Heterophasic propylene copolymer composition
By using a heterogeneous propylene copolymer composition with significant melt flow index differences, elastomer and inorganic filler, the shortcomings of injection molded products in terms of puncture impact toughness and processability are solved, and a combination of high performance and convenient processing is achieved. .
Patent Information
- Application Number
- CN202380027116.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-06
- Publication Date
- 2024-11-08
AI Technical Summary
The existing multiphase propylene copolymer injection molded products have shortcomings in puncture impact toughness and processability, and it is difficult to meet good performance and processing convenience at the same time.
The first and second heterophase propylene copolymer compositions with significant melt flow index differences are used, consisting of a propylene matrix and a dispersed ethylene-α-olefin copolymer, respectively, and an elastomer and an inorganic filler are added during the injection molding process. , the performance of the product is improved by adjusting the component ratio and the catalyst system.
It realizes good puncture impact toughness and processability of injection molded products, provides greater flexibility and energy saving, while ensuring high performance of products.
Smart Images

Figure BDA0005039603180000191 
Figure BDA0005039603180000201 
Figure BDA0005039603180000211
Abstract
Description
Technical Field
[0001] The present invention relates to a composition comprising a heterophasic propylene copolymer and a process for preparing the composition. The present invention further relates to a kit of parts for making the composition. The present invention further relates to an injection molded article comprising the composition and an injection molding process. The present invention further relates to a masterbatch and its use in an injection molding process. Background Art
[0002] Injection molded articles made from compositions based on heterophasic propylene copolymers are used for various applications. It is known to add various components such as elastomers and fillers to heterophasic propylene copolymers to obtain injection molded articles with different properties. Injection molded articles are typically made by melt mixing the heterophasic propylene copolymer with additional components to obtain pellets and feeding these pellets to an injection molding machine.
[0003] There is a need for a composition having good puncture impact toughness of the injection-molded articles according to the invention and good processability during injection molding. Summary of the invention
[0004] Accordingly, the present invention provides a composition comprising a first heterophasic propylene copolymer having a first melt flow index MFI1 measured at 230 °C using 2.16 kg according to ISO 1133-1:2011, an elastomer, an inorganic filler, additives including stabilizers and a second heterophasic propylene copolymer having a second melt flow index MFI2 measured at 230 °C using 2.16 kg according to ISO 1133-1:2011, wherein the composition has a melt flow index measured at 230 °C using 2.16 kg according to ISO 1133-1:2011 of at least 12.0 dg / min, and wherein the ratio of MFI1 to MFI2 or the ratio of MFI2 to MFI1 is at least 5.8, more preferably at least 5.9, more preferably at least 6.0,
[0005] wherein the first heterophasic propylene copolymer consists of: (ia) a propylene based matrix, wherein the propylene based matrix consists of a propylene homopolymer and / or a propylene copolymer consisting of at least 90 wt.-% propylene monomer units and at most 10 wt.-% ethylene and / or α-olefin monomer units, based on the total weight of the propylene based matrix, and (ib) a dispersed ethylene-α-olefin copolymer, wherein the total amount of the propylene based matrix in the heterophasic propylene copolymer and the total amount of the dispersed ethylene-α-olefin copolymer sums to 100 wt.-%, and
[0006] wherein the second heterophasic propylene copolymer consists of: (iia) a propylene based matrix, wherein the propylene based matrix consists of a propylene homopolymer and / or a propylene copolymer consisting of at least 90 wt% propylene monomer units and at most 10 wt% ethylene and / or α-olefin monomer units, based on the total weight of the propylene based matrix, and (iib) a dispersed ethylene-α-olefin copolymer, wherein the total amount of the propylene based matrix in the heterophasic propylene copolymer and the total amount of the dispersed ethylene-α-olefin copolymer is 100 wt%,
[0007] wherein the first heterophasic propylene copolymer is HECO-A and the second heterophasic propylene copolymer is HECO-B or the first heterophasic propylene copolymer is HECO-B and the second heterophasic propylene copolymer is HECO-A,
[0008] wherein HECO-A has a melt flow rate measured at 230°C using 2.16 kg according to ISO 1133-1:2011 of greater than 25 to 120 dg / min, the amount of ethylene-α-olefin copolymer in HECO-A is 10 to 40 wt%, and
[0009] HECO-B has a melt flow rate of 1.0 to 25 dg / min, measured at 230° C. using 2.16 kg according to ISO 1133-1:2011, and the amount of the ethylene-α-olefin copolymer in HECO-B is 20 to 50% by weight.
[0010] The present invention provides a composition comprising a first heterophasic propylene copolymer and a second heterophasic propylene copolymer having a relatively large difference in MFI. Such a high ratio has been found to result in good puncture impact toughness and a desired MFI of the injection molded article according to the present invention as well as good processability during injection molding.
[0011] Relative to the total amount
[0012] Preferably the amount of the first heterophasic propylene copolymer is from 10 to 50 wt%, more preferably from 20 to 40 wt%, based on the composition.
[0013] Preferably, the amount of elastomer is from 5.0 to 20% by weight, more preferably from 8.0 to 12% by weight relative to the composition.
[0014] Preferably, the amount of the inorganic filler is 5.0 to 30 wt %, more preferably 8.0 to 22 wt %, more preferably 8.0 to 17 wt %, relative to the composition.
[0015] Preferably, the amount of the additive is 0.01 to 5.0% by weight, more preferably 0.1 to 3.0% by weight, relative to the composition.
[0016] Preferably, the amount of the stabilizer is 0.01 to 1.0% by weight, more preferably 0.1 to 2.0% by weight, based on the composition.
[0017] Preferably, the amount of the second multiphase propylene copolymer is 30 to 80% by weight, more preferably 40 to 70% by weight, based on the composition.
[0018] Preferably, the total amount of the first multiphase propylene copolymer, the elastomer, the inorganic filler, the additive, and the second multiphase propylene copolymer is at least 95% by weight, at least 98% by weight, at least 99% by weight, or 100% by weight, based on the composition.
[0019] First and second heterophasic propylene copolymers
[0020] The first multiphase propylene copolymer has a first melt flow index MFI1 measured at 230 °C using 2.16 kg in accordance with ISO 1133-1:2011, and the second multiphase propylene copolymer has a second melt flow index MFI2 measured at 230 °C using 2.16 kg in accordance with ISO 1133-1:2011. MFI1 is different from MFI2.
[0021] The ratio of MFI1 to MFI2 or the ratio of MFI2 to MFI1 is at least 5.8, more preferably at least 5.9, and even more preferably at least 6.0.
[0022] The first multiphase propylene copolymer has a first Charpy impact strength IS1 at 23 °C in accordance with ISO 179 / 1eA(II), and the second multiphase propylene copolymer has a second Charpy impact strength IS2 at 23 °C in accordance with ISO 179 / 1eA(II). IS1 and IS2 are typically different.
[0023] Preferably, the ratio of IS1 to IS2 or the ratio of IS2 to IS1 is at least 5.0, more preferably at least 6.0.
[0024] In some embodiments, MFI1 > MFI2 and IS1 < IS2. In some embodiments, the ratio of MFI1 to MFI2 is at least 5.8, more preferably at least 5.9, and even more preferably at least 6.0, and the ratio of IS2 to IS1 is at least 5.0, more preferably at least 6.0.
[0025] In some embodiments, MFI1 < MFI2 and IS1 > IS2. In some embodiments, the ratio of MFI2 to MFI1 is at least 5.8, more preferably at least 5.9, and even more preferably at least 6.0, and the ratio of IS1 to IS2 is at least 5.0, more preferably at least 6.0.
[0026] Heterophasic propylene copolymers are generally prepared in one or more reactors by polymerizing propylene in the presence of a catalyst and subsequently polymerizing an ethylene-α-olefin mixture. The resulting polymer material is heterophasic, but the specific morphology usually depends on the preparation method and the ratio of the monomers used.
[0027] The heterophasic propylene copolymers employed in the present invention can be produced using any conventional technology known to the skilled person, for example, multistage process polymerization, such as bulk polymerization, gas phase polymerization, slurry polymerization, solution polymerization or any combination thereof. Any conventional catalyst system can be used, for example, Ziegler-Natta or metallocene. Such techniques and catalysts are described, for example, in WO06 / 010414; Polypropylene and other Polyolefins, Ser van der Ven, Studies in Polymer Science 7, Elsevier, 1990; WO06 / 010414, US4399054 and US4472524.
[0028] Preferably, the heterophasic propylene copolymer is produced using a Ziegler-Natta catalyst.
[0029] The heterophasic propylene copolymer can be prepared by a process comprising the following steps:
[0030] - polymerizing propylene and optionally ethylene and / or α-olefins in the presence of a catalyst system to obtain a propylene-based substrate, and
[0031] - Subsequently polymerizing ethylene and α-olefins in a propylene-based matrix in the presence of a catalyst system to obtain dispersed ethylene-α-olefin copolymers. These steps are preferably carried out in different reactors. The catalyst systems of the first and second steps may be different or identical.
[0032] The heterophasic propylene copolymer of the composition of the present invention consists of a propylene-based matrix and a dispersed ethylene-α-olefin copolymer. The propylene-based matrix typically forms the continuous phase in the heterophasic propylene copolymer. The amount of the propylene-based matrix and the dispersed ethylene-α-olefin copolymer can be determined by 13 C-NMR determination, as is well known in the art.
[0033] In the heterophasic propylene copolymer in the composition of the present invention the sum of the total weight of the propylene based matrix and the total weight of the dispersed ethylene-α-olefin copolymer is 100 wt% of the heterophasic propylene copolymer.
[0034] The propylene-based matrix consists of a propylene homopolymer and / or a propylene copolymer consisting of at least 90 wt% of propylene monomer units and up to 10 wt% of comonomer units selected from ethylene monomer units and α-olefin monomer units having 4 to 10 carbon atoms, e.g. consisting of at least 95 wt% of propylene monomer units and up to 5 wt% of comonomer units, based on the total weight of the propylene-based matrix.
[0035] Preferably, the comonomer in the propylene copolymer of the propylene based matrix is selected from ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene, and is preferably ethylene.
[0036] Preferably, the propylene based matrix consists of a propylene homopolymer. The fact that the propylene based matrix consists of a propylene homopolymer is advantageous in that a higher stiffness is obtained compared to the case where the propylene based matrix is a propylene-α-olefin copolymer.
[0037] The α-olefin in the ethylene-α-olefin copolymer is preferably selected from α-olefins having 3 to 8 carbon atoms. Examples of suitable α-olefins having 3 to 8 carbon atoms include, but are not limited to, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene. More preferably, the α-olefin in the ethylene-α-olefin copolymer is selected from α-olefins having 3 to 4 carbon atoms and any mixture thereof, and the α-olefin is more preferably propylene, in which case the ethylene-α-olefin copolymer is an ethylene-propylene copolymer.
[0038] The heterophasic propylene copolymer can be obtained directly from the reactor(s), but can also be prepared by visbreaking an intermediate heterophasic propylene copolymer prepared in a sequential multi(stage)reactor polymerization process and having an initial melt flow rate (MFR 500 wt %) measured according to ISO 1133:2011 at 230°C using 2.16 kg i ), which is carried out by contacting the intermediate heterophasic propylene copolymer with a peroxide in a melt mixing process to form a copolymer having a melt flow rate (MFR) measured according to ISO 1133:2011 at 230°C using 2.16 kg HECO ) of a heterophasic propylene copolymer having a visbreaking ratio MFR HECO / MFR i In the range of 1.2 to 25.
[0039] Catalyst system
[0040] Ziegler-Natta catalyst systems are well known in the art. The term generally refers to a catalyst system comprising a solid catalyst compound containing a transition metal (primary catalyst) and an organometallic compound (co-catalyst). Optionally, one or more electron donor compounds (external donors) may also be added to the catalyst system.
[0041] The transition metal in the transition metal-containing solid catalyst compound is usually selected from Groups 4 to 6 of the Periodic Table of Elements (latest IUPAC notation); more preferably, the transition metal is selected from Group 4; most preferably, titanium (Ti) is used as the transition metal.
[0042] Although various transition metals can be applied, it is most preferred that titanium is concerned below. However, it is also applicable to the use of other transition metals different from Ti. The titanium-containing compound that can be used as the transition metal compound in the present invention is generally loaded on a carrier containing magnesium and / or containing inorganic oxides (such as silicon oxide or aluminum oxide) that is insoluble in hydrocarbons, and is generally combined with an internal electron donor compound. The solid catalyst compound containing the transition metal can be formed, for example, by reacting titanium halide (IV), an organic internal electron donor compound and a magnesium-containing and / or silicon-containing carrier. The solid catalyst compound containing the transition metal can be further processed or modified with other electron donors or Lewis acid species, and / or can be subjected to one or more washing procedures, as well known in the art.
[0043] Some examples of Ziegler-Natta (pro)catalysts which can be suitably used for the preparation of the heterophasic propylene copolymer (A) and methods for their preparation can be found in EP 1 273 595, EP 0 019 330, US 5,093,415, Example 2 of US 6,825,146, US 4,771 ,024 column 10, line 61 to column 11, line 9, WO 03 / 068828, US 4,866,022, WO 96 / 32426 A, Example 1 of WO 2007 / 134851 A1 and WO 2015 / 091983, all of which are hereby incorporated by reference.
[0044] The (pro)catalyst thus prepared can be used in the polymerization of heterophasic propylene copolymers using an external donor such as exemplified herein and a cocatalyst such as exemplified herein.
[0045] In one embodiment, the heterophasic propylene copolymer is made using a phthalate-free catalyst.
[0046] Because of the increasingly stringent government regulations on the maximum phthalate content of polymers, it is preferred to use so-called phthalate-free internal donors. In the context of the present invention, "substantially phthalate-free" or "phthalate-free" means having a phthalate content based on the total weight of the catalyst that is lower than, for example, 150ppm, alternatively lower than, for example, 100ppm, alternatively lower than, for example, 50ppm, alternatively, for example, lower than 20ppm, for example, 0ppm. The example of phthalates includes, but is not limited to, dialkyl phthalates, wherein the alkyl group contains from about two to about ten carbon atoms. The example of phthalates includes, but is not limited to, diisobutyl phthalate, ethylbutyl phthalate, diethyl phthalate, di-n-butyl phthalate, bis(2-ethylhexyl)phthalate and diisodecyl phthalate.
[0047] Examples of phthalate-free internal donors include, but are not limited to, 1,3-diethers, such as 9,9-bis(methoxymethyl)fluorene, optionally substituted malonates, maleates, succinates, glutarates, benzoates, cyclohexene-1,2-dicarboxylate, benzoates, citraconates, aminobenzoates, silyl esters, and derivatives and / or mixtures thereof.
[0048] The catalyst system comprising the Ziegler-Natta procatalyst may be activated with an activator, for example an activator selected from benzamides and monoesters, such as alkyl benzoates.
[0049] Catalyst system includes cocatalyst. " Cocatalyst " used herein is a term well known in the art in the field of Ziegler-Natta catalysts, and is considered to be a material capable of converting a primary catalyst into an active polymerization catalyst. Generally speaking, a cocatalyst is an organometallic compound of a metal of the 1st, 2nd, 12th or 13th family containing the periodic system (Handbook of Chemistry and Physics, 70th edition, CRC Press, 1989-1990). Cocatalyst can include any compound known in the art to be used as "cocatalyst", such as hydride, alkylate or arylate of aluminum, lithium, zinc, tin, cadmium, beryllium, magnesium and their combination. Cocatalyst can be a hydrocarbyl aluminum cocatalyst, as known to technicians. Preferably, the cocatalyst is selected from trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, trihexyl aluminum, diisobutyl aluminum hydride, trioctyl aluminum, dihexyl aluminum hydride and their mixture, and most preferably, the cocatalyst is triethyl aluminum (abbreviated as TEAL).
[0050] Examples of external donors are known to those skilled in the art and include, but are not limited to, external electron donors selected from the group consisting of compounds having a structure according to formula III (R 90 )2N-Si(OR 91)3, having a structure according to formula IV (R 92 )Si(OR 93 )3, and mixtures thereof, wherein R 90 , R 91 , R 92 and R 93 Each of the groups is independently a linear, branched or cyclic substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, preferably wherein R 90 , R 91 , R 92 and R 93 The groups are each independently a straight-chain unsubstituted alkyl group having 1 to 8 carbon atoms, such as ethyl, methyl or n-propyl, such as diethylaminotriethoxysilane (DEATES), n-propyltriethoxysilane (nPTES), n-propyltrimethoxysilane (nPTMS); and alkyl groups having the general formula Si(OR a ) 4-n R b n An organosilicon compound, wherein n may be 0 to 2, and R a and R b Each of independently represents an alkyl or aryl group, optionally containing one or more heteroatoms such as O, N, S or P, having, for example, 1-20 carbon atoms; such as diisobutyldimethoxysilane (DiBDMS), tert-butylisopropyldimethoxysilane (tBuPDMS), cyclohexylmethyldimethoxysilane (CHMDMS), dicyclopentyldimethoxysilane (DCPDMS) or diisopropyldimethoxysilane (DiPDMS). More preferably, the external electron donor is selected from diisopropyldimethoxysilane (DiPDMS) or diisobutyldimethoxysilane (DiBDMS).
[0051] Preferably the heterophasic propylene copolymer is produced in a sequential multi-reactor polymerization process, e.g. in a gas phase process, in the presence of:
[0052] a) a Ziegler-Natta procatalyst comprising a compound of a transition metal of Group 4 to 6 of IUPAC, a Group 2 metal compound and an internal donor, wherein the internal donor is preferably a non-phthalic compound, more preferably a non-phthalate ester, even more preferably wherein the internal donor is selected from 1,3-diethers, such as 9,9-bis(methoxymethyl)fluorene, optionally substituted malonates, maleates, succinates, glutarates, benzoates, cyclohexene-1,2-dicarboxylates, benzoates, citraconates, aminobenzoates, silyl esters and derivatives and / or mixtures thereof;
[0053] b) a promoter (Co), and
[0054] c) Optional external donor.
[0055] CRYSTEX Method
[0056] The CRYSTEX method described in WO2019179959 and hereinafter allows the determination of the following properties of heterophasic propylene copolymers:
[0057] - ethylene content in the heterophasic propylene copolymer (TC2 overall);
[0058] - the intrinsic viscosity (IV overall) of the heterophasic propylene copolymer;
[0059] - amount of crystalline insoluble fraction in the heterophasic propylene copolymer (CXI equivalent bulk sample; HT fraction);
[0060] - amount of amorphous soluble fraction in the heterophasic propylene copolymer (CXS equivalent bulk sample; LT fraction);
[0061] - Ethylene content in the crystallized insoluble fraction (TC2-HT fraction);
[0062] - Ethylene content in the amorphous soluble fraction (TC2-LT fraction);
[0063] - intrinsic viscosity of the insoluble fraction of the crystallization (IV-HT fraction);
[0064] - Intrinsic viscosity of the amorphous soluble fraction (IV-LT fraction).
[0065] The measurement of these properties can be carried out according to the CRYSTEX method by a CRYSTEX QC instrument of CRYSTEX QC Polymer Char (Valencia, Spain). A schematic diagram of the CRYSTEX QC instrument is given in Del Hierro, P.; Ortin, A.; Monrabal, B.; 'Soluble Fraction Analysis in polypropylene, The Column', February 2014, pp. 18-23.
[0066] The CRYSTEX QC instrument includes an infrared detector (IR4) and an online double capillary viscometer. Quantification of HT fraction, LT fraction, TC2 whole, TC2-HT fraction, TC2-LT fraction can be accomplished by an infrared detector that detects IR absorbance in two different bands (CH3 and CH2). IV whole, IV-HT fraction, IV-LT fraction can be measured by an online double capillary viscometer.
[0067] The sample of the heterophasic propylene copolymer to be analyzed was weighed at a concentration of 5 mg / mL. After automatically filling the vial with 1,2,4-TCB containing 250 mg / L 2,6-tert-butyl-4-methylphenol (BHT) as antioxidant, the sample was dissolved at 170°C with continuous stirring at 800 rpm for 120 min until complete dissolution was achieved.
[0068] A defined volume of the sample solution is injected into a column filled with an inert carrier, where crystallization of the sample and separation of the soluble fraction from the crystalline fraction are performed. This process is repeated twice.
[0069] During the first injection the whole sample is subjected to measurements at elevated temperature in order to determine IV integral [dl / g] and TC2 integral (m / m %) of the heterophasic propylene copolymer.
[0070] During the second injection, measurements were performed at low temperature to determine TC2 LT (m / m%), IV LT [dl / g] and the amorphous soluble fraction (CXS equivalent whole sample) (m / m%), followed by measurements at high temperature to determine the TC2 HT fraction (m / m%), IV HT fraction [dl / g] and the crystalline insoluble fraction (CXI equivalent whole sample (m / m%)).
[0071] The crystallized insoluble fraction and the amorphous soluble fraction were separated by temperature cycling of dissolution at 165°C, crystallization at 40°C and redissolution in 1,2,4-trichlorobenzene (1,2,4-TCB) at 165°C.
[0072] The HT fraction and the LT fraction are determined by calibrating the measurement using the Cold Xylene Soluble (CXS) and Cold Xylene Insoluble (CXI) fractions of various heterophasic propylene copolymers with a known CXS content in the range of 8 to 35 wt.-% determined by the standard gravimetric method according to ISO 16152.
[0073] TC2 bulk, TC2-HT fraction and TC2-LT fraction were determined by calibrating the measurements using mixtures of Sabic PP homopolymer 520P and Sabic HDPE M200056 having known ethylene contents ranging from 0 wt% to 50 wt%.
[0074] IV bulk, IV-HT fraction and IV-LT fraction were determined by calibration measurements using several commercial ethylene-propylene copolymers varying between 1 and 6 dL / g of IV bulk, IV-HT fraction and IV-LT fraction determined according to ISO-1628-1 and ISO-1628-3 in decalin at 135°C.
[0075] HECO-A and HECO-B
[0076] Two types of heterophasic propylene copolymers (HECO-A and HECO-B) suitable for use in the present invention are described in detail below. HECO-A and HECO-B are suitable as the first heterophasic propylene copolymer or the second heterophasic propylene copolymer. In some embodiments, the first heterophasic propylene copolymer is HECO-A and the second heterophasic propylene copolymer is HECO-B. In other embodiments, the first heterophasic propylene copolymer is HECO-B and the second heterophasic propylene copolymer is HECO-A.
[0077] HECO-A
[0078] Preferably, HECO-A has a melt flow rate measured according to ISO 1133-1:2011 using 2.16 kg at 230°C in the range of greater than 25 dg / min and up to 120 dg / min, more preferably 30 to 110 dg / min, more preferably 40 to 100 dg / min.
[0079] Preferably, HECO-A has a mass of 3.0 to 15 kJ / m 2 The charpy impact strength is measured at 23°C according to ISO179 / 1eA (II).
[0080] Preferably the dispersed ethylene-α-olefin copolymer is present in HECO-A in an amount of 10 to 40 wt%, such as 10 to 20 wt% or 20 to 30 wt%.The amount of dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer may sometimes be referred to herein as RC.
[0081] Preferably, the amount of ethylene monomer units in the ethylene-α-olefin copolymer in HECO-A is 20 to 60 wt%, preferably 30 to 55 wt%, for example 40 to 50 wt%. The amount of ethylene monomer units in the dispersed ethylene-α-olefin copolymer in the heterophasic propylene copolymer may sometimes be referred to herein as RCC2.
[0082] HECO-A may have a Mw / Mn in the range of 3.0 to 11.0, for example in the range of 4.0 to 9.0, wherein Mw represents the weight average molecular weight and Mn represents the number average molecular weight, and wherein Mw and Mn are measured according to ISO 16014-1(4):2003.
[0083] HECO-A can be separated into an amorphous soluble fraction and a crystalline insoluble fraction according to the CRYSTEX QC method described herein.
[0084] Preferably, HECO-A has a soluble fraction with an intrinsic viscosity of 1.50 to 3.50 dL / g, such as 1.60 to 3.20 dL / g, as measured by an online double capillary viscometer according to the CRYSTEX QC method described herein.
[0085] Preferably, HECO-A has an insoluble fraction having an intrinsic viscosity of 0.85 to 1.15 dL / g, such as 0.90 to 1.10 dL / g, as measured by an online double capillary viscometer according to the CRYSTEX QC method described herein.
[0086] HECO-B
[0087] Preferably, HECO-B has a melt flow rate measured according to ISO 1133-1:2011 using 2.16 kg at 230°C in the range of 1.0 to 25 dg / min, eg, 2.0 to 20 dg / min, 3.0 to 15 dg / min, 5.0 to 12 dg / min.
[0088] Preferably, HECO-B has a thermal conductivity of at least 50 kJ / m 2 The charpy impact strength is measured at 23°C according to ISO179 / 1eA (II).
[0089] Preferably, the dispersed ethylene-α-olefin copolymer in HECO-B is present in an amount of 20 to 50 wt%, preferably 30 to 40 wt%.
[0090] Preferably, the amount of ethylene monomer units in the ethylene-α-olefin copolymer in HECO-B is 45 to 65 wt%, preferably 50 to 60 wt%.
[0091] HECO-B may have a Mw / Mn in the range of 3.0 to 11.0, for example in the range of 4.0 to 9.0, wherein Mw represents the weight average molecular weight and Mn represents the number average molecular weight, and wherein Mw and Mn are measured according to ISO 16014-1(4):2003.
[0092] HECO-B can be separated into an amorphous soluble fraction and a crystalline insoluble fraction according to the CRYSTEX method described herein.
[0093] Preferably, HECO-B has a soluble fraction with an intrinsic viscosity of 1.50 to 3.50 dL / g, such as 1.60 to 3.20 dL / g, as measured by an online double capillary viscometer according to the CRYSTEX QC method described herein.
[0094] Preferably, HECO-B has an insoluble fraction having an intrinsic viscosity of 1.20 to 2.00 dL / g, such as 1.25 to 1.95 dL / g, as measured by an online double capillary viscometer according to the CRYSTEX QC method described herein.
[0095] Elastomer
[0096] Preferably, the elastomer is a copolymer of ethylene and an α-olefin comonomer having 4 to 8 carbon atoms. Preferably, the elastomer has a molecular weight of 0.850 to 0.915 g / cm 3 density.
[0097] The α-olefin comonomer in the elastomer is preferably an acyclic monoolefin such as 1-butene, 1-pentene, 1-hexene, 1-octene or 4-methylpentene.
[0098] Thus, the elastomer is preferably selected from ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers and mixtures thereof. More preferably, the elastomer is selected from ethylene-1-butene copolymers and ethylene-1-octene copolymers.
[0099] Preferably, the density of the elastomer is 0.855 to 0.900 g / cm 3 , more preferably 0.855 to 0.880 g / cm 3 In some embodiments, the density of the elastomer is 0.855 to 0.865 g / cm 3 In some embodiments, the density of the elastomer is 0.865 to 0.880 g / cm 3 .
[0100] Preferably, the elastomer has a melt flow index according to ISO 1133:2011 using 2.16 kg at 190° C. of 0.1 to 40 dg / min. The melt flow index of the elastomer according to ISO 1133:2011 using 2.16 kg at 190° C. may be, for example, 0.1 to 3.0 dg / min, 3.0 to 10 dg / min, or 10 to 40 dg / min.
[0101] Preferably, the amount of ethylene in the elastomer is at least 50 mol%. More preferably, the amount of ethylene in the elastomer is at least 57 mol%, such as at least 60 mol%, at least 65 mol% or at least 70 mol%. Even more preferably, the amount of ethylene in the elastomer is at least 75 mol%. Particularly good transparency (and low haze) is obtained within these ranges. The amount of ethylene in the elastomer can typically be up to 97.5 mol%, such as up to 95 mol% or up to 90 mol%.
[0102] Elastomers suitable for use in the present invention are commercially available, for example under the trademark EXACT TM Available from Exxon Chemical Company of Houston, Texas, or under the trademark ENGAGE TM Polymers (a series of metallocene-catalyzed plastomers) are available from Dow Chemical Company, Midland, Michigan, or as Nexlene TM Available from SK Chemicals. Elastomers can be prepared using methods known in the art, such as by using a single-site catalyst, i.e., a catalyst whose transition metal component is an organometallic compound and at least one ligand has a cyclopentadienyl anionic structure, wherein such ligand is coordinated to the transition metal cation through the bonding of the anionic structure. This type of catalyst is also known as a "metallocene" catalyst. Metallocene catalysts are described, for example, in U.S. Patents Nos. 5,017,714 and 5,324,820. Elastomers can also be prepared using conventional types of heterogeneous multisite Ziegler-Natta catalysts.
[0103] Preferably the total amount of dispersed ethylene-α-olefin copolymer in the first heterophasic propylene copolymer, elastomer and dispersed ethylene-α-olefin copolymer in the second heterophasic propylene copolymer is 25 to 45 wt%, such as 30 to 40 wt% relative to the injection moulded article.
[0104] The elastomer may be a single type of elastomer or a mixture of different types of elastomers having different melt flow indices and / or densities. In the case where the elastomer is a mixture of different types of elastomers, the properties of the elastomer are calculated as a weighted average of the elastomers used.
[0105] Inorganic fillers
[0106] Suitable examples of inorganic fillers include talc, calcium carbonate, wollastonite, barium sulfate, kaolin, glass flakes, layered silicates (bentonite, montmorillonite, montmorillonite) and mica. For example, the inorganic filler is selected from talc, calcium carbonate, wollastonite, mica and mixtures thereof. More preferably, the inorganic filler is talc.
[0107] Preferably, the inorganic filler has a median diameter d50, determined according to ISO 13320-1:2020, of 5 to 20 μm, preferably 3 to 15 μm.
[0108] additive
[0109] Additives include stabilizers. The stabilizer may, for example, be selected from heat stabilizers, antioxidants and / or UV stabilizers. Examples include common stabilizers such as Irgafos 168, Irganox 1010 and / or Irganox B225.
[0110] Additives may further include nucleating agents, colorants such as pigments and dyes; clarifying agents; surface tension adjusting agents; lubricants; flame retardants; mold release agents; flow improvers; plasticizers; antistatic agents; foaming agents; and slip agents.
[0111] LDPE
[0112] In some embodiments the composition of the invention additionally comprises a low density polyethylene. The amount of low density polyethylene may for example be from 1.0 to 10 wt.-% relative to the sum of the first heterophasic propylene copolymer and the low density polyethylene.
[0113] Preferably, the low density polyethylene (LDPE) has a density of 915 to 932 kg / m 3 More preferably, the LDPE has a density of 915 to 928 kg / m 3 The range is preferably between 918 and 922 kg / m 3 Density measured at 23°C according to ISO 1183-1:2012 in the range.
[0114] Preferably, the low density polyethylene has a melt flow rate (MFR) determined according to ISO 1133:2011 using 2.16 kg at 230° C. in the range of 0.30 to 20 dg / min, preferably in the range of 1.0 to 15 dg / min, more preferably in the range of 1.5 to 10 dg / min. LDPE,230 ).
[0115] Preferably, the low density polyethylene (B) has a melt flow rate (MFR) determined according to ISO 1133:2011 using 2.16 kg at 190° C. in the range of 0.10 to 5.0 dg / min, preferably in the range of 0.20 to 3.8 dg / min. LDPE,190 ).
[0116] The LDPE used in the present invention can be produced by using autoclave high pressure technology or by tubular reactor technology. Examples of suitable LDPE are commercially available LDPE 2201H0.
[0117] Method for preparing the composition
[0118] The present invention further provides a process for preparing the composition according to the invention. The process may comprise melt mixing a first heterophasic propylene copolymer, an elastomer, an inorganic filler, additives and a second heterophasic propylene copolymer in an extruder.
[0119] In a more preferred embodiment, the method for preparing the composition according to the present invention comprises providing a masterbatch and a base composition. In these embodiments, the method comprises the following steps:
[0120] I) providing a masterbatch by melt mixing in an extruder a first heterophasic propylene copolymer, an elastomer, an inorganic filler and additives,
[0121] II) providing a base composition comprising a second heterophasic propylene copolymer, and
[0122] III) Providing a composition by melt mixing a masterbatch and a base composition.
[0123] The obtained composition may be in the form of pellets.
[0124] The present invention further provides a kit of parts for making the composition according to the invention comprising a masterbatch comprising a first heterophasic propylene copolymer, an elastomer, an inorganic filler and additives and a base composition comprising a second heterophasic propylene copolymer.
[0125] Injection molding
[0126] The composition according to the invention can be used in a process for producing an injection-molded article from the composition. Accordingly, the present invention provides an injection-molded article comprising or consisting of a composition according to the invention.
[0127] The present invention further provides a method for preparing an injection molded article, wherein a masterbatch is provided separately from a base composition by melt mixing. The masterbatch comprises a first heterophasic propylene copolymer, an elastomer, an inorganic filler and an additive comprising a stabilizer. The base composition comprises a second heterophasic propylene copolymer. The masterbatch and the base composition are preferably provided in the form of pellets. Subsequently, the masterbatch and the base composition are fed to an injection molding machine.
[0128] The injection molding machine includes an extruder part, followed by an injection molding part. The masterbatch and the base composition are fed to the extruder part to obtain a melt mixture. The melt mixture is then processed in the injection molding part to obtain an injection molded article.
[0129] Therefore, the present invention provides a method for preparing an injection molded article, wherein the method comprises the following steps:
[0130] i) providing a masterbatch by melt mixing in an extruder a first heterophasic propylene copolymer, an elastomer, an inorganic filler and additives,
[0131] ii) providing a base composition comprising a second heterophasic propylene copolymer, and
[0132] iii) using an injection molding machine including an extruder section and an injection molding section to provide an injection molded article by melt-mixing the masterbatch and the base composition in the extruder section and processing the obtained melt mixture in the injection molding section to obtain an injection molded article.
[0133] According to the injection molding method of the present invention, a masterbatch is provided which can be melt-mixed with a base composition in an injection molding machine, and various injection molded products having properties adjusted as required can be obtained.
[0134] The invention relating to the process for producing injection-moulded articles is based on the recognition that the use of a masterbatch comprising an elastomer and an inorganic filler leads to considerable energy savings.
[0135] Melt mixing all the components of the final composition to be injection molded to provide pellets requires a lot of energy because the amount to be melt mixed is relatively large, especially when the final composition contains elastomers. This may also require large extruders. These pellets are then melt mixed and injection molded in an injection molding machine.
[0136] In contrast, the amount to be melt mixed to obtain the masterbatch is smaller, which requires less energy. This can also allow the use of a smaller extruder. The masterbatch can be melt mixed with the base composition in the extruder portion of the injection molding machine, after which the final composition is injection molded.
[0137] Since the energy required in the injection molding machine does not differ much between the two processes, the overall energy consumption of the process according to the invention involving the production of a masterbatch requiring less energy is smaller.
[0138] Furthermore, the use of a masterbatch provides greater flexibility for obtaining injection molded articles with different properties. According to the present invention, injection molded articles with different properties can be easily obtained simply by adjusting the amount of the masterbatch relative to the base composition.
[0139] Masterbatch
[0140] The masterbatch comprises the first heterophasic propylene copolymer, an elastomer, an inorganic filler and additives including stabilizers.
[0141] Preferably the amount of the first heterophasic propylene copolymer in the masterbatch is from 40 to 80 wt%, more preferably from 50 to 70 wt%, based on the masterbatch.
[0142] Preferably, the amount of elastomer in the masterbatch is from 10 to 35% by weight, more preferably from 15 to 30% by weight, relative to the masterbatch.
[0143] Preferably, the amount of the inorganic filler in the masterbatch is 5.0 to 40 wt %, more preferably 8.0 to 35 wt %, more preferably 10 to 30 wt %, relative to the masterbatch.
[0144] Preferably, the amount of the additive in the masterbatch is 0.01 to 5.0 wt%, more preferably 0.1 to 3.0 wt%, relative to the masterbatch.
[0145] Preferably, the amount of the stabilizer in the masterbatch is 0.01 to 2.0 wt %, more preferably 0.1 to 1.0 wt %, relative to the masterbatch.
[0146] Preferably, the total amount of first heterophasic propylene copolymer, elastomer, inorganic filler and additives in the masterbatch is at least 90 wt%, at least 95 wt%, at least 98 wt%, at least 99 wt% or 100 wt% relative to the masterbatch.
[0147] The first heterophasic propylene copolymer may be a single type of heterophasic propylene copolymer or a mixture of different types of heterophasic propylene copolymers with different melt flow indices. In case where the first heterophasic propylene copolymer is a mixture of different types of heterophasic propylene copolymers, the properties of the first heterophasic propylene copolymer are calculated as weighted averages of the heterophasic propylene copolymers used.
[0148] In some embodiments the masterbatch additionally comprises a low density polyethylene.The amount of low density polyethylene may for example be from 1.0 to 10 wt.-% relative to the sum of the first heterophasic propylene copolymer and the low density polyethylene.
[0149] Basic composition
[0150] The base composition comprises or consists of a second heterophasic propylene copolymer.
[0151] Preferably the amount of the second heterophasic propylene copolymer in the base composition is from 93 to 100 wt.-% or from 94 to 99.5 wt.-%, such as at least 95 wt.-%, at least 97 wt.-% or at least 98 wt.-% relative to the base composition.
[0152] The base composition may further comprise additives including stabilizers.
[0153] Preferably, the amount of the additive in the base composition is 0.01 to 5.0 wt %, more preferably 0.1 to 3.0 wt %, relative to the base composition.
[0154] Preferably, the amount of the stabilizer in the base composition is 0.01 to 1.0 wt %, more preferably 0.1 to 2.0 wt %, relative to the base composition.
[0155] The second heterophasic propylene copolymer may be a single type of heterophasic propylene copolymer or a mixture of different types of heterophasic propylene copolymers with different melt flow indices. In case where the second heterophasic propylene copolymer is a mixture of different types of heterophasic propylene copolymers, the properties of the second heterophasic propylene copolymer are calculated as weighted averages of the heterophasic propylene copolymers used.
[0156] In some embodiments the base composition additionally comprises a low density polyethylene. The amount of low density polyethylene may for example be from 1.0 to 10 wt.-% relative to the sum of the second heterophasic propylene copolymer and the low density polyethylene.
[0157] The invention further provides a kit of parts for producing the injection-molded articles according to the invention, comprising a masterbatch and a base composition.
[0158] In some embodiments, the masterbatch and base composition included in the kit of the present invention are provided simultaneously or separately. "Separately" is mentioned in the sense of time and / or place. For example, the masterbatch and base composition can be provided by the same supplier or by different suppliers at different times and / or in different places.
[0159] application
[0160] Preferably, the injection molded article according to the present invention is an automobile part, preferably an automobile exterior part, such as a bumper.
[0161] Properties of the composition
[0162] Preferably, the composition according to the invention has one or more of the following properties:
[0163] - a breaktype value of at least 1.2, preferably at least 2.0, more preferably at least 2.4, more preferably at least 2.6, wherein the breaktype value is determined by determining the breaktype of 5 samples according to the instrumented falling weight (IFW) test according to ISO 6603-2 at -20°C using a 65x65x3.2 mm injection molded plaque, 1000 mm dart height and 20 kg dart weight, wherein the values of 4, 3, 2 and 1 are designated as breaktypes YD, YS, YU and NY, respectively and the average of the five values is taken;
[0164] - a melt flow index MFI measured according to ISO 1133-1:2011 using 2.16 kg at 230°C of at least 12.0 dg / min, preferably at least 13.0 dg / min, more preferably at least 15.0 dg / min and at most 25 dg / min, more preferably at most 20 dg / min; for example 16.0 dg / min, 17.0 dg / min, 18.0 dg / min or 19.0 dg / min, and
[0165] - A penetration energy of at least 50 J as determined by instrumented falling weight (IFW) testing according to ISO 6603-2 at -20°C using a 65 x 65 x 3.2 mm injection moulded plaque, 1000 mm dart height and 20 kg dart weight.
[0166] The present invention further provides a masterbatch comprising a heterophasic propylene copolymer, an elastomer, a filler and a stabilizer, wherein the heterophasic propylene copolymer is HECO-A or HECO-B, wherein HECO-A has a melt flow rate of more than 25 to 120 dg / min, measured according to ISO 1133-1:2011 using 2.16 kg at 230 °C and a melt flow rate of 3.0 to 15 kJ / m 2 The charpy impact strength measured by ISO179 / 1eA (II) after 7 days at 23°C, and HECO-B has a melt flow rate measured according to ISO1133-1:2011 using 2.16 kg at 230°C of 1.0 to 25 dg / min and at least 50 kJ / m 2 The Charpy impact strength is measured at 23°C according to ISO 179 / 1eA (II).
[0167] The present invention further provides the use of a masterbatch according to the invention for the preparation of injection molded articles having an improved fracture type value, wherein the fracture type value is determined by determining the fracture type of 5 samples according to an instrumented falling weight (IFW) test in accordance with ISO 6603-2 at -20°C using an injection molded plaque of 65x65x3.2 mm, a dart height of 1000 mm and a dart weight of 20 kg, wherein the values of 4, 3, 2 and 1 are designated as fracture types YD, YS, YU and NY, respectively, and the average of the five values is taken.
[0168] It is to be noted that the present invention relates to the subject matter defined in the independent claims alone or in combination with any possible combination of the features described herein, preferably in particular those combinations of the features presented in the claims. It will therefore be understood that all combinations of features relating to the composition according to the invention, all combinations of features relating to the method according to the invention, and all combinations of features relating to the composition according to the invention with features relating to the method according to the invention are described herein.
[0169] It is also noted that the term "comprising" does not exclude the presence of other elements. However, it is also understood that a description of a product / composition comprising certain components also discloses a product / composition consisting of these components. A product / composition consisting of these components may be advantageous because it provides a simpler, more economical method for preparing the product / composition. Similarly, it is also understood that a description of a method comprising certain steps also discloses a method consisting of these steps. A method consisting of these steps may be advantageous because it provides a simpler, more economical method.
[0170] When values are mentioned for a lower limit and an upper limit for a parameter, it is understood that the range resulting from the combination of the value for the lower limit and the value for the upper limit is also disclosed.
[0171] The invention is now explained with the aid of the following examples without, however, being restricted thereto.
[0172] The following materials were used:
[0173] Heterophasic propylene copolymers and homopolymers
[0174]
[0175] MFI: ISO1133-1:2011, 2.16kg, 230℃
[0176] LT-Fraction-IV and HT-Fraction-IV were determined according to the CRYSTEX method.
[0177] Each of HECO1 to HECO13 is a mixture of a heterophasic propylene copolymer and, for example, a stabilizer. The amount of the heterophasic propylene copolymer in each of HECO1 to HECO13 is at least 98 wt%, except HECO6, which contains LDPE in an amount of 5 wt% and in which the amount of the heterophasic propylene copolymer is about 94 wt%. For HECO6, the indicated RC and RCC2 are the RC and RCC2 of the heterophasic propylene copolymer in HECO6 (i.e., RC and RCC2 are measured without LDPE).
[0178] Charpy impact strength is according to Charpy ISO 179 / 1eA (II) after 7 days at 23°C. Each of the heterophasic propylene copolymers in HECO1 to HECO13 comprises a propylene based matrix which is a propylene homopolymer.
[0179] Elastomers (copolymers of ethylene and α-olefin comonomers)
[0180]
[0181] filler
[0182] LUZENAC HAR T84: talc having a median diameter d50 measured according to ISO 13320-1:2020 of 10 μm
[0183] Additives: stabilizer (IRGANOX B225), nucleating agent (NA), slip agent, black masterbatch
[0184] The components as shown in Tables 2 and 3 were melt mixed to obtain pellets of the masterbatch. These pellets and pellets of the base composition consisting of the components shown in Table 1 were fed to the extruder part of the injection molding machine. The amounts in the table are expressed in % by weight relative to the sum of the masterbatch and the base composition. Injection molded articles were obtained and the properties in Table 4 were measured.
[0185] Table 1: Second heterophasic propylene copolymer in the base composition
[0186]
[0187] Table 2: First heterophasic propylene copolymer in masterbatch
[0188]
[0189] Table 3: Other components in the masterbatch
[0190] POE1 POE2 POE3 filler NA Stabilizer Slip Agent Colorants Example 1 0 0 10 15 0 0.2 0.1 1 Example 2 0 0 10 15 0 0.2 0.1 1 Example 3 5 0 5 10 0 0.2 0.1 1 Example 4 0 0 8 10 0 0.2 0.1 1 Comparative Example 5 0 0 13 15 0 0.2 0.1 1 Comparative Example 6 0 0 10 15 0 0.2 0.1 1 Example 7 5 0 5 15 0 0.2 0.1 1 Example 8 0 5 5 15 0 0.2 0.1 1 Comparative Example 9 5 0 5 15 0 0.2 0.1 1 Example 10 5 0 5 15 0 0.2 0.1 1 Embodiment 11 7 0 5 10 0.1 0.2 0.1 1 Example 12 5 0 5 15 0 0.2 0.1 1 Comparative Example 13 0 0 14 15 0 0.2 0.1 1 Comparative Example 14 4 0 4 15 0 0.2 0.1 1 Comparative Example 15 0 0 0 15 0 0.2 0.1 1 Comparative Example 16 0 0 0 15 0.1 0.2 0.1 1 Comparative Example 17 0 0 10 15 0 0.2 0.1 1 Comparative Example 18 4 0 4 15 0 0.2 0.1 1 Comparative Example 19 0 0 6 15 0 0.2 0.1 1
[0191] Table 4: Properties: MFI ratio, total MFI, simply supported beam, VEM fracture type, VEM value
[0192]
[0193] MFI ratio: MFI1 / MFI2 or MFI2 / MFI1, whichever is greater
[0194] MFI: ISO1133-1:2011, 2.16kg, 230℃
[0195] Charpy: Charpy impact strength, ISO179 / 1eA (II) after 7 days at 23°C
[0196] Flexural modulus: ISO 178 (II) after 7 days at 23°C
[0197] Fracture type value and puncture energy: Instrumented falling weight (IFW) test according to ISO 6603-2, at -20°C using 65 x 65 x 3.2 mm injection molded plaques, 1000 mm dart height and 20 kg dart weight, average value of 5 samples (YD=4, YS=3, YU=2, NY=1)
[0198] Injection-molded articles having different properties were successfully obtained from various types of masterbatches and various types of base compositions.
[0199] Example 1 to Comparative Example 6: Base composition with low MFI, high impact; Base composition with high MFI, low impact MB
[0200] In Example 1, pellets of a base composition comprising a second heterophasic propylene copolymer with low MFI and high impact strength are melt mixed with pellets of a masterbatch consisting of a first heterophasic propylene copolymer with high MFI and low impact strength, an elastomer, talc and additives including stabilizers. The ratio of the MFI of the first heterophasic propylene copolymer (MFI1) to the MFI of the second heterophasic propylene copolymer (MFI2) is 10. The dart impact performance is good in terms of break type and puncture energy. The overall MFI, impact strength and flexural modulus are also good.
[0201] The compositions of Examples 2-4 are similar to Example 1 and show similar good properties. In Example 2 the amount of heterophasic propylene copolymer with low MFI and high impact strength (second heterophasic propylene copolymer) is greater than in Example 1. The break type is even better than in Example 1, while the other properties are still good.
[0202] Comparative Example 5 is similar to Example 1, except that the masterbatch comprises a homopolymer (very high MFI, very low impact strength) instead of a heterophasic propylene copolymer (high MFI, low impact). The MFI of the homopolymer is high and the ratio of the MFI of the homopolymer to the MFI of the first heterophasic propylene copolymer is 15. In terms of break type, the dart impact properties in Example 1 are better than those in Comparative Example 5. The impact strength in Example 1 is also better than that in Comparative Example 5.
[0203] Comparative Example 6 is similar to Example 1, except that the second heterophasic propylene copolymer in the base composition is of a type having a higher MFI and lower impact strength than used in Example 1. The ratio of the MFI of the first heterophasic propylene copolymer (MFI1) to the MFI of the second heterophasic propylene copolymer (MFI2) is 5. The dart impact properties in Example 1 are better than those in Comparative Example 6 in terms of break type and puncture energy.
[0204] Examples 7 to 12: Base compositions with high MFI and low impact; MB compositions with low MFI and high impact
[0205] In examples 7 and 8, unlike in example 1, the second heterophasic propylene copolymer in the base composition has a high MFI and low impact strength, whereas the first heterophasic propylene copolymer in the masterbatch has a low MFI and high impact strength. The ratio of the MFI of the second heterophasic propylene copolymer (MFI2) to the MFI of the first heterophasic propylene copolymer (MFI1) is 6. Similar to example 1, all properties are good.
[0206] Comparative Example 9 is similar to Example 7, but the heterophasic propylene copolymer with low MFI and high impact strength (first heterophasic propylene copolymer) has a higher MFI and a lower impact strength than used in Example 7. The ratio of the MFI of the second heterophasic propylene copolymer (MFI2) to the MFI of the first heterophasic propylene copolymer (MFI1) is 3. The dart impact properties in Example 7 are better than those in Comparative Example 9 in terms of break type.
[0207] Example 10 is similar to example 7, but the second heterophasic propylene copolymer in the base composition is of a type with different RC and RCC2 than used in example 7. Similar as in example 7, the ratio of the MFI of the second heterophasic propylene copolymer (MFI2) to the MFI of the first heterophasic propylene copolymer (MFI1) is 6. Similar to example 7, all properties are good.
[0208] Example 11 is similar to example 10, except that the heterophasic propylene copolymer with low MFI and high impact strength (first heterophasic propylene copolymer) has lower MFI and high impact strength than used in example 10. The ratio of the MFI of the second heterophasic propylene copolymer (MFI2) to the MFI of the first heterophasic propylene copolymer (MFI1) is 11. The amount of heterophasic propylene copolymer with low MFI and high impact strength (first heterophasic propylene copolymer) is smaller than in example 10. Similar to example 10, all properties are good.
[0209] Example 12 is similar to example 10, but the heterophasic propylene copolymer with high MFI and low impact strength (second heterophasic propylene copolymer) has a higher MFI and a different RCC2 than used in example 10. The ratio of the MFI of the second heterophasic propylene copolymer (MFI2) to the MFI of the first heterophasic propylene copolymer (MFI1) is 8. Similar to example 10, all properties are good.
[0210] Comparative Example 13: Base composition with low MFI, low impact; MB with high MFI, low impact
[0211] In Comparative Example 13, a heterophasic propylene copolymer with low MFI and low impact strength was used as the base composition. A heterophasic propylene copolymer with high MFI and low impact strength was used in a masterbatch. The ratio of the MFI of the heterophasic propylene copolymer in the masterbatch to the MFI of the heterophasic propylene copolymer in the base composition was 4.3. The dart impact properties in Example 1 were better than those in Comparative Example 13 in terms of both the break type and the puncture energy.
[0212] Comparative Example 14: Base composition with high MFI, high impact; MB with low MFI, low impact
[0213] In Comparative Example 14, a heterophasic propylene copolymer with high MFI and high impact strength was used as the base composition. A heterophasic propylene copolymer with low MFI and low impact strength was used in the masterbatch. The ratio of the MFI of the heterophasic propylene copolymer in the base composition to the MFI of the heterophasic propylene copolymer in the masterbatch was 3. The ratio of the impact strength of the heterophasic propylene copolymer in the base composition to the MFI of the heterophasic propylene copolymer in the masterbatch was 3.8.
[0214] In terms of fracture type, the dart impact property in Example 1 is better than that in Comparative Example 14. The overall MFI in Comparative Example 14 is lower than that in Example 1.
[0215] Comparative Example 15: Base composition with high MFI, high impact; MB with high MFI, high impact
[0216] In Comparative Example 15, the ratio of the MFI of the heterophasic propylene copolymer in the base composition to the MFI of the heterophasic propylene copolymer in the masterbatch is 1.5. The ratio of the impact strength of the heterophasic propylene copolymer in the base composition to the MFI of the heterophasic propylene copolymer in the masterbatch is 2.6. No elastomer is present in the masterbatch. In terms of the fracture type, the dart impact properties in Example 1 are better than those in Comparative Example 15. The overall MFI in Comparative Example 15 is lower than the overall MFI in Example 1.
[0217] Comparative Example 16: MB without HECO
[0218] In Comparative Example 16, no HECO or elastomer was present in the masterbatch. In terms of fracture type, the dart impact property in Example 1 was better than that in Comparative Example 16. The overall MFI in Comparative Example 16 was lower than that in Example 1.
[0219] Comparative Example 17: MB without HECO
[0220] In Comparative Example 17, HECO is not present in the masterbatch. In terms of fracture type, the dart impact property in Example 1 is better than that in Comparative Example 16. The overall MFI in Comparative Example 16 is lower than that in Example 1.
[0221] Comparative Examples 18 and 19
[0222] In comparative examples 18 and 19 the ratio of the MFI of the heterophasic propylene copolymer in the base composition to the MFI of the heterophasic propylene copolymer in the masterbatch is 1.1. The dart impact properties are good in terms of breaking type. The overall MFI is relatively low.
[0223] None of the comparative examples simultaneously achieved the desired overall MFI of at least 12 dg / min and a break type value of at least 2.
Claims
1. A composition comprising a first heterophasic propylene copolymer having a first melt flow index MFI1 determined according to ISO 1133-1:2011 using 2.16 kg at 230 °C, an elastomer, an inorganic filler, additives including stabilizers and a second heterophasic propylene copolymer having a second melt flow index MFI2 determined according to ISO 1133-1:2011 using 2.16 kg at 230 °C, in, The composition has a melt flow index of at least 12.0 dg / min as measured according to ISO 1133-1:2011 using 2.16 kg at 230°C, and wherein the ratio of MFI1 to MFI2 or the ratio of MFI2 to MFI1 is at least 5.8, more preferably at least 5.9, more preferably at least 6.0, wherein the first heterophasic propylene copolymer consists of: (ia) a propylene based matrix, wherein the propylene based matrix consists of a propylene homopolymer and / or a propylene copolymer consisting of at least 90 wt% propylene monomer units and at most 10 wt% ethylene and / or α-olefin monomer units, based on the total weight of the propylene based matrix, and (ib) a dispersed ethylene-α-olefin copolymer, wherein the total amount of the propylene based matrix in the heterophasic propylene copolymer and the total amount of the dispersed ethylene-α-olefin copolymer sums to 100 wt%, and wherein the second heterophasic propylene copolymer consists of: (iia) a propylene based matrix, wherein the propylene based matrix consists of a propylene homopolymer and / or a propylene copolymer consisting of at least 90 wt% propylene monomer units and at most 10 wt% ethylene and / or α-olefin monomer units, based on the total weight of the propylene based matrix, and (iib) a dispersed ethylene-α-olefin copolymer, wherein the total amount of the propylene based matrix in the heterophasic propylene copolymer and the total amount of the dispersed ethylene-α-olefin copolymer sums up to 100 wt%, wherein the first heterophasic propylene copolymer is HECO-A and the second heterophasic propylene copolymer is HECO-B, or the first heterophasic propylene copolymer is HECO-B and the second heterophasic propylene copolymer is HECO-A, wherein the HECO-A has a melt flow rate of greater than 25 to 120 dg / min measured at 230° C. using 2.16 kg according to ISO 1133-1:2011, the amount of the ethylene-α-olefin copolymer in the HECO-A is 10 to 40% by weight, and the amount of the ethylene monomer unit in the ethylene-α-olefin copolymer in the HECO-A is 20 to 60% by weight, and The HECO-B has a melt flow rate of 1.0 to 25 dg / min as measured according to ISO 1133-1:2011 using 2.16 kg at 230 °C. The amount of the ethylene-α-olefin copolymer in the HECO-B is 20 to 50% by weight, and the amount of ethylene monomer units in the ethylene-α-olefin copolymer in the HECO-B is 45 to 65% by weight.
2. The composition according to claim 1, wherein the first multiphase propylene copolymer has a first impact strength IS1 at 23 °C according to ISO 179 / 1eA(II) and the second multiphase propylene copolymer has a second impact strength IS2 at 23 °C according to ISO 179 / 1eA(II), where MFI1 > MFI2 and IS1 < IS2, or MFI1 < MFI2 and IS1 > IS2.
3. The composition according to any one of the preceding claims, wherein The HECO-A has a range of 3.0 to 15 kJ / m 2 The Charpy impact strength measured at 23°C by ISO179 / 1eA(II), and The HECO-B has a strength of at least 50 kJ / m 2 The charpy impact strength is measured at 23°C according to ISO179 / 1eA (II).
4. The composition according to claim 3, wherein the HECO-A has a soluble fraction with an intrinsic viscosity of 1.50 to 3.50 dL / g as measured by an on-line double capillary viscometer according to the CRYSTEX QC method, and / or the HECO-A has an insoluble fraction with an intrinsic viscosity of 0.85 to 1.15 dL / g as measured by an on-line double capillary viscometer according to the CRYSTEX QC method.
5. The composition according to claim 3 or 4, wherein the HECO-B has a soluble fraction with an intrinsic viscosity of 1.50 to 3.50 dL / g as measured by an on-line double capillary viscometer according to the CRYSTEX QC method, and / or the HECO-B has an insoluble fraction with an intrinsic viscosity of 1.20 to 2.00 dL / g as measured by an on-line double capillary viscometer according to the CRYSTEX QC method.
6. The composition according to any one of the preceding claims, wherein the amount of the first multiphase propylene copolymer is 10 to 50% by weight, preferably 20 to 40% by weight, based on the composition, the amount of the elastomer is 5.0 to 20% by weight, preferably 8.0 to 12% by weight, based on the composition, the amount of the inorganic filler is 5.0 to 30% by weight, preferably 8.0 to 22% by weight, more preferably 8.0 to 17% by weight, and the amount of the second multiphase propylene copolymer is 30 to 80% by weight, preferably 40 to 70% by weight, based on the composition.
7. A composition according to any one of the preceding claims, wherein the composition has a fracture type value of at least 1.2, preferably at least 2.0, more preferably at least 2.4, more preferably at least 2.6, wherein the fracture type value is determined by determining the fracture type of 5 samples according to the instrumented falling weight (IFW) test according to ISO 6603-2 at -20°C using an injection molded plaque of 65x65x3.2 mm, a dart height of 1000 mm and a dart weight of 20 kg, wherein the values of 4, 3, 2 and 1 are designated as fracture types YD, YS, YU and NY, respectively and the average of the five values is taken.
8. A method for preparing a composition according to any one of claims 1 to 7, wherein the method comprises the following steps: I) providing a masterbatch by melt mixing said first heterophasic propylene copolymer, said elastomer, said inorganic filler and said additives in an extruder, II) providing a base composition comprising said second heterophasic propylene copolymer, and III) providing the composition by melt mixing the masterbatch and the base composition.
9. The method according to claim 8, wherein The amount of the first heterophasic propylene copolymer is 40 to 80 wt%, preferably 50 to 70 wt%, based on the masterbatch, The amount of the elastomer is 10 to 35% by weight, preferably 15 to 30% by weight, relative to the masterbatch. The amount of the inorganic filler is 5.0 to 40% by weight, more preferably 8.0 to 35% by weight, more preferably 10 to 30% by weight, based on the masterbatch, and The amount of the additive is 0.01 to 5.0 wt %, more preferably 0.1 to 3.0 wt %, relative to the masterbatch.
10. The method according to any one of claims 8 to 9, wherein The amount of the second heterophasic propylene copolymer relative to the base composition is from 93 to 100 wt.-% or from 94 to 99.5 wt.-%, such as at least 95 wt.-%, at least 97 wt.-% or at least 98 wt.-%.
11. The method according to any one of claims 8 to 10, wherein the weight ratio between the masterbatch and the base composition is from 1:10 to 10:1, such as from 1:1 to 10:1, 1:1 to 5:1 or 1:1 to 2:
1.
12. Kit of parts for making the composition according to any one of claims 1 to 7, comprising a masterbatch comprising the first heterophasic propylene copolymer, the elastomer, the inorganic filler and the additives and a base composition comprising the second heterophasic propylene copolymer.
13. An injection molded article comprising the composition according to any one of claims 1 to 7.
14. A method for preparing an injection molded article according to claim 13, wherein the method comprises the following steps: i) providing a masterbatch by melt mixing said first heterophasic propylene copolymer, said elastomer, said inorganic filler and said additives in an extruder, ii) providing a base composition comprising said second heterophasic propylene copolymer, and iii) using an injection molding machine including an extruder part and an injection molding part to provide the injection molded article by melt-mixing the masterbatch and the base composition in the extruder part and processing the obtained melt mixture in the injection molding part to obtain the injection molded article.
15. A kit of parts for making an injection molded article according to claim 13, comprising the masterbatch and the base composition.