Gallium nitride sintered body and its manufacturing method

By reacting nitrogen compound gas with gallium nitride bulk material under specific conditions to form a dense surface layer, the densification and re-oxidation problems of gallium nitride sintered bodies in hot pressing are solved, improving its mechanical properties and oxidation resistance, making it suitable for applications such as sputtering targets.

CN118922395BActive Publication Date: 2026-11-10TOSOH CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380029836.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-17
Publication Date
2026-11-10
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Gallium nitride sintered bodies prepared by existing hot pressing processes are difficult to densify and are prone to re-oxidation, leading to increased oxygen content and affecting their application performance.

Method used

By reacting gallium nitride bulk with nitrogen-containing compound gas under specific conditions, a dense surface layer is formed, which inhibits re-oxidation, controls the oxygen content to below 0.3 atm%, controls the Ga/(Ga+N) ratio to between 0.5 and 0.60, and optimizes the density to the range of 3.80 g/cm3 to 5.50 g/cm3.

Benefits of technology

It achieves densification and re-oxidation suppression of gallium nitride sintered bodies, improves mechanical properties and oxidation resistance, and is suitable for applications such as sputtering targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922395B_ABST
    Figure CN118922395B_ABST
Patent Text Reader

Abstract

This invention provides at least one of the following: a gallium nitride sintered body, a method for manufacturing the same, and its use, which suppresses the increase in oxygen content due to re-oxidation after sintering compared to conventional gallium nitride sintered bodies obtained by hot pressing; a gallium nitride sintered body having a surface layer with a higher density than the interior of the sintered body; and the atomic weight ratio of gallium to the sum of gallium and nitrogen being greater than 0.5 and less than 0.60.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to sintered gallium nitride. Background Technology

[0002] To stably form gallium nitride (GaN) films via sputtering, a sintered GaN body is used as the sputtering target. Such GaN sintered bodies are manufactured, for example, by hot isostatic pressing (HIP). However, HIP is not only costly but also makes it difficult to produce large sintered bodies. On the other hand, hot pressing (HP) is known as a cheaper method for manufacturing GaN sintered bodies than HIP. However, GaN is difficult to densify in HP. Furthermore, the oxygen content of sintered bodies obtained by HP tends to increase after sintering due to residual metallic gallium, oxidation of GaN, and re-oxidation of the sintered body.

[0003] Therefore, further densification and reduction of oxygen content in gallium nitride sintered bodies manufactured by HP processing have been studied to date (e.g., Patent Documents 1-3).

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-144424

[0007] Patent Document 2: Japanese Patent Application Publication No. 2017-024970

[0008] Patent Document 3: Japanese Patent Application Publication No. 2019-001681 Summary of the Invention

[0009] The problem the invention aims to solve

[0010] Patent Document 1 reduces gallium oxide by flowing ammonia gas into the sintered body obtained by HP treatment, thereby lowering the oxygen content of the sintered body. However, since gallium oxide has a higher density than gallium nitride, it is difficult to further densify the gallium nitride sintered body while reducing gallium oxide.

[0011] Patent documents 2 and 3 use gallium nitride powder with low oxygen concentration as the raw material for gallium nitride. Using this powder, a sintered body with low oxygen content can be obtained. However, patent documents 2 and 3 are improvements on the raw material side and do not solve the problems of the HP treatment itself. Furthermore, they are not techniques that directly prevent the increase in oxygen content in the sintered body caused by re-oxidation.

[0012] The purpose of this disclosure is to provide at least one of the following: a gallium nitride sintered body, a method for manufacturing the same, and a use thereof, which, compared to conventional gallium nitride sintered bodies obtained by HP processing, suppresses the increase in oxygen content caused by re-oxidation after sintering.

[0013] Solution for solving the problem

[0014] The inventors investigated the prevention of re-oxidation and densification of gallium nitride sintered bodies obtained by HP treatment after sintering, focusing on the metallic gallium contained in the gallium nitride sintered bodies. They further discovered that by nitriding such metallic gallium under specific conditions, densification of the sintered body can be achieved, and re-oxidation after sintering can be suppressed.

[0015] That is, the present invention is as described in the claims, and the main points of this disclosure are as follows.

[0016] [1] A gallium nitride sintered body having a surface layer with a higher density than the interior of the sintered body, and the atomic weight ratio of gallium to the sum of gallium and nitrogen being greater than 0.5 and less than 0.60.

[0017] [2] The oxygen content of the sintered body described in [1] above is less than 0.3 atm%.

[0018] [3] The sintered body described in [1] or [2] above has a measured density of 3.80 g / cm³. 3 Above and 5.50 g / cm 3 the following.

[0019] [4] The sintered body according to any one of [1] to [3] above contains gallium.

[0020] [5] A method for manufacturing a sintered body according to any one of [1] to [4] above, comprising the following steps:

[0021] The nitrogen-containing compound gas is reacted with the bulk gallium nitride under a nitrogen-containing compound gas flow atmosphere of 0.5 L / min or higher and a reaction temperature of 1025 °C or lower.

[0022] [6] According to the manufacturing method described in [5] above, the bulk body is a pre-sintered body of gallium nitride.

[0023] [7] According to the manufacturing method described in [6] above, the pre-sintered body is a gallium nitride sintered body obtained by hot pressing.

[0024] [8] According to the manufacturing method described in [5] above, the bulk body is a shaped body of gallium nitride.

[0025] [9] The manufacturing method according to any one of [5] to [8] above, wherein the bulk contains at least gallium metal on its surface.

[0026]

[10] The manufacturing method according to any one of [5] to [9] above, wherein the nitrogen-containing compound gas is one or more gases selected from the group consisting of ammonia, hydrazine and alkylamine.

[0027]

[11] A sputtering target comprising any one of the sintered bodies described in any one of [1] to [4] above.

[0028] The effects of the invention

[0029] According to this disclosure, at least one of the following can be provided: a gallium nitride sintered body, a method for manufacturing the same, and its use, in which the increase in oxygen content due to re-oxidation after sintering is suppressed compared to conventional gallium nitride sintered bodies obtained by HP processing. Attached Figure Description

[0030] Figure 1 SEM image of the cross-section of the sintered body of Example 4 (magnification: 500x).

[0031] Figure 2 SEM image of the cross section of the sintered body of Comparative Example 1 (magnification: 500x). Detailed Implementation

[0032] The following describes an example of an embodiment of the sintered body of the present disclosure.

[0033] The sintered body of this embodiment is a gallium nitride sintered body having a surface layer with a higher density than the interior of the sintered body, and having an atomic weight ratio of gallium to the sum of gallium and nitrogen of more than 0.5 and less than 0.60.

[0034] This embodiment relates to a gallium nitride (GaN) sintered body. A gallium nitride (GaN) sintered body is a sintered body with gallium nitride as the main component (matrix, parent phase), primarily composed of gallium nitride, and is thus called a gallium nitride sintered body. However, it may also contain components other than gallium nitride, such as metallic gallium, and preferably includes metallic gallium. For example, the sintered body of this embodiment can be described as a sintered body containing metallic gallium and primarily composed of gallium nitride.

[0035] The sintered body of this embodiment may contain doping elements. Examples of doping elements for forming an n-type semiconductor include one or more selected from the group consisting of silicon (Si), germanium (Ge), tin (Sn), and lead (Pb). Examples of doping elements for forming a p-type semiconductor include one or more selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), vanadium (V), zinc (Zn), and cadmium (Cd). Examples of doping elements for forming an LED with arbitrary color rendering include at least one of aluminum (Al) and indium (In).

[0036] The sintered body of this embodiment has a surface layer with a higher density than the interior of the sintered body. This surface layer is not easily oxidized and can significantly suppress the re-oxidation of the sintered body.

[0037] In this embodiment, the surface layer and the interior of the sintered body can be observed using a scanning electron microscope (hereinafter also referred to as "SEM") on the cross-section of the sintered body. Figure 1 As shown in the SEM image of the cross-section of the sintered body, in the direction from the surface towards the opposite surface ( Figure 1 The dense tissue structure changes to a sparse tissue structure in the direction of the arrow (hereinafter also referred to as the "thickness direction"), and it is possible to identify regions where dense and sparse parts coexist. Figure 1 The dotted line area (hereinafter also referred to as the "variation area"). The presence of a variation area observable in SEM images at magnification of 100-500x is considered as the presence of a surface layer in the sintered body. On the other hand, as... Figure 2 As shown, if there is a uniform microstructure in the thickness direction and no variation area can be identified, it is considered that there is no surface layer.

[0038] In the sintered body of this embodiment, the density of the surface layer is higher than that of the interior of the sintered body. By having such a surface layer, the mechanical properties of the sintered body are improved. The densities of the surface layer and the interior of the sintered body can be confirmed by SEM observation of a cross-section of the sintered body. Specifically, firstly, SEM observation is performed on a region of 0-1% in the thickness direction (hereinafter also referred to as the "surface region") as the surface layer, and SEM observation is performed on a region of 40-50% in the thickness direction (hereinafter also referred to as the "interior region") as the interior of the sintered body. Next, image analysis is performed on the surface region and the interior region respectively using common image analysis software (e.g., Image-Pro10, manufactured by H.O.T. Co., Ltd.), and the porosity and its area are detected. The porosity can be determined from the SEM observation. Figure 2 Detection in the value-enhanced image. As a result of image analysis, based on the area [μm] of the portion excluding the pore. 2 ] Observation area relative to the SEM image [μm 2The area density [%] of each region can be calculated using the following formula.

[0039] Area density [%] = {(area excluding pores) / (observed area of ​​SEM image)} × 100%

[0040] In the sintered body of this embodiment, the area density of the surface layer is higher than the area density of the interior of the sintered body. For example, it is preferable that the area density of the surface layer is higher than the area density of the interior of the sintered body. The area density difference (=(area density of the surface region) - (area density of the interior region)) is preferably 10% or more, 15% or more, or 20% or more. Alternatively, it can be 30% or less or 25% or less. The upper and lower limits of the area density difference of the sintered body can be any combination of the above, for example, 10% or more and 30% or less, or 20% or more and 25% or less.

[0041] Furthermore, regarding the density inside the sintered body, as an area density, examples include less than 90%, less than 80%, less than 70%, less than 65%, less than 60%, or less than 58%. Alternatively, examples include more than 50% or more than 55%. The upper and lower limits of the area density inside the sintered body can be any combination of the above, for example, more than 50% and less than 90%, more than 50% and less than 65%, or more than 55% and less than 60%.

[0042] In this embodiment, the thickness of the surface layer is arbitrary, for example, 10 μm or more, 20 μm or more, or 50 μm or more. Alternatively, thicknesses of 500 μm or less, 300 μm or less, 200 μm or less, 150 μm or less, 120 μm or less, 100 μm or less, or 80 μm or less can be used. For example, thicknesses of 10 μm or more and 500 μm or less, 10 μm or more and 100 μm or less, or 20 μm or more and 80 μm or less can be used. The thickness of the surface layer is measured as the length from the outermost surface to the changing region in a SEM image of the cross-section of the sintered body in this embodiment. Based on this SEM image, the thickness is measured at 5 points at equal intervals in a direction perpendicular to the thickness direction in 5 or more fields of view, preferably 10 ± 2 fields of view, and the average value is calculated.

[0043] The preferred bulk density of the sintered body in this embodiment is 3.80 g / cm³. 3 Above and 5.50 g / cm 3 The following is a preferred bulk density: 3.80 g / cm³. 3 Above, 4.00 g / cm 3 Above or 4.20 g / cm 3That's all. With such a bulk density, the sintered body of this embodiment easily possesses sufficient strength when used as a sputtering target. A higher bulk density is preferred; for example, 5.00 g / cm³ is an example. 3 Below, 4.80g / cm 3 Below or 4.70 g / cm 3 The upper and lower limits of the bulk density of the sintered body can be any combination of the above, for example, 3.80 g / cm³. 3 Above and 5.00 g / cm 3 Below, or 4.20 g / cm 3 Above and 4.70 g / cm 3 the following.

[0044] In this embodiment, "density" is the bulk density determined according to the method of JIS R1634, and the pretreatment can be performed by vacuum method using distilled water.

[0045] In the sintered body of this embodiment, the atomic weight ratio of gallium to the sum of gallium and nitrogen ([mol / mol]; hereinafter also referred to as "Ga / (Ga+N)") is greater than 0.5 and less than 0.60. By keeping Ga / (Ga+N) within this range, the dissolution of metallic gallium can be suppressed, and re-oxidation can also be suppressed. Since there is a tendency for further re-oxidation to be less likely, Ga / (Ga+N) is preferably 0.51 or more, 0.52 or more, or 0.53 or more, and preferably 0.58 or less, 0.57 or less, 0.56 or less, 0.55 or less, or 0.54 or less. The upper and lower limits of Ga / (Ga+N) of the sintered body can be any combination of the above, for example, more than 0.5 and less than 0.58, more than 0.51 and less than 0.56, more than 0.52 and less than 0.55, or more than 0.53 and less than 0.54.

[0046] The oxygen content of the sintered body in this embodiment is preferably 0.3 atm% or less, more preferably 0.2 atm% or less, and even more preferably 0.1 atm% or less. The sintered body in this embodiment is preferably oxygen-free (i.e., oxygen content is 0 atm%), and examples include oxygen content of 0 atm% or more, more than 0 atm%, or 0.01 atm% or more. With such an oxygen content, the film obtained by sputtering it tends to exhibit characteristics more suitable for applications such as light-emitting diodes and power devices. The upper and lower limits of the oxygen content of the sintered body can be any combination of the above, for example, 0 atm% or more and 0.3 atm% or less. Examples include 0 atm% or more and 0.2 atm% or less, more than 0 atm% and 0.2 atm% or less, or 0.01 atm% or more and 0.1 atm% or less.

[0047] The composition of the sintered body in this embodiment can be considered as represented by the following formula.

[0048] 100 = W Ga [Quality%] + W O [Quality%] + W N [Quality%] + W X [mass%] (1)

[0049] (1) In the formula, W Ga W O W N and W X These represent the mass percentages of gallium, oxygen, nitrogen, and dopant elements in the sintered body, respectively. W O and W N The value was determined by thermal decomposition of gallium nitride sintered bodies using a conventional oxygen and nitrogen analysis device (such as the LECO ON736, manufactured by Leco). Additionally, W... X The value was determined by glow discharge mass spectrometry analysis. W Ga It is based on W O W N and W X The measured value is obtained by formula (1).

[0050] The oxygen content is calculated using the following equation (2).

[0051] Oxygen content [atm%] =

[0052] (W) O / M O ) / {(W Ga / M Ga )+(W N / M N )+(W O / M O )+(W X / M X )} (2)

[0053] (2) In the formula, M O The atomic weight of oxygen is 16.00 [g / mol], M Ga The atomic weight of gallium is 69.72 [g / mol], and M... N The atomic weight of nitrogen is 14.01 g / mol. Additionally, M... X It is the atomic weight of the doping element. For example, the atomic weight of silicon is 28.09 g / mol, the atomic weight of magnesium is 24.31 g / mol, the atomic weight of aluminum is 26.98 g / mol, and the atomic weight of indium is 114.82 g / mol.

[0054] Ga / (Ga+N) is the value obtained according to the following equation (3).

[0055] Ga / (Ga+N)=(W Ga / M Ga ) / {(W Ga / M Ga )+(W N / M N )}(3)

[0056] The sintered body of this embodiment can be used for known applications of gallium nitride sintered bodies, but it is particularly preferred to manufacture a sintered body for sputtering targets.

[0057] Next, the method for manufacturing the sintered body according to this embodiment will be described.

[0058] The manufacturing method of the sintered body in this embodiment is arbitrary as long as it has the above-described characteristics. As a preferred manufacturing method, one can exemplify a method comprising the following steps: reacting a nitrogen-containing compound gas with a bulk gallium nitride at a reaction temperature of 1025°C or lower under a nitrogen-containing compound gas flow atmosphere of 0.5 L / min or higher. Reacting gallium nitride sintered bodies with nitrogen-containing compound gases has been studied. However, in this embodiment, it has been found that the flow rate of the nitrogen-containing compound gas affects the reaction state with the gallium nitride sintered body. Therefore, by controlling the flow rate of the nitrogen-containing compound gas, the surface reaction of the bulk body can be promoted, and the sintered body of this embodiment can be easily obtained. In this embodiment, "bulk body" refers to an object that is not amorphous but has a certain shape, such as powder or liquid; examples include sintered bodies and molded bodies.

[0059] In a process (hereinafter also referred to as "densification process") in which a nitrogen-containing compound gas is reacted with a bulk gallium nitride in an atmosphere of flow of nitrogen-containing compound gas at a flow rate of 0.5 L / min or higher, the metallic gallium present on the surface of the gallium nitride sintered body is effectively nitrided to form a dense layer of gallium nitride (surface layer).

[0060] The gallium nitride bulk (hereinafter also referred to as "bulk") supplied for the densification process is essentially a bulk composed of gallium nitride, but preferably contains metallic gallium as a trace component, preferably a gallium nitride bulk containing metallic gallium, and more preferably a gallium nitride bulk containing metallic gallium at least on the surface.

[0061] The bulk body is preferably a pre-sintered gallium nitride body containing metallic gallium, and more preferably a pre-sintered gallium nitride body containing metallic gallium at least on its surface. Such a sintered body can be any gallium nitride sintered body obtained by any manufacturing method, but is preferably a gallium nitride sintered body obtained by HIP (High-Intensity Interval) or HP (High-Performance Interval) processing, and more preferably a gallium nitride sintered body obtained by HP processing. Gallium nitride sintered bodies obtained by HP processing readily contain metallic gallium on their surface.

[0062] Furthermore, the bulk body is preferably a shaped gallium nitride body containing metallic gallium, and more preferably a shaped gallium nitride body containing metallic gallium at least on its surface. Shaped gallium nitride bodies obtained through molding processes readily contain metallic gallium on their surface.

[0063] Additionally, the Ga / (Ga+N) of a block can be greater than 0.50 or greater than 0.55. The Ga / (Ga+N) of a block can be less than 0.60 or less than 0.58. The upper and lower limits of the Ga / (Ga+N) of a block can be any combination of the above, for example, greater than 0.50 and less than 0.60, greater than 0.50 and less than 0.58, or greater than 0.55 and less than 0.58.

[0064] The bulk material preferably contains gallium at least on its surface. By including gallium on the surface, the surface can be easily densified using a densification process, where the gallium present on the surface is nitrided. In this embodiment, the presence of gallium in the bulk material can be confirmed simply by the presence of Ga (metal) XRD peaks in its surface XRD pattern.

[0065] The bulk material is preferably gallium oxide-free. In this embodiment, "gallium oxide-free" means that it does not have gallium oxide powder X-ray diffraction peaks in its powder X-ray diffraction pattern. The bulk material may contain gallium oxide to the extent that no gallium oxide powder X-ray diffraction peaks are identified in its powder X-ray diffraction pattern. No gallium oxide powder X-ray diffraction peaks are identified when the ratio of the peak intensity of the gallium oxide (002) plane to the peak intensity of the gallium nitride (002) plane is less than 1%.

[0066] The oxygen content of the bulk material is preferably 0.3 atm% or less, 0.2 atm% or less, or 0.1 atm% or less. This easily suppresses the formation of pores caused by oxygen loss during the densification process, and the resulting increase in surface roughness. A low oxygen content in the bulk material is preferred, but examples include 0 atm% or more. Any combination of the above-mentioned upper and lower limits of the oxygen content in the bulk material is acceptable.

[0067] The bulk density of the bulk material is preferably 3.50 g / cm³. 3 Above or 4.00 g / cm 3 The above. If the bulk density of the block is 3.50 g / cm³.3 The above process, through densification, yields a gallium nitride sintered body with practical mechanical strength. A high bulk density is preferred, for example, 5.00 g / cm³. 3 Below or 4.80g / cm 3 The upper and lower limits of the bulk density of the mass can be any combination of the above.

[0068] In the densification process, the nitrogen-containing compound gas is reacted with the gallium nitride bulk at a reaction temperature of 1025°C or lower under a nitrogen-containing compound gas flow atmosphere of 0.5 L / min or higher. Under a nitrogen-containing compound gas flow atmosphere of less than 0.5 L / min, the reaction between metallic gallium and the nitrogen-containing compound gas will not proceed sufficiently, and even if the reaction does occur, gallium nitride of a degree sufficient to densify the surface of the bulk will not form. The flow rate of the nitrogen-containing compound gas is 0.5 L / min or higher, preferably 1.0 L / min or higher or 2.0 L / min or higher. The flow rate of the nitrogen-containing compound gas does not need to be increased to a necessary level; 10.0 L / min or lower, 8.0 L / min or lower, or 7.0 L / min or lower are sufficient. The flow rate of the nitrogen-containing compound gas can be any combination of the above, such as 0.5 L / min or more and 10.0 L / min or less, 1.0 L / min or more and 8.0 L / min or less, 2.0 L / min or more and 7.0 L / min or less, or 2.0 L / min or more and 4.0 L / min or less.

[0069] In this embodiment, "nitrogen-containing compound gas" is a gas containing a compound whose structure includes nitrogen atoms, and preferably a gas containing a nitrogen-containing compound that reacts with the bulk. Specific examples of nitrogen-containing compound gases include one or more gases selected from the group consisting of ammonia, hydrazine, and alkylamines, and more specifically, ammonia.

[0070] In the densification process, the nitrogen-containing gas is reacted with the bulk material under a flowing atmosphere of nitrogen-containing gas at a reaction temperature below 1025°C. The reaction can be carried out under conditions where the nitrogen-containing gas contacts the bulk material and promotes its nitriding; one or more types selected from the group consisting of a firing furnace, a tubular furnace, and an atmosphere furnace can be used, with an atmosphere furnace being preferred. Furthermore, the reaction can be carried out under a flowing atmosphere of nitrogen-containing gas, and furthermore, it can be carried out under either a pressurized atmosphere or an atmospheric pressure atmosphere; for simplicity, an atmospheric pressure atmosphere is preferred.

[0071] The reaction temperature is 1025°C or below. If the reaction temperature exceeds 1025°C, nitriding of the sintered body surface occurs rapidly in the densification process atmosphere of this embodiment, resulting in defects such as surface peeling. As a result, in addition to low density, it is also prone to re-oxidation after sintering. The reaction temperature is preferably 1020°C or below, more preferably 1000°C or below, and even more preferably 990°C or below. The reaction temperature can be any temperature at which the reaction between the nitrogen-containing compound gas and the bulk material takes place; if it is 900°C or above or 950°C or above, the reaction proceeds efficiently. The upper and lower limits of the reaction temperature can be any combination of the above, for example, 900°C or above and 1020°C, 900°C or above and 1000°C, or 950°C or above and 1000°C.

[0072] The heating rate up to the reaction temperature is arbitrary, for example, it can be above 100°C / hour and below 400°C / hour.

[0073] The processing time (hereinafter also referred to as "holding time") of the nitrogen-containing compound gas and the bulk material at the reaction temperature can be arbitrarily set according to the amount and size of the bulk material supplied to the reaction and the performance of the reactor used in the reaction. Examples of holding time at the above reaction temperature are 0.5 hours or more, 1 hour or more, 10 hours or less, or 5 hours or less. The upper and lower limits of the processing time can be any combination of the above, for example, 0.5 hours or more and 10 hours or more and 5 hours or less.

[0074] The manufacturing method of this embodiment may include a process for processing the sintered body after the densification process (hereinafter also referred to as the "processing process").

[0075] The processing step is a process of shaping the gallium nitride sintered body into a shape appropriate for the desired application. For example, when using the sintered body of this embodiment as a sputtering target, it can be processed using one or more processing methods selected from surface grinding, rotary grinding, and cylindrical grinding. Additionally, during the processing step, the sintered body can also be bonded to a backing plate.

[0076] Next, the sputtering target containing the sintered body of this embodiment will be described.

[0077] The sputtering target containing the sintered body of this embodiment (hereinafter also referred to as "the target of this embodiment") is a sputtering target formed by bonding the sintered body of this embodiment to a support body via a bonding layer.

[0078] The shape of the target in this embodiment is arbitrary, and can be exemplified by at least one of the flat and cylindrical shapes, or other shapes suitable for the application.

[0079] In this embodiment, the target bonds the sintered body of this embodiment to the support via a bonding layer. The bonding layer may be composed of a solder containing one or more elements selected from the group consisting of tin, indium, and zinc. Since the electrical and thermal conductivity of the target is easily increased, the bonding layer is preferably composed of an indium-containing solder. It should be noted that when the bonding layer is an indium-containing solder, the target of this embodiment may have a layer (hereinafter also referred to as a "barrier layer") between the gallium nitride sintered body and the bonding layer to improve wettability. This improves the indium wettability of the gallium nitride sintered body, resulting in a stronger bond between the gallium nitride sintered body and the bonding layer. The barrier layer may be composed of a component with high indium wettability, preferably at least one of nickel and chromium.

[0080] On the other hand, due to the increased cost, the target in this embodiment preferably does not have a layer containing tungsten (W), and it is particularly preferred that it does not have a layer containing tungsten as a barrier layer.

[0081] In this embodiment, the support in the target is preferably selected from one or more materials chosen from the group consisting of copper, stainless steel, and titanium. Furthermore, the shape of the support can be any desired shape corresponding to the shape of the sintered body in this embodiment; examples include at least one shape chosen from flat plates and cylindrical shapes, or other shapes suitable for the application.

[0082] Example

[0083] The present disclosure will now be described through examples. However, the present disclosure is not limited to these examples.

[0084] (composition)

[0085] Using an oxygen / nitrogen analyzer (LECO ON736, manufactured by Leco), the oxygen [mass%] and nitrogen [mass%] content of the gallium nitride sinter were determined by inactive gas melting-infrared absorption method. Based on the obtained oxygen and nitrogen mass ratios, the mass ratio of gallium was calculated using equation (1) above, the oxygen content [atm%] was calculated using equation (2) above, and Ga / (Ga+N) was calculated using equation (3) above.

[0086] (bulk density)

[0087] The bulk density of the gallium nitride sintered body was determined according to the method in JIS R1634. Pretreatment was performed using a vacuum method with distilled water.

[0088] (density)

[0089] As the density of the surface layer and the interior of the sintered body, the cross-section of the sintered body was observed using SEM, and the areal density of each was determined from the obtained SEM images. Specifically, the cross-section observation involved embedding the sintered body in resin, cutting it, and grinding it until the surface roughness Ra ≤ 1.0 μm, thereby exposing the cross-section. This cross-section was observed using an SEM (device name: VE-9800, manufactured by KEYENCE). The SEM observation conditions are as follows.

[0090] Accelerating voltage: 10kV

[0091] Magnification: (Surface area) 100x, (Internal area) 500x

[0092] Field of view: 10 fields of view

[0093] In the SEM images of the cross-section, the area from the surface of the sintered body in the thickness direction of 0-1% is considered the surface region, and the area in the thickness direction of 40-50% is considered the internal region. The area density is calculated from the image analysis of each SEM image. That is, image analysis software (Image-Pro10, manufactured by Berton) is used to analyze the SEM images of the cross-section. Figure 2 Value-based analysis distinguishes between pores and other structures (i.e., grains constituting the sintered body), thereby detecting pores and determining their area [μm]. 2 After detection, the area [μm] of the region excluding the pore is used as the basis for the analysis. 2 The observation area [μm] relative to the SEM image 2 The area density [%] of the surface region and the interior region can be calculated using the following formula.

[0094] Area density [%] = {(Area of ​​the region excluding pores) / (Observed area of ​​the SEM image)} × 100%

[0095] For a single test sample, SEM images of cross-sections from 10 fields of view are analyzed, and their average value is used as the area density of each test sample.

[0096] (Thickness of the surface layer)

[0097] In SEM images of cross-sections obtained using the same method as for the surface layer's area density, regions where density changes within the surface layer are considered variable regions, and the area from the surface to the variable region is considered the surface layer itself, and its thickness is measured. This measurement is performed on 10 fields of view, and the average value is taken as the surface layer thickness.

[0098] (Vickers hardness)

[0099] The Vickers hardness of sintered bodies was determined using a method based on JIS Z2244. Five measurements were taken from a single test specimen, and the average value was taken as the Vickers hardness.

[0100] (Determination of flexural strength)

[0101] The three-point flexural strength of the sintered body was determined according to the method of JIS R1601. The test was performed twice, and the average value was taken as the flexural strength.

[0102] Example 1

[0103] 50 g of gallium nitride powder (4N purity; 99.99%) was filled into a cylindrical carbon container with a diameter of 53 mm. The carbon container was placed in a hot press and heated to 1000 °C at a rate of 200 °C / h, and then hot-pressed at a treatment temperature of 1070 °C and a treatment pressure of 40 MPa for 2 hours. After hot pressing, the container was cooled to approximately 50 °C over 5 hours, and the gallium nitride sintered body was recovered. The gallium nitride sintered body was then machined to form a 2-inch diameter, 3.8 mm thick circular plate-shaped gallium nitride sintered body, which was used as a pre-sintered body. The bulk density of the pre-sintered body was 4.47 g / cm³. 3 XRD peaks of metallic Ga were confirmed in the XRD pattern.

[0104] The pre-sintered body was placed in an atmosphere furnace (product name: MS-4272, manufactured by Motoyama Corporation) and heat-treated under the following conditions to obtain the sintered body of this embodiment.

[0105] Heat treatment atmosphere: Ammonia flow atmosphere (ammonia flow rate: 2L / min)

[0106] Heating rate: 200℃ / hour

[0107] Temperature maintained: 980℃

[0108] Duration: 1 hour

[0109] Cooling rate: 200℃ / hour

[0110] Example 2

[0111] Except for setting the ammonia flow rate to 4 L / min, the sintered body of this embodiment was obtained using the same method as in Example 1.

[0112] Example 3

[0113] Except for setting the ammonia flow rate to 6 L / min, the sintered body of this embodiment was obtained using the same method as in Example 1.

[0114] Example 4

[0115] Except for setting the holding time at 980°C to 5 hours, the sintered body of this embodiment was obtained using the same method as in Example 1.

[0116] Example 5

[0117] Except for setting the holding time at 980°C to 10 hours, the sintered body of this embodiment was obtained using the same method as in Example 1.

[0118] Example 6

[0119] Prepare 8g of a mixed powder of metallic gallium and gallium nitride with a Ga / (Ga+N) ratio of 0.59, and fill it into a rectangular mold measuring 10mm x 40mm. After filling, uniaxially press the powder under a pressure of 100MPa to obtain a molded body. Perform cold isostatic pressing on the molded body under a pressure of 300MPa to produce a CIP-treated body. Place the CIP-treated body (powder-pressed body) on an alumina sintering plate and sinter it in an atmosphere furnace under the following conditions to obtain the sintered body of this embodiment.

[0120] Heat treatment atmosphere: Ammonia flow atmosphere (ammonia flow rate 2L / min)

[0121] Heating rate: 200℃ / hour

[0122] Temperature maintained: 950℃

[0123] Duration: 5 hours

[0124] Cooling rate: 200℃ / hour

[0125] Comparative Example 1

[0126] The gallium nitride sintered body obtained by the same method as the pre-sintered body used in Example 1 was used as the sintered body of this comparative example.

[0127] Comparative Example 2

[0128] Except for maintaining the temperature at 1030°C, the sintered body of this comparative example was obtained using the same method as in Example 1.

[0129] The manufacturing conditions for the examples and comparative examples are shown in Table 1, and the evaluation results are shown in Table 2.

[0130] [Table 1]

[0131]

[0132] [Table 2]

[0133]

[0134] As can be confirmed from the table above, in the embodiments, the area density of the surface region is higher than that of the internal region, resulting in a surface layer with a higher density than the interior of the sintered body. On the other hand, it can be confirmed that in Comparative Example 1, which did not undergo a densification process, the area densities of the surface region and the internal region are equal, resulting in the absence of a surface layer and a higher oxygen content. Furthermore, although Comparative Example 2 was processed using the same pre-sintered body as the embodiments, Ga / (Ga+N) was less than 0.5, and the oxygen content was high, confirming that it was easily re-oxidized. Thus, it can be confirmed that the increase in oxygen content of the sintered body in the embodiments was suppressed.

[0135] In addition, through densification treatment, Example 2 achieved a density of 0.07 g / cm³. 3 Example 3: 0.08 g / cm³ 3 Example 4 showed a concentration of 0.09 g / cm³. 3 The bulk density increased. This confirms that the densification treatment in the examples tends to increase the bulk density of the sintered body.

[0136] Test Example

[0137] The Vickers hardness and flexural strength of the sintered bodies of the Examples and Comparative Examples were measured. The measurements were performed separately for each sintered body (hereinafter also referred to as "unprocessed sintered body") and for sintered bodies whose surface layer had been removed by grinding (hereinafter also referred to as "processed sintered body"). It should be noted that Comparative Example 1 did not have a surface layer, therefore the aforementioned processing was not performed, and the flexural strength, etc., were measured. The results are shown in the table below.

[0138] [Table 3]

[0139]

[0140] As can be confirmed from the table above, the Vickers hardness and flexural strength of the sintered bodies in the embodiments are improved due to the presence of the surface layer. Furthermore, for the sintered bodies of Comparative Example 2, the Vickers hardness and flexural strength of the unprocessed sintered body are higher than those of the processed sintered body, but the increase is smaller. Therefore, it is considered that the surface layer was not sufficiently formed in the manufacturing method of Comparative Example 2.

[0141] The entire contents of the description, claims, drawings and abstract of Japanese Patent Application No. 2022-049235, filed on March 25, 2022, are incorporated herein by reference and are included as a disclosure of this disclosure.

Claims

1. A gallium nitride sintered body having a surface layer with a higher density than the interior of the sintered body, wherein the atomic weight ratio of gallium to the sum of gallium and nitrogen in the sintered body is greater than 0.5 and less than 0.60; The thickness of the surface layer is more than 10 μm and less than 500 μm; The area density difference of the sintered body is more than 10% and less than 30%, and the area density difference = the area density of the surface region - the area density of the internal region; The surface region is the region that accounts for 0 to 1% of the thickness of the sintered body, and the internal region is the region that accounts for 40 to 50% of the thickness of the sintered body. The oxygen content of the sintered body is below 0.2 atm%. The area density [%] = {(area excluding pores) / (observed area of ​​SEM image)} × 100%.

2. The sintered body according to claim 1, wherein, The atomic weight ratio of gallium to the sum of gallium and nitrogen is greater than 0.5 and less than 0.

58.

3. The sintered body according to claim 1 or 2 has a measured density of 3.80 g / cm³. 3 Above and 5.50 g / cm 3 the following.

4. The sintered body according to claim 1 or 2, comprising metallic gallium.

5. A method for manufacturing a sintered body according to any one of claims 1 to 4, comprising the following steps: In an atmosphere of nitrogen-containing compound gas flow of 0.5 L / min or higher, the nitrogen-containing compound gas is reacted with a bulk gallium nitride at a reaction temperature of 1025 °C or lower, the bulk containing at least metallic gallium on its surface.

6. The manufacturing method according to claim 5, wherein, The bulk material is a pre-sintered gallium nitride body.

7. The manufacturing method according to claim 5, wherein, The atomic weight ratio of gallium to the sum of gallium and nitrogen in the bulk is greater than 0.50 and less than 0.

60.

8. The manufacturing method according to claim 5, wherein, The block is a shaped form of gallium nitride.

9. The manufacturing method according to any one of claims 5 to 8, wherein, The oxygen content of the block is below 0.3 atm%.

10. The manufacturing method according to claim 5, wherein, The nitrogen-containing compound gas is one or more gases selected from the group consisting of ammonia, hydrazine, and alkylamines.

11. A sputtering target comprising the sintered body according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Gallium nitride sintered body or gallium nitride molded article, and method for producing them

    JP2012144424A

  • Gallium nitride-based sintered body and manufacturing method therefor

    JP2017024970A

  • Gallium nitride particle and manufacturing method thereof

    JP2019001681A

  • Dielectric thin film element and electronic circuit device

    JP2022049235A

  • Gallium nitride sintered article of gallium nitride molded article and method for producing these articles

    CN103270000A