.0 mol %, greater than or equal to 7.0 mol % and less than or equal to 10.0 mol %, greater than or equal to 14.0 mol % and less than or equal to 55.0 mol %, greater than or equal to 14.0 mol % and less than or equal to 25.0 mol %, greater than or equal to 16.5 mol % and less than or equal to 25.0 mol %, greater than or equal to 19.0 mol % and less than or equal to 25.0 mol %.

[0065] In some embodiments, the sum of GeO2+TeO2 of the glass composition may be greater than or equal to 0.0 mol%, greater than or equal to 10.0 mol%, or greater than or equal to 20.0 mol%. In some other embodiments, the sum of GeO2+TeO2 of the glass composition may be less than or equal to 25.0 mol%, less than or equal to 20.0 mol%, or less than or equal to 10.0 mol%. In some more embodiments, the sum of GeO2+TeO2 of the glass composition may be greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 20.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%, greater than or equal to 10.0 mol% and less than or equal to 25.0 mol%, or greater than or equal to 10.0 mol% and less than or equal to 20.0 mol%.

[0066] In some embodiments, the glass composition may have a sum of Na2O+K2O greater than or equal to 0.0 mol%, or greater than or equal to 0.3 mol%.

[0067] In some embodiments, the sum of P2O5+B2O3 of the glass composition may be greater than or equal to 0.0 mol%, or greater than or equal to 20.0 mol%. In some other embodiments, the sum of P2O5+B2O3 of the glass composition may be less than or equal to 35.0 mol%, or less than or equal to 20.0 mol%. In some more embodiments, the sum of P2O5+B2O3 of the glass composition may be greater than or equal to 20.0 mol% and less than or equal to 35.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 35.0 mol%, or greater than or equal to 0.0 mol% and less than or equal to 20.0 mol%.

[0068] In some embodiments, the sum of TiO2+Nb2O5 of the glass composition may be greater than or equal to 0.0 mol%, greater than or equal to 25.0 mol%, greater than or equal to 36.0 mol%, or greater than or equal to 50.0 mol%. In some other embodiments, the sum of TiO2+Nb2O5 of the glass composition may be less than or equal to 70.0 mol%, less than or equal to 58.0 mol%, or less than or equal to 50.0 mol%. In some more embodiments, the sum of TiO2+Nb2O5 of the glass composition can be greater than or equal to 25.0 mol% and less than or equal to 70.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 70.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 58.0 mol%, greater than or equal to 0.0 mol% and less than or equal to 50.0 mol%, greater than or equal to 25.0 mol% and less than or equal to 58.0 mol%, greater than or equal to 25.0 mol% and less than or equal to 50.0 mol%, greater than or equal to 36.0 mol% and less than or equal to 70.0 mol%, greater than or equal to 36.0 mol% and less than or equal to 58.0 mol%, or greater than or equal to 36.0 mol% and less than or equal to 50.0 mol%.

[0069] In some embodiments, the difference in glass composition Alk2O+RO+Bi2O3+3*Al2O3-P2O5 is limited. When the difference (Alk2O+RO+Bi2O3+3*Al2O3-P2O5) is zero or positive (i.e., the total content of Alk2O, RO, Bi2O3 in the glass and three times the content of Al2O3 are equal to or greater than the content of P2O5), the glass can be melted from solid materials (e.g., metaphosphates (KPO3, NaPO3, BaP2O6, BiPO4, AlP3O9, etc.)), simplifying the melting process and reducing costs. When the difference (Alk2O+RO+Bi2O3+3*Al2O3-P2O5) is negative, it is generally necessary to use liquid starting materials (e.g., phosphoric acid (H3PO4)), making the process more complicated and expensive, or to use more expensive solid materials (e.g., titanium phosphate (TiP2O7)), which also increases the cost of the starting materials. Therefore, it is preferred that the difference (Alk2O+RO+Bi2O3+3*Al2O3-P2O5) is positive or zero. In some embodiments, the difference Alk2O+RO+Bi2O3+3*Al2O3-P2O5 of the glass may be greater than or equal to -8 mol%, greater than or equal to 0.000 mol%, or greater than or equal to 10 mol%. In some other embodiments, the difference Alk2O+RO+Bi2O3+3*Al2O3-P2O5 of the glass may be less than or equal to 11 mol%, less than or equal to 10 mol%, or less than or equal to 0.000 mol%. In some more embodiments, the difference in glass Alk2O+RO+Bi2O3+3*Al2O3-P2O5 can be greater than or equal to -8 mol% and less than or equal to 11 mol%, greater than or equal to -8 mol% and less than or equal to 10 mol%, greater than or equal to -8 mol% and less than or equal to 0.000 mol%, greater than or equal to 0.000 mol% and less than or equal to 11 mol%, or greater than or equal to 0.000 mol% and less than or equal to 10 mol%.

[0070] In some embodiments, the refractive index of the glass at 587.56 nm is n d It may be greater than or equal to 1.8, greater than or equal to 1.9, or greater than or equal to 2.0.

[0071] In some embodiments, the Abbe number of the glass is d It may be less than or equal to 20.0, less than or equal to 19.5, less than or equal to 19.0, or less than or equal to 18.5.

[0072] In some embodiments, the glass transition temperature T g The glass transition temperature T of the glass may be greater than or equal to 550°C and less than or equal to 650°C, and all ranges and subranges between the foregoing values.g The glass transition temperature T of the glass may be greater than or equal to 550° C., greater than or equal to 560° C., greater than or equal to 590° C., greater than or equal to 620° C., greater than or equal to 630° C., or greater than or equal to 640° C. In some other embodiments, the glass transition temperature T of the glass may be greater than or equal to 550° C., greater than or equal to 560° C., greater than or equal to 590° C., greater than or equal to 620° C., greater than or equal to 630° C., or greater than or equal to 640° C. g The glass transition temperature T of the glass may be less than or equal to 650° C., less than or equal to 640° C., less than or equal to 630° C., less than or equal to 620° C., less than or equal to 590° C., or less than or equal to 560° C. In some further embodiments, the glass transition temperature T g The temperature may be greater than or equal to 550°C and less than or equal to 650°C, greater than or equal to 550°C and less than or equal to 560°C, greater than or equal to 560°C and less than or equal to 650°C, greater than or equal to 560°C and less than or equal to 590°C, greater than or equal to 590°C and less than or equal to 650°C, greater than or equal to 590°C and less than or equal to 620°C, greater than or equal to 620°C and less than or equal to 650°C, greater than or equal to 620°C and less than or equal to 630°C, greater than or equal to 630°C and less than or equal to 650°C, greater than or equal to 630°C and less than or equal to 640°C.

[0073] In some embodiments, the ratio of the refractive index to the density of the glass ("refractive ratio") (n d -1) / d RT It may be greater than or equal to 0.20, greater than or equal to 0.22, or greater than or equal to 0.24.

[0074] In some embodiments, the density of glass at room temperature is RT Can be less than or equal to 5.5g / cm 3 , less than or equal to 5.2g / cm 3 , less than or equal to 5.0g / cm 3 , less than or equal to 4.8g / cm 3 , less than or equal to 4.6g / cm 3 , less than or equal to 4.4g / cm 3 , or less than or equal to 4.2g / cm 3 .

[0075] In some embodiments, the amount of glass n d -(1.14+0.192*d RT ) can be greater than or equal to 0.000.

[0076] In some embodiments, the amount of glass n d -(1.205+0.192*d RT ) can be greater than or equal to 0.000.

[0077] Refractive index n dWith density d RT is a glass property that can be predicted from the glass composition. Linear regression analysis was performed on the exemplary glasses of the present disclosure in the following example section and other glass compositions described in the literature to determine the properties that can be predicted for the refractive index n d and density d RT The composition dependence of the equation.

[0078] Satisfies the compositional constraints specified in Table 1 below and has the properties of interest (n d and RT ) of glass compositions (for each property (n d and RT ) were randomly selected from literature data in the publicly available SciGlass information system database and from exemplary glasses in the examples herein. Linear regression analysis was performed on the above specified data set and outliers were excluded to determine the values ​​in Table 2 below for predicting n d and RT The prediction parameter P n and P d Another subset of glass compositions that meet the compositional constraints of Table 1 was used as a validation set to evaluate the ability to interpolate within the compositional constraints of Table 1 and to predict the parameter P n and P d The standard deviations specified in Table 2 were established. An external data set of prior art glass compositions, also randomly selected from the SciGlass Information System database, was used to assess the ability to predict properties outside the composition limits of Table 1 with reasonable accuracy (n d and RT ) capability. Multiple iterations of this process are performed to determine the d and RT ) is the best formula. Formulas (I) and (II) in Table 2 are the results of the analysis.

[0079] The data of comparative glass compositions including training data set, validation data set and external data set used in linear regression modeling were obtained from the publicly available SciGlass information system database. The following formulas (I) and (II) were obtained based on linear regression analysis:

[0080] P n =1.865-0.0052736*P2O5+0.0071201*Nb2O5+0.0031659*TiO2-0.0008032*

[0081] BaO-0.0047736*K2O-0.00076807*CaO-0.0027991*Na2O-0.0016514*Li2O -0.00069646*SrO+0.0032628*WO3+0.007519*Bi2O3-0.0040698*B2O3-0.0 035951*SiO2-0.00067102*ZnO+0.0022313*ZrO2-0.0019531*MgO-0.00350 6*Al2O3+0.0019216*TeO2+0.0025766*PbO-0.0018844*GeO2+0.0065444*T l 2O+0.0052048*Ag2O,(I),

[0082] P d =4.45-0.020780*Al2O3-0.020918*B2O3+0.014152*BaO+0.061008*Bi2O3

[0083] -0.0067411*CaO+0.013529*CdO+0.012560*Cs2O+0.0028892*Ga2O3-0.0057012*GeO2-0.017838*K 2O+0.046524*La2O3-0.013919*Li2O-0.010279*MgO-0.0064231*MoO3-0.012983*Na2O+0.0083294* Nb2O5-0.028926*P2O5+0.031742*PbO-0.019022*SiO2+0.0045214*SrO+0.050158*Ta2O5+0.00884 86*TeO2-0.0063053*TiO2-0.018941*V2O5+0.027483*WO3-0.0010277*ZnO+0.0100487*ZrO2, (II).

[0084] In formulas (I) and (II) and Tables 1 and 2, P n is the predicted refractive index n at 587.56 nm d The predicted parameters are calculated from the components of the glass composition expressed in mol%, and P d is the predicted room temperature density d RT and are calculated from the components of the glass composition expressed in mol%.

[0085] In formulas (I) and (II), each component of the glass composition is listed by its chemical formula, wherein the chemical formula refers to the concentration of the component expressed in mole %. For example, for formulas (I) and (II), P2O5 refers to the concentration of P2O5 in the glass composition expressed in mole %. It should be understood that not all components listed in formulas (I) and (II) must be present in a particular glass composition, and that formulas (I) and (II) are equally applicable to glass compositions that contain fewer than all components listed in the formulas. It should also be understood that formulas (I) and (II) are also applicable to glass compositions within the scope of the present disclosure and claims that contain components other than the components listed in the formulas. If a component listed in formulas (I) and (II) is not present in a particular glass composition, the concentration of the component in the glass composition is 0 mole % and the contribution of the component to the value calculated by the formula is zero. In Table 1, R m O n is the sum of all oxides.

[0086] Table 1: Composition space used for modeling

[0087]

[0088] Table 2: Property prediction models

[0089]

[0090] Figure 1 is the parameter P calculated by formula (I) for some comparative glasses (“comparative glasses”) and some exemplary glasses (“exemplary glasses”) taken from the literature. n The measured refractive index n d The graph of the function of . Figure 1 As shown in the data, for most glasses, the parameter P n The standard deviation of the composition dependence is the measured n d The values ​​are within the range of ±0.015 units, corresponding to the standard errors specified in Table 2.

[0091] Figure 2 is the parameter P calculated by formula (II) for some reference glasses (“comparative glasses”) and some exemplary glasses (“exemplary glasses”) d The measured density d RT The graph of the function of . Figure 2 As shown in the data, for most glasses, the parameter P d The standard deviation of the composition dependence is the measured d RT The range is ±0.075 units, which corresponds to the standard deviation specified in Table 2.

[0092] Table 3 identifies combinations of components and their respective amounts according to some embodiments of the present disclosure. The exemplary glass A in Table 3 may include additional components according to any aspect of the present disclosure described herein.

[0093] Table 3: Exemplary Glass A

[0094] Components Amount (mol%) <![CDATA[P2O5]]> 15.9 to 50.0 mol% <![CDATA[Bi2O3]]> 4.5 to 50.0 mol% <![CDATA[TiO2]]> 0.0 to 50.0 mol% <![CDATA[Nb2O5]]> 0.0 to 50.0 mol% <![CDATA[Li2O]]> 0.0 to 25.0 mol% <![CDATA[K2O]]> 0.0 to 25.0 mol% <![CDATA[Na2O]]> 0.0 to 20.0 mol% <![CDATA[WO3]]> 0.0 to 6.0 mol% <![CDATA[Sum of (TiO2 + Nb2O5)]]> 25.0 to 70.0 mol% <![CDATA[Total of alkali metal oxides Alk2O]]> 0.5 to 30.0 mol% The sum of divalent metal oxides RO 0.5 to 30.0 mol% <![CDATA[Sum of (GeO2 + TeO2)]]> 0.0 to 25.0 mol%

[0095] Exemplary glass A according to an embodiment of the present disclosure may satisfy the following conditions:

[0096] Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol%]≥-8.0,

[0097] The chemical formulas herein refer to the amounts of the components in the glass expressed in mol %.

[0098] Table 4 identifies combinations of components and their respective amounts according to some embodiments of the present disclosure. The exemplary glass B in Table 4 may include additional components according to any aspect of the present disclosure described herein.

[0099] Table 4: Exemplary Glass B

[0100] Components Amount (mol%) <![CDATA[P2O5]]> 23.0 to 35.0 mol% <![CDATA[Bi2O3]]> 4.5 to 35.0 mol% <![CDATA[Nb2O5]]> 0.5 to 55.0 mol% <![CDATA[TiO2]]> 0.5 to 55.0 mol% <![CDATA[Li2O]]> 0.3 to 20.0 mol%

[0101] Exemplary glass B according to an embodiment of the present disclosure may satisfy the following conditions:

[0102] n d -(1.14+0.192*d RT )>0.000,

[0103] where n d is the refractive index at 587.56 nm, and d RT is the density at room temperature.

[0104] According to some embodiments of the present disclosure, exemplary glass B may also satisfy the following conditions:

[0105] n d -(1.205+0.192*d RT )>0.000,

[0106] where n d is the refractive index at 587.56 nm, and d RT is the density at room temperature.

[0107] Example

[0108] The following examples describe various features and advantages provided by the present disclosure and are not intended to limit the present disclosure and the appended claims.

[0109] To prepare glass samples for some exemplary glasses of the present disclosure, about 15 grams of each sample (content of target substance greater than 99.99 wt %) was melted from a batch of raw materials in a platinum or platinum rhodium crucible (Pt:Rh=80:20) at a temperature of about 1300°C for 1 hour. One of two controlled cooling conditions was applied. Under the first condition (designated as "15-minute test"), the sample was cooled from 1100°C to 500°C inside the furnace in about 15 minutes. Under the second condition (designated as "2.5-minute test"), the sample was cooled from 1100°C to 500°C in about 2.5 minutes. The temperature readings were taken by direct reading of the furnace temperature or using an IR camera reading with a calibrated scale. The first condition (15-minute test) corresponds approximately to a cooling rate of up to 300°C / min at a temperature of 1000°C, while the second test corresponds approximately to a cooling rate of up to 600°C / min at 1000°C. A temperature of 1000°C corresponds approximately to the temperature at which the expected cooling rate is close to the maximum. At lower temperatures, the cooling rate is significantly reduced. A typical schedule for the first and second cooling schemes is as follows: Figure 3 For these samples, the observations designated as "15-minute devitrification test" and "2.5-minute devitrification test" are designated in Table 5; an observation of "1" is used to indicate that the glass composition passes the corresponding test, wherein if the melt of the composition forms a glass that does not contain crystals visible under an optical microscope at a magnification of 100x to 500x, the composition is considered to have passed the designated devitrification test. An observation of "0" is used to indicate that the glass composition does not pass the designated devitrification test.

[0110] To prepare other glass samples for exemplary glasses of the present disclosure, one kilogram batch was prepared in a pure platinum crucible unless otherwise stated. The crucible was placed in a furnace set to a temperature of 1250°C, and the temperature in the furnace was then raised to 1300°C and held at 1300°C for 2 hours. The furnace temperature was then lowered to 1250°C to allow the glass to equilibrate at this temperature for one hour, and then poured onto a steel table and annealed at about Tg for one hour.

[0111] Some sample melts are also melted in a "one liter" platinum crucible heated by the Joule effect. In this process, about 3700g of raw materials (batch components) are used. At 1250°C, the crucible is filled with batch components within 1.5 hours. Then, the temperature is raised to 1300°C and maintained for one hour. During this step, the glass is continuously stirred at 60rpm. Then, the temperature is reduced to 1200°C to allow equilibrium for 30 minutes and continue stirring at a rate of 20rpm. The delivery tube is heated at 1225°C, and the glass melt is cast on a cooled graphite table to form glass. The glass is formed into rods with a thickness of about 25mm, a width of 50mm and a length of 90cm. These rods are detected under an optical microscope to check crystallization, and all are free of crystallization. It is observed under an optical microscope that the glass quality is good, and the rods are free of stripes and bubbles. The glass is placed at about T g The rods were then placed in an annealing furnace at about T for 1 hour to perform rough annealing. g The samples were annealed in a static furnace at 1 °C for one hour and then the temperature was decreased at 1 °C / min.

[0112] The chemical analysis of the samples tested was not carried out because similar samples prepared from independent melts were chemically analyzed by XRF (X-ray fluorescence for all oxides, except B2O3 and Li2O), by ICP (Inductively Coupled Plasma Spectroscopy for B2O3), by FES (Flame Emission Spectroscopy for Li2O). These analyses gave deviations from the batch composition within ±2.0 mass % for the main components.

[0113] Exemplary glass compositions are listed in Table 5. Comparative glass compositions are listed in Table 6. In Tables 5 and 6, the underlying abbreviation "n" refers to the refractive index at the corresponding wavelength in nm; for example, n 632.8nm Refers to the refractive index at a wavelength of 632.8nm.

[0114] Table 5: Exemplary glass compositions

[0115]

[0116] Table 5 (continued)

[0117]

[0118]

[0119] Table 5 (continued)

[0120]

[0121]

[0122] Table 5 (continued)

[0123]

[0124]

[0125] Table 5 (continued)

[0126]

[0127]

[0128] Table 5 (continued)

[0129]

[0130] Table 5 (continued)

[0131]

[0132]

[0133] Table 5 (continued)

[0134]

[0135]

[0136] Table 5 (continued)

[0137]

[0138]

[0139] Table 5 (continued)

[0140]

[0141]

[0142] Table 6 below lists the glass compositions and properties of comparative glasses C1 to C12.

[0143] Table 6: Composition and properties of comparative glass

[0144]

[0145] Table 6 (continued)

[0146]

[0147] The reference index of each of the comparative glasses listed in Table 6 is as follows: [1] CN113024107A; [2] JP2004123448A; [3] JP2006111499A; [4] JP2010083701; [5] US2021179479; [6] US8647994B2; [7] US8716157B2; [8] WO2019151404A1; [9] US2021048665;

[10] US7309670B2;

[11] US7553785B2;

[12] US7994082B2.

[0148] Figure 4 is a graph showing density parameters P for some of the exemplary glasses and some of the comparative glasses. d and the refractive index parameter P n The exemplary glasses (solid circles) are Examples 13 to 21, 34 to 49, 51 to 57, and 75 in Table 5. The comparative glasses (open circles) are Examples C1 to C8 in Table 6. The refractive index n used to predict the refractive index at 587.56 nm is determined according to formula (I). d The refractive index parameter P n According to formula (II), the density d at room temperature is determined RT The density parameter P d . Figure 4 All exemplary glasses and comparative glasses shown have the characteristics specified in Table 7.

[0149] Table 7: Figure 4 and Figure 5 Limitations of glass compositions shown

[0150] Components unit Minimum maximum <![CDATA[P2O5]]> Mole % 23 35 <![CDATA[Bi2O3]]> Mole % 4.5 35 <![CDATA[Nb2O5]]> Mole % 0.5 55 <![CDATA[TiO2]]> Mole % 0.5 55 <![CDATA[Li2O]]> Mole % 0.3 20

[0151] Figure 4 The comparative glass is selected as having the following characteristics among the known glasses having the characteristics specified in Table 7: Figure 4 The parameter P shown d The range of values ​​of parameter P n The highest value.

[0152] Corresponds to Figure 4 The line segments of the formula y=1.14+0.192*x shown provide a visual representation of the differences between the comparative glasses and the exemplary glasses 13 to 21, 34 to 49, 51 to 57, and 75 having the characteristics specified in Table 7. Figure 4 As shown, the exemplary glass (solid circle) falls above the line segment y=1.14+0.192*x and has no Figure 4The comparative glass shown (open circle) falls above the line segment y=1.14+0.192*x, where y corresponds to the parameter P used to predict the refractive index at 587.56 nm. n , and x corresponds to the parameter P used to predict the density at room temperature d In other words, Figure 4 Some of the exemplary glasses shown satisfy the following formula (III)(a), and no comparative glass satisfies the following formula (III)(a):

[0153] P n -(1.14+0.192*P d )>0.00(III)(a)

[0154] like Figure 4 As shown, some of the exemplary glasses fall above the line segment y=1.18+0.192*x, and none Figure 4 The comparative glass shown falls above the line segment y=1.18+0.192*x, where y corresponds to the parameter P used to predict the refractive index at 587.56 nm. n , and x corresponds to the parameter P used to predict the density at room temperature d In other words, Figure 4 Some of the exemplary glasses shown satisfy the following formula (III)(b), and no comparative glass satisfies the following formula (III)(b):

[0155] P n -(1.18+0.192*P d )>0.00(III)(b)

[0156] By predicting, Figure 4 The illustrative example shown is in d RT and n d The combinatorial aspect (i.e., for a given n d With lower d RT , or for a given d RT With higher n d ) is superior to the best known comparative glass having the characteristics specified in Table 7.

[0157] Figure 5 is a graph showing the density d at room temperature for some of the exemplary glasses and some of the comparative glasses. RT and the refractive index n at 587.56nm d The exemplary glasses (solid circles) are Examples 17, 34 to 43, 46 to 48, and 51 to 57 in Table 5. The comparative glasses (open circles) are Examples C2, C4, C5, C7, and C9 to C12 in Table 6. Figure 5All exemplary glasses and comparative glasses shown have the characteristics specified in Table 7.

[0158] Figure 5 The comparative glasses shown are selected as having the following characteristics among the known glasses having the characteristics specified in Table 7: Figure 5 The density d at room temperature is shown RT The refractive index n at 587.56 nm is within the range of d The highest measured value.

[0159] Corresponds to Figure 5 The line segments of the formula y=1.140+0.192*x shown provide a visual representation of the differences between the comparative glasses and the exemplary glasses 17, 34 to 43, 46 to 48, and 51 to 57 having the characteristics specified in Table 7. Figure 5 As shown, the exemplary glass mentioned (solid circle) falls above the line segment y=1.140+0.192*x and has no Figure 5 The comparative glass shown (open circle) falls above the line segment y=1.140+0.192*x, where y corresponds to n d , and x corresponds to d RT In other words, Figure 5 Some of the exemplary glasses shown satisfy the following formula (IV)(a), and no comparative glasses satisfy the following formula (IV)(a):

[0160] n d -(1.140+0.192*d RT )>0.00(IV)(a)

[0161] like Figure 5 As shown, some of the exemplary glasses fall above the line segment y=1.18+0.192*x, and none Figure 5 The comparative glass shown falls above the line segment y=1.18+0.192*x, where y corresponds to n d , and x corresponds to d RT In other words, Figure 5 Some of the exemplary glasses shown satisfy the following formula (IV)(b), and no comparative glasses satisfy the following formula (IV)(b):

[0162] n d -(1.18+0.192*d RT )>0.00(IV)(b)

[0163] Satisfying formula (IV)(b) Figure 5 The illustrated exemplary embodiment is characterized by a glass having the characteristics specified in Table 7. RT n at comparable values ​​ofd The highest value.

[0164] This means that under the conditions specified in Table 7 above, the density d RT Some of the exemplary glasses have a refractive index n at 587.56 nm. d This can be explained by the fact that, according to the measurements, in the glass at comparable d RT These exemplary glasses have a high n d The value of (i.e., according to the measurement, at d RT and n d The combinatorial aspect (i.e., for a given n d With lower d RT , or for a given d RT With higher n d ) is superior to the best known comparative glass having the characteristics specified in Table 7.

[0165] Draw on Figure 4 and Figure 5 The values ​​of all properties specified by Table 7 and formulas (III) (a), (III) (b), (IV) (a) and (IV) (b) for comparative glasses C1 to C12 are listed in Table 8 below. The full composition of the comparative glasses is presented in Table 6. The full composition and properties of the exemplary glasses are presented in Table 5.

[0166] Table 8: Properties of Comparative Example Glasses Having the Characteristics Specified in Table 7

[0167]

[0168]

[0169] Table 8 (continued)

[0170]

[0171] like Figure 4 and Figure 5 As shown, both the predicted and measured property data confirm that some of the exemplary glasses have a refractive index n at 587.56 nm that is greater than the best of the comparative glasses having the characteristics specified in Table 7. d The density at room temperature d RT A better combination.

[0172] The present disclosure includes the following non-limiting aspects. To the extent not yet described, any of the features of the first to thirty-fifth aspects may be combined in part or in whole with any one or more of the features of other aspects of the present disclosure to form additional aspects, even without explicitly describing such a combination.

[0173] According to a first aspect, a glass comprising a plurality of components is provided, wherein the glass has a composition of components, comprising: 15.9 mol% or more and 50.0 mol% or less of P2O5, 4.5 mol% or more and 50.0 mol% or less of Bi2O3, 0.0 mol% or more and 50.0 mol% or less of TiO2, 0.0 mol% or more and 50.0 mol% or less of Nb2O5, 0.0 mol% or more and 25.0 mol% or less of Li2O, 0.0 mol% or more and 25.0 mol% or less of K2O, 0.0 mol% or more and 20.0 mol% or less of Na2O, 0.0 mol% or more and 6.0 mol% or more of W. O3, greater than or equal to 0.0 mol% and less than or equal to 1.0 mol% V2O5, greater than or equal to 25.0 mol% and less than or equal to 70.0 mol% of the sum of TiO2 + Nb2O5, greater than or equal to 0.5 mol% and less than or equal to 30.0 mol% of Alk2O, greater than or equal to 0.5 mol% and less than or equal to 30.0 mol% of RO, greater than or equal to 0.0 mol% and less than or equal to 25.0 mol% of GeO2 + TeO2, and may optionally contain Al2O3, wherein the composition of the components satisfies the following condition: Alk2O + RO + Bi2O3 + 3*Al2O3-P2O5 [mol%] ≥ -8.0, wherein Alk2O is the sum of alkali metal oxides, and RO is the sum of divalent metal oxides.

[0174] According to a second aspect, there is provided the glass as described in the first aspect, wherein the glass satisfies the following conditions: d <4.8, and P n >2.0, where P n The refractive index n at 587.56 nm is predicted from the glass composition in terms of mole % of the components according to formula (I). d Parameters:

[0175] P n =1.865-0.0052736*P2O5+0.0071201*Nb2O5+0.0031659*TiO2-0.0008032*

[0176] BaO-0.0047736*K2O-0.00076807*CaO-0.0027991*Na2O-0.0016514*Li2O-0.000 69646*SrO+0.0032628*WO3+0.007519*Bi2O3-0.0040698*B2O3-0.0035951*SiO2- 0.00067102*ZnO+0.0022313*ZrO2-0.0019531*MgO-0.003506*Al2O3+0.0019216 *TeO2+0.0025766*PbO-0.0018844*GeO2+0.0065444*Tl2O+0.0052048*Ag2O, (I),

[0177] And P d The density d at room temperature is predicted from the glass composition in terms of mole % of the components according to formula (II). RT Parameters:

[0178] P d =4.45-0.020780*Al2O3-0.020918*B2O3+0.014152*BaO+0.061008*Bi2O3

[0179] -0.0067411*CaO+0.013529*CdO+0.012560*Cs2O+0.0028892*Ga2O3-0.0057012*GeO2-0.017838*K 2O+0.046524*La2O3-0.013919*Li2O-0.010279*MgO-0.0064231*MoO3-0.012983*Na2O+0.0083294* Nb2O5-0.028926*P2O5+0.031742*PbO-0.019022*SiO2+0.0045214*SrO+0.050158*Ta2O5+0.00884 86*TeO2-0.0063053*TiO2-0.018941*V2O5+0.027483*WO3-0.0010277*ZnO+0.0100487*ZrO2, (II).

[0180] According to a third aspect, there is provided a glass as described in any one of aspects 1-2, wherein the density of the glass at room temperature is RT Less than or equal to 4.8, and the refractive index n at 587.56nm d The value is greater than or equal to 2.0.

[0181] According to a fourth aspect, a glass as described in any one of aspects 1-3 is provided, wherein the Abbe number νd of the glass is less than or equal to 20.

[0182] According to a fifth aspect, there is provided a glass as described in the fourth aspect, wherein the Abbe number νd is less than or equal to 18.5.

[0183] According to a sixth aspect, there is provided a glass as described in any one of aspects 1 to 5, wherein the glass transition temperature T g Greater than or equal to 550°C and less than or equal to 650°C.

[0184] According to a seventh aspect, there is provided the glass of any one of aspects 1-6, wherein the glass does not crystallize when cooled from 1100° C. to 500° C. in air within 15 minutes.

[0185] According to an eighth aspect, a glass as described in any one of aspects 1 to 7 is provided, wherein the composition of the components comprises greater than or equal to 23.5 mol% and less than or equal to 25.5 mol% of P2O5, greater than or equal to 10.0 mol% and less than or equal to 40.0 mol% of Nb2O5, greater than or equal to 4.5 mol% and less than or equal to 30.0 mol% of Bi2O3, greater than or equal to 0.3 mol% and less than or equal to 40.0 mol% of TiO2, and greater than or equal to 0.0 mol% of TiO2. % and less than 15.0 mol % B2O3, greater than or equal to 0.0 mol % and less than 10.0 mol % BaO, greater than or equal to 0.0 mol % and less than 10.0 mol % CaO, greater than or equal to 0.0 mol % and less than 10.0 mol % K2O, greater than or equal to 0.0 mol % and less than 10.0 mol % Li2O, and greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % Na2O.

[0186] According to a ninth aspect, a glass as described in any of aspects 1-8 is provided, wherein the composition of components comprises one or more of the following components: 24.05 mol% or more and 25.05 mol% or less of P2O5, 14.0 mol% or more and 33.0 mol% or less of Nb2O5, 10.0 mol% or more and 36.0 mol% or less of TiO2, 5.0 mol% or more and 25.0 mol% or less of Bi2O3, 0.0 mol% or more and 9.0 mol% or less of BaO, 0.0 mol% or more and 9.0 mol% or less of CaO, 0.0 mol% or more and 7.5 mol% or less of K2O, 0.0 mol% or more and 6.5 mol% or less of Li2O, and 0.0 mol% or more and 6.5 mol% or less of Na2O.

[0187] According to a tenth aspect, a glass as described in any of aspects 1-9 is provided, wherein the composition of the components includes greater than or equal to 24.2 mol% and less than or equal to 25.0 mol% P2O5, greater than or equal to 16.5 mol% and less than or equal to 30.5 mol% Nb2O5, greater than or equal to 13.0 mol% and less than or equal to 33.0 mol% TiO2, greater than or equal to 5.0 mol% and less than or equal to 23.0 mol% Bi2O3, greater than or equal to 1.75 mol% and less than or equal to 8.00 mol% BaO, greater than or equal to 0.0 mol% and less than or equal to 9.0 mol% CaO, greater than or equal to 0.0 mol% and less than or equal to 7.5 mol% K2O, greater than or equal to 0 mol% and less than or equal to 5.75 mol% Li2O, and greater than or equal to 0 mol% and less than or equal to 5.75 mol% Na2O.

[0188] According to an eleventh aspect, a glass as described in any one of aspects 1 to 10 is provided, wherein the composition of the components satisfies the following condition: Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol %]≥0.000.

[0189] According to a twelfth aspect, a glass as described in any of aspects 1-7 and 11 is provided, wherein the composition of the components comprises greater than or equal to 18.0 mol % and less than or equal to 28.0 mol %, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % TeO2, greater than or equal to 0.0 mol % and less than or equal to 5.0 mol % GeO2, greater than or equal to 0.0 mol % and less than or equal to 5.0 mol % SiO2, and a sum of P2O5+B2O3 of greater than or equal to 20.0 mol % and less than or equal to 35.0 mol %.

[0190] According to a thirteenth aspect, a glass as described in any of aspects 1-12 is provided, wherein the composition of the components comprises greater than or equal to 0.1 mol % Li2O and greater than or equal to 0.3 mol % of the sum of Na2O+K2O.

[0191] According to a fourteenth aspect, a glass as described in any of aspects 1-13 is provided, wherein the composition of the component comprises greater than or equal to 0.3 mol % and less than or equal to 20.0 mol % of R2O and greater than or equal to 0.3 mol % and less than or equal to 20.0 mol % of RO, wherein R2O is the sum of monovalent metal oxides.

[0192] According to a fifteenth aspect, there is provided a method for manufacturing an optical element, the method comprising: processing glass, wherein the glass is the glass according to any one of aspects 1-14.

[0193] According to a sixteenth aspect, an optical element comprising glass is provided, wherein the glass is the glass according to any one of aspects 1-15.

[0194] According to a seventeenth aspect, a glass comprising a plurality of components is provided, wherein the composition of the components of the glass comprises 23.0 mol% or more and 35.0 mol% or less of P2O5, 4.5 mol% or more and 35.0 mol% or less of Bi2O3, 0.5 mol% or more and 55.0 mol% or less of Nb2O5, 0.5 mol% or more and 55.0 mol% or less of TiO2, 0.5 mol% or more and 0.6 mol% or less of TiO2, 0.5 mol% or more and 0.7 ...6 mol% or less of Nb2O5, 0.5 mol% or more and 0.6 mol% or less of TiO2, 0.5 mol% or more and 0.6 mol% or less of TiO2, 0.5 mol% or more and 0.6 mol% or less of Nb2O5, 0.5 mol% or more and 0.6 mol% or less of TiO2, 0.5 mol% or more and 0.6 mol% or less of 3 mol % and less than or equal to 20.0 mol % of Li2O, and may optionally contain one or more components selected from BaO, K2O, CaO, Na2O, SrO, WO3, B2O3, SiO2, ZnO, ZrO2, MgO, Al2O3, TeO2, PbO, GeO2, Tl2O, Ag2O, CdO, Cs2O, Ga2O3, La2O3, MoO3, Ta2O5 and V2O5, and the glass satisfies the following conditions: P n -(1.14+0.192*P d )>0.000, where P n The refractive index n at 587.56 nm is predicted from the glass composition in terms of mole % of the components according to formula (I). d Parameters:

[0195] P n =1.865-0.0052736*P2O5+0.0071201*Nb2O5+0.0031659*TiO2-0.0008032*

[0196] BaO-0.0047736*K2O-0.00076807*CaO-0.0027991*Na2O-0.0016514*Li2O-0.000 69646*SrO+0.0032628*WO3+0.007519*Bi2O3-0.0040698*B2O3-0.0035951*SiO2- 0.00067102*ZnO+0.0022313*ZrO2-0.0019531*MgO-0.003506*Al2O3+0.0019216 *TeO2+0.0025766*PbO-0.0018844*GeO2+0.0065444*Tl2O+0.0052048*Ag2O, (I),

[0197] And P dThe density d at room temperature is predicted from the glass composition in terms of mole % of the components according to formula (II). RT Parameters:

[0198] P d =4.45-0.020780*Al2O3-0.020918*B2O3+0.014152*BaO+0.061008*Bi2O3

[0199] -0.0067411*CaO+0.013529*CdO+0.012560*Cs2O+0.0028892*Ga2O3-0.0057012*GeO2-0.017838*K 2O+0.046524*La2O3-0.013919*Li2O-0.010279*MgO-0.0064231*MoO3-0.012983*Na2O+0.0083294* Nb2O5-0.028926*P2O5+0.031742*PbO-0.019022*SiO2+0.0045214*SrO+0.050158*Ta2O5+0.00884 86*TeO2-0.0063053*TiO2-0.018941*V2O5+0.027483*WO3-0.0010277*ZnO+0.0100487*ZrO2, (II).

[0200] According to an eighteenth aspect, there is provided the glass as described in the seventeenth aspect, wherein the glass satisfies the following conditions: d -(1.14+0.192*d RT )>0.000, where n d is the refractive index at 587.56 nm, d RT [g / cm 3 ] is the density at room temperature.

[0201] According to a nineteenth aspect, there is provided a glass as described in any one of aspects 17-18, wherein the glass satisfies the following conditions: n d -(1.205+0.192*d RT )>0.000, where n d is the refractive index at 587.56 nm, d RT [g / cm 3 ] is the density at room temperature.

[0202] According to the twentieth aspect, there is provided the glass as described in any one of aspects 17-19, wherein the glass satisfies the following conditions: n -(1.205+0.192*P d)>0.000.

[0203] According to the twenty-first aspect, there is provided the glass as described in any one of aspects 17-20, wherein the glass satisfies the following conditions: d <4.8, and P n >2.0.

[0204] According to the twenty-second aspect, the glass according to any one of aspects 17-21 is provided, wherein the density of the glass at room temperature is RT Less than or equal to 4.8g / cm 3 , and the refractive index n at 587.56nm d Greater than or equal to 2.0.

[0205] According to the twenty-third aspect, there is provided a glass as described in any one of aspects 17-22, wherein the Abbe number v of the glass d Less than or equal to 20.

[0206] According to a twenty-fourth aspect, there is provided a glass according to the twenty-third aspect, wherein the Abbe number ν d Less than or equal to 18.5.

[0207] According to the twenty-fifth aspect, there is provided a glass as described in any one of aspects 17-24, wherein the glass transition temperature T g Greater than or equal to 550°C and less than or equal to 650°C.

[0208] According to a twenty-sixth aspect, there is provided the glass of any one of aspects 17-25, wherein the glass does not crystallize when cooled from 1100° C. to 500° C. in air within 15 minutes.

[0209] According to a twenty-seventh aspect, a glass as described in any one of aspects 17 to 26 is provided, wherein the composition of the components comprises greater than or equal to 23.5 mol% and less than or equal to 25.5 mol% of P2O5, greater than or equal to 10.0 mol% and less than or equal to 40.0 mol% of Nb2O5, greater than or equal to 4.5 mol% and less than or equal to 30.0 mol% of Bi2O3, greater than or equal to 0.5 mol% and less than or equal to 40.0 mol% of TiO2, greater than or equal to 0.3 mol% and less than or equal to 10.0 mol % Li2O, greater than or equal to 0.0 mol % and less than or equal to 15.0 mol % B2O3, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % BaO, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % CaO, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % K2O, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % Na2O, and greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % WO3.

[0210] According to a twenty-eighth aspect, a glass as described in any one of aspects 17-27 is provided, wherein the composition of the components includes one or more of the following components: greater than or equal to 24.05 mol% and less than or equal to 25.05 mol% of P2O5, greater than or equal to 14.0 mol% and less than or equal to 33.0 mol% of Nb2O5, greater than or equal to 10.0 mol% and less than or equal to 36.0 mol% of TiO2, greater than or equal to 5.0 mol% and less than or equal to 25.0 mol% of Bi 2O3, 0.3 mol% or more and 6.5 mol% or less of Li2O, 0.0 mol% or more and 9.0 mol% or less of BaO, 0.0 mol% or more and 9.0 mol% or less of CaO, 0.0 mol% or more and 7.5 mol% or less of KO, 0.0 mol% or more and 6.5 mol% or less of Na2O, and 0.0 mol% or more and 6.5 mol% or less of WO3.

[0211] According to a twenty-ninth aspect, a glass as described in any one of aspects 17 to 28 is provided, wherein the composition of the components comprises greater than or equal to 24.2 mol% and less than or equal to 25.0 mol% of P2O5, greater than or equal to 16.5 mol% and less than or equal to 30.5 mol% of Nb2O5, greater than or equal to 13.0 mol% and less than or equal to 33.0 mol% of TiO2, greater than or equal to 5.0 mol% and less than or equal to 23.0 mol% of Bi2O3, greater than or equal to 14.5 mol% and less than or equal to 25.0 mol% of Nb2O5, greater than or equal to 16.5 mol% and less than or equal to 30.5 mol% of TiO2, % and less than or equal to 8.00 mol % of BaO, 0.3 mol % or more and less than or equal to 5.8 mol % of Li2O, 0.0 mol % or more and less than or equal to 9.0 mol % of CaO, 0.0 mol % or more and less than or equal to 7.5 mol % of K2O, 0.0 mol % or more and less than or equal to 6.0 mol % of WO3, and 0 mol % or more and less than or equal to 5.75 mol % of Na2O.

[0212] According to the thirtieth aspect, a glass as described in any of aspects 17-29 is provided, wherein the composition of the components satisfies the following condition: Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol %]≥0.000, wherein Alk2O is the sum of alkali metal oxides and RO is the sum of divalent metal oxides.

[0213] According to a thirty-first aspect, a glass as described in any of aspects 17-26 and 30 is provided, wherein the composition of the components comprises greater than or equal to 23.0 mol % and less than or equal to 28.0 mol %, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % TeO2, greater than or equal to 0.0 mol % and less than or equal to 5.0 mol % GeO2, greater than or equal to 0.0 mol % and less than or equal to 5.0 mol % SiO2, and greater than or equal to 20.0 mol % and less than or equal to 35.0 mol % of the sum of P2O5+B2O3.

[0214] According to a thirty-second aspect, a glass as described in any of aspects 17-31 is provided, wherein the composition of the components comprises a sum of Na2O+K2O greater than or equal to 0.3 mol%.

[0215] According to a thirty-third aspect, a glass as described in any of aspects 17-32 is provided, wherein the composition of the component comprises greater than or equal to 0.3 mol % and less than or equal to 20.0 mol % of R2O and greater than or equal to 0.3 mol % and less than or equal to 20.0 mol % of RO, wherein R2O is the sum of monovalent metal oxides and RO is the sum of divalent metal oxides.

[0216] According to a thirty-fourth aspect, there is provided a method for manufacturing an optical element, the method comprising: processing glass, wherein the glass is the glass described in any one of aspects 17-33.

[0217] According to a thirty-fifth aspect, an optical element comprising glass is provided, wherein the glass is the glass according to any one of aspects 17-34.

[0218] Many changes and modifications may be made to the above-described embodiments of the present disclosure without departing from the spirit and various principles of the present disclosure. All of these modifications and variations are intended to be included within the scope of the present disclosure and protected by the claims.

[0219] To the extent not yet described, different features of various aspects of the present disclosure may be used in combination with each other as desired. Not explicitly stating or describing a particular feature for each aspect of the present disclosure does not mean that it cannot be explained or described, but rather is for the sake of brevity of description. Thus, various features of different aspects may be mixed and matched as desired to form new aspects, regardless of whether the new aspects are explicitly disclosed.

Claims

1. A glass comprising a plurality of components, the glass having a composition of the components, comprising: greater than or equal to 15.9 mol % and less than or equal to 50.0 mol % of P2O5, 4.5 mol % or more and 50.0 mol % or less of Bi2O3, greater than or equal to 0.0 mol % and less than or equal to 50.0 mol % of TiO2, greater than or equal to 0.0 mol % and less than or equal to 50.0 mol % Nb2O5, greater than or equal to 0.0 mol % and less than or equal to 25.0 mol % of Li2O, greater than or equal to 0.0 mol % and less than or equal to 25.0 mol % of K2O, greater than or equal to 0.0 mol % and less than or equal to 20.0 mol % of Na2O, WO3 greater than or equal to 0.0 mol % and less than or equal to 6.0 mol %, greater than or equal to 0.0 mol % and less than or equal to 1.0 mol % of V2O5, The sum of TiO2+Nb2O5 is greater than or equal to 25.0 mol % and less than or equal to 70.0 mol %, The sum of greater than or equal to 0.5 mol % and less than or equal to 30.0 mol % of Alk2O, The sum of greater than or equal to 0.5 mol % and less than or equal to 30.0 mol % of RO, The sum of GeO2+TeO2 is greater than or equal to 0.0 mol% and less than or equal to 25.0 mol%, and optionally containing Al2O3, The composition of the components satisfies the following conditions: Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol%]≥-8.0, Where Alk2O is the sum of alkali metal oxides, and RO is the sum of divalent metal oxides.

2. The glass according to claim 1, wherein the glass satisfies the following conditions: P d <4.8, and P n >2.0, in P n The refractive index n at 587.56 nm is predicted by calculation from the glass composition in terms of the mole % of the components according to formula (I). d Parameters: P n =1.865-0.0052736*P2O5+0.0071201*Nb2O5+0.0031659*TiO2-0.0008032* BaO-0.0047736*K2O-0.00076807*CaO-0.0027991*Na2O-0.0016514*Li2O-0.000 69646*SrO+0.0032628*WO3+0.007519*Bi2O3-0.0040698*B2O3-0.0035951*SiO2- 0.00067102*ZnO+0.0022313*ZrO2-0.0019531*MgO-0.003506*Al2O3+0.0019216 *TeO2+0.0025766*PbO-0.0018844*GeO2+0.0065444*Tl2O+0.0052048*Ag2O, (I), And P d The density d at room temperature is calculated from the glass composition in terms of the mole % of the components according to formula (II). RT Parameters: <h2 style=";text-align:left;direction:ltr">P<h2 style=";text-align:left;direction:ltr"> d <h2 style=";text-align:left;direction:ltr"> =4.45-0.020780*Al2O3-0.020918*B2O3+0.014152*BaO+0.061008*Bi2O3- 0.0067411*CaO+0.013529*CdO+0.012560*Cs2O+0.0028892*Ga2O3-0.0057012*GeO2-0.017838*K2 O+0.046524*La2O3-0.013919*Li2O-0.010279*MgO-0.0064231*MoO3-0.012983*Na2O+0.0083294* Nb2O5-0.028926*P2O5+0.031742*PbO-0.019022*SiO2+0.0045214*SrO+0.050158*Ta2O5+0.00884 86*TeO2-0.0063053*TiO2-0.018941*V2O5+0.027483*WO3-0.0010277*ZnO+0.0100487*ZrO2, (II).

3. The glass according to any one of claims 1 to 2, wherein the glass has Abbe number ν less than or equal to 20 d .

4. The glass of any one of claims 1 to 3, wherein the glass does not crystallize when cooled from 1100°C to 500°C in air within 15 minutes.

5. The glass of any one of claims 1 to 4, wherein the composition of the components comprises: greater than or equal to 23.5 mol % and less than or equal to 25.5 mol % of P2O5, greater than or equal to 10.0 mol % and less than or equal to 40.0 mol % Nb2O5, 4.5 mol % or more and 30.0 mol % or less of Bi2O3, greater than or equal to 0.3 mol % and less than or equal to 40.0 mol % of TiO2, greater than or equal to 0.0 mol % and less than or equal to 15.0 mol % B2O3, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % of BaO, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % of CaO, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % of K2O, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % Li2O, and Greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % Na2O.

6. The glass of any one of claims 1-5, wherein the composition of the components comprises: greater than or equal to 24.2 mol % and less than or equal to 25.0 mol % of P2O5, greater than or equal to 16.5 mol % and less than or equal to 30.5 mol % Nb2O5, greater than or equal to 13.0 mol % and less than or equal to 33.0 mol % TiO2, 5.0 mol % or more and 23.0 mol % or less of Bi2O3, greater than or equal to 1.75 mol % and less than or equal to 8.00 mol % of BaO, greater than or equal to 0.0 mol % and less than or equal to 9.0 mol % of CaO, greater than or equal to 0.0 mol % and less than or equal to 7.5 mol % of K2O, greater than or equal to 0 mol % and less than or equal to 5.75 mol % Li2O, and Greater than or equal to 0 mol % and less than or equal to 5.75 mol % Na2O.

7. The glass according to any one of claims 1 to 6, wherein the composition of the components satisfies the following conditions: Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol%]≥0.

000.

8. The glass of any one of claims 1-7, wherein the composition of the components comprises: greater than or equal to 0.1 mol % Li2O, and Greater than or equal to 0.3 mol% of the sum of Na2O + K2O.

9. A method for manufacturing an optical element, the method comprising processing glass, wherein the glass is the glass according to any one of claims 1 to 8.

10. An optical element comprising glass, wherein the glass is the glass according to any one of claims 1 to 9.

11. A glass comprising a plurality of components, the glass having a composition of the components, comprising: greater than or equal to 23.0 mol % and less than or equal to 35.0 mol % of P2O5, 4.5 mol % or more and 35.0 mol % or less of Bi2O3, greater than or equal to 0.5 mol % and less than or equal to 55.0 mol % Nb2O5, greater than or equal to 0.5 mol % and less than or equal to 55.0 mol % TiO2, 0.3 mol % or more and 20.0 mol % or less of Li2O, and optionally comprising one or more components selected from the group consisting of BaO, K2O, CaO, Na2O, SrO, WO3, B2O3, SiO2, ZnO, ZrO2, MgO, Al2O3, TeO2, PbO, GeO2, Tl2O, Ag2O, CdO, Cs2O, Ga2O3, La2O3, MoO3, Ta2O5 and V2O5, The glass meets the following conditions: P n -(1.14+0.192*P d )>0.000, in P n The refractive index n at 587.56 nm is predicted by calculation from the glass composition in terms of the mole % of the components according to formula (I). d : P n =1.865-0.0052736*P2O5+0.0071201*Nb2O5+0.0031659*TiO2-0.0008032* BaO-0.0047736*K2O-0.00076807*CaO-0.0027991*Na2O-0.0016514*Li2O-0.000 69646*SrO+0.0032628*WO3+0.007519*Bi2O3-0.0040698*B2O3-0.0035951*SiO2- 0.00067102*ZnO+0.0022313*ZrO2-0.0019531*MgO-0.003506*Al2O3+0.0019216 *TeO2+0.0025766*PbO-0.0018844*GeO2+0.0065444*Tl2O+0.0052048*Ag2O, (I), And P d The density d at room temperature is predicted by calculation from the glass composition in terms of the mole % of the components according to formula (II). RT Parameters: <h2 style=";text-align:left;direction:ltr">P<h2 style=";text-align:left;direction:ltr"> d <h2 style=";text-align:left;direction:ltr"> =4.45-0.020780*Al2O3-0.020918*B2O3+0.014152*BaO+0.061008*Bi2O3- 0.0067411*CaO+0.013529*CdO+0.012560*Cs2O+0.0028892*Ga2O3-0.0057012*GeO2-0.017838*K2 O+0.046524*La2O3-0.013919*Li2O-0.010279*MgO-0.0064231*MoO3-0.012983*Na2O+0.0083294* Nb2O5-0.028926*P2O5+0.031742*PbO-0.019022*SiO2+0.0045214*SrO+0.050158*Ta2O5+0.00884 86*TeO2-0.0063053*TiO2-0.018941*V2O5+0.027483*WO3-0.0010277*ZnO+0.0100487*ZrO2, (II).

12. The glass according to claim 11, wherein the glass satisfies the following conditions: n d -(1.14+0.192*d RT )>0.000, where n d is the refractive index at 587.56 nm, d RT [g / cm 3 ] is the density at room temperature.

13. The glass according to any one of claims 11 to 12, wherein the glass has Abbe number ν less than or equal to 20 d .

14. The glass of any one of claims 11-13, wherein the glass does not crystallize when cooled from 1100°C to 500°C in air within 15 minutes.

15. The glass of any one of claims 11-14, wherein the composition of the components comprises: greater than or equal to 23.5 mol % and less than or equal to 25.5 mol % of P2O5, greater than or equal to 10.0 mol % and less than or equal to 40.0 mol % Nb2O5, 4.5 mol % or more and 30.0 mol % or less of Bi2O3, greater than or equal to 0.5 mol % and less than or equal to 40.0 mol % of TiO2, greater than or equal to 0.3 mol % and less than or equal to 10.0 mol % of Li2O, greater than or equal to 0.0 mol % and less than or equal to 15.0 mol % B2O3, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % of BaO, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % of CaO, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % of K2O, greater than or equal to 0.0 mol % and less than or equal to 10.0 mol % Na2O, and WO3 is greater than or equal to 0.0 mol% and less than or equal to 10.0 mol%.

16. The glass of any one of claims 11-15, wherein the composition of the components comprises: greater than or equal to 24.2 mol % and less than or equal to 25.0 mol % of P2O5, greater than or equal to 16.5 mol % and less than or equal to 30.5 mol % Nb2O5, greater than or equal to 13.0 mol % and less than or equal to 33.0 mol % TiO2, 5.0 mol % or more and 23.0 mol % or less of Bi2O3, greater than or equal to 1.75 mol % and less than or equal to 8.00 mol % of BaO, greater than or equal to 0.3 mol % and less than or equal to 5.8 mol % Li2O, greater than or equal to 0.0 mol % and less than or equal to 9.0 mol % of CaO, greater than or equal to 0.0 mol % and less than or equal to 7.5 mol % of K2O, 0.0 mol % or more and 6.0 mol % or less of WO3, and Greater than or equal to 0 mol % and less than or equal to 5.75 mol % Na2O.

17. The glass of any one of claims 11 to 16, wherein the composition of the components satisfies the following conditions: Alk2O+RO+Bi2O3+3*Al2O3-P2O5[mol%]≥0.000, Wherein the chemical formula means the content of the corresponding component in the glass, Alk2O is the sum of alkali metal oxides, and RO is the sum of divalent metal oxides.

18. The glass of any one of claims 11-17, wherein the composition comprises: Greater than or equal to 0.3 mol% of the sum of Na2O + K2O.

19. The glass of any one of claims 11-18, wherein the composition of the components comprises 0.3 mol % or more and 20.0 mol % or less of R2O, and greater than or equal to 0.3 mol % and less than or equal to 20.0 mol % RO, Where R2O is the sum of monovalent metal oxides, and RO is the sum of divalent metal oxides.

20. A method for manufacturing an optical element, the method comprising processing glass, wherein the glass is the glass according to any one of claims 11 to 19.

21. An optical element comprising glass, wherein the glass is the glass according to any one of claims 11 to 20.

Citation Information

Patent Citations

  • High-refraction high-dispersion optical glass and optical element

    CN113024107A

  • Optical glass suitable for being molded

    JP2004123448A

  • Optical glass, preform for precision press molding, and their manufacturing method, optical element and its manufacturing method

    JP2006111499A

  • Optical glass, glass gob for press forming and optical element

    JP2010083701A

  • Optical glass and optical component

    US20210179479A1