Construction method of thermal barrier coating and heat-resistant component

By using high-speed flame spraying technology on heat-resistant alloy substrates, the surface coating is formed and the ceramic powder aggregation area is controlled, and the problem of high cost of physical vapor deposition of electron beams is solved, and the formation of high-efficiency and low-cost thermal barrier coating is achieved. Reduces the manufacturing cost of heat-resistant components.

CN118922577APending Publication Date: 2024-11-08MITSUBICHI HEAVY IND AERO ENGINES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026618.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-14
Filing Date
2023-03-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the cost of forming a thermal barrier coating by physical vapor deposition of electron beams is high and slow, and it is difficult to reduce costs while ensuring thermal barrier properties and thermal cycle durability.

Method used

The surface coating is formed by high-speed flame spraying on the heat-resistant alloy substrate, and the temperature is maintained above 300°C and below 450°C. A suspension containing ceramic powder is used to ensure that the area of ​​the unmelted ceramic powder is smaller than the cross-sectional area of ​​the surface coating. 0.15%.

Benefits of technology

The formation of a topcoat with the same thermal barrier properties and thermal cycle durability is achieved in a lower cost and shorter time, reducing the cost of equipment introduction and suppressing the manufacturing cost of heat-resistant components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922577A_ABST
    Figure CN118922577A_ABST
Patent Text Reader

Abstract

A method for constructing a thermal barrier coating according to at least one embodiment of the present invention is provided with a step for forming a top coat on a bond coat formed on a heat-resistant alloy substrate of an object. In the step of forming the top coat layer, a suspension containing a ceramic powder is sprayed by high-speed flame spraying while maintaining the temperature of the top coat layer at 300-450 DEG C, thereby forming the top coat layer in which the ratio of the area of a region in which the unmelted ceramic powder agglomerates to the area of the cross-section of the top coat layer is 0.15% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a construction method of a thermal barrier coating and a heat-resistant component.

[0002] This application claims priority based on Japanese Patent Application No. 2022-066894 filed with the Japan Patent Office on April 14, 2022, and the contents of which are incorporated herein by reference. Background Art

[0003] It is known that a thermal barrier coating (TBC) is provided in heat-resistant parts exposed to high-temperature combustion gases, such as burner panels or turbine blades in aircraft engines, turbine blades or split rings in industrial gas turbines, etc. Such a thermal barrier coating includes a bonding coating formed on a heat-resistant alloy substrate and a top coating as a thermal barrier layer formed on the bonding coating.

[0004] The bond coat is formed on the heat-resistant alloy substrate, for example, by spraying (see, for example, Patent Document 1). In addition, in order to ensure thermal cycle durability, the top coat is sometimes formed by electron beam physical vapor deposition (EB-PVD) to include cracks called longitudinal cracks extending in the thickness direction of the top coat within the layer (see, for example, Patent Document 2).

[0005] Previous technical literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2016 / 076305

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-065384 Summary of the invention

[0009] Technical issues to be solved by the invention

[0010] The initial cost of the device for electron beam physical vapor deposition is more than 10 times higher than that of the spraying device. In addition, the operating cost for forming a layer by electron beam physical vapor deposition is about 10 times the operating cost for forming a layer by spraying, etc., which is relatively expensive. In addition, the formation speed of the layer formed by electron beam physical vapor deposition is about a fraction of the formation speed of the layer formed by spraying, etc., which is relatively low. Therefore, a method for forming a top coating at a lower cost while ensuring the thermal barrier properties or thermal cycle durability of the top coating as a thermal barrier coating is desired.

[0011] In view of the above circumstances, at least one embodiment of the present invention aims to reduce the cost of a thermal barrier coating in a heat-resistant component.

[0012] Means for solving technical problems

[0013] (1) A method for applying a thermal barrier coating according to at least one embodiment of the present invention comprises the step of forming a topcoat layer on a bonding coat layer formed on a heat-resistant alloy substrate of an object.

[0014] In the process of forming the top coating, while maintaining the temperature of the top coating at above 300°C and below 450°C, a suspension containing ceramic powder is sprayed by high-speed flame spraying, thereby forming the top coating in which the area of ​​the region where the unmelted ceramic powder is condensed is less than 0.15% relative to the area of ​​the cross-section of the top coating.

[0015] (2) A heat-resistant component according to at least one embodiment of the present invention includes the top coating layer formed by the thermal barrier coating application method according to the method of (1) above.

[0016] Effects of the Invention

[0017] According to at least one embodiment of the present invention, the cost of a thermal barrier coating in a heat-resistant component can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of a cross section of a heat-resistant component provided with a thermal barrier coating applied by a thermal barrier coating application method according to some embodiments.

[0019] Figure 2 This is a diagram showing the appearance of a burner panel for an aircraft engine as an example of a heat-resistant component.

[0020] Figure 3 The present invention is a flowchart showing the procedure of a method for applying a thermal barrier coating according to some embodiments.

[0021] Figure 4A It is a diagram for explaining the outline of an apparatus involved in a method for applying a thermal barrier coating according to some embodiments.

[0022] Figure 4B This is a diagram showing an example of a cooling method for maintaining the temperature of the top coat layer within the above-mentioned temperature range.

[0023] Figure 5 This is a graph schematically showing changes in the temperature of the top coating layer after the start of spraying.

[0024] Figure 6 This is a graph showing the relationship between the thermal conductivity of the topcoat and the temperature during spraying.

[0025] Figure 7 This is a graph showing the relationship between the peeling critical temperature difference and the temperature during spraying.

[0026] Figure 8 This is a graph showing the relationship between the peeling critical temperature difference and the transverse crack length.

[0027] Fig. 9 This is a graph showing the relationship between the deposited film thickness per spraying pass and the temperature during spraying.

[0028] Fig. 10A This is a table showing the measurement results of the density of longitudinal cracks dispersed in the surface direction.

[0029] Fig. 10B This is a table showing the measurement results of the maximum length of the transverse crack.

[0030] Fig.11 It is a diagram for explaining an embodiment related to cooling of a heat-resistant member.

[0031] Fig. 12A It is a diagram for explaining an embodiment related to cooling of a plurality of heat-resistant members.

[0032] Fig. 12B This is a diagram for explaining another embodiment related to cooling of a plurality of heat-resistant members.

[0033] Fig.13 It is a diagram for explaining an embodiment related to cooling of a heat-resistant member.

[0034] Fig.14 It is a diagram for explaining an embodiment related to cooling of a heat-resistant member.

[0035] Fig.15 This is a schematic diagram for explaining the application angle when spraying multiple holes.

[0036] Fig.16 This is a graph showing experimental results of the relationship between the hole diameter and the hole clogging rate by the sprayed material.

[0037] Fig.17 This is a table showing the compositions of the suspension X and the suspension Y used to examine the influence of the region where the unmelted ceramic powder aggregates.

[0038] Fig.18A Graph showing the particle size distribution of the solid component of the suspension X.

[0039] Fig.18B Graph showing the particle size distribution of the solid component of the suspension Y.

[0040] Fig.19A is a SEM image of the solid component of suspension X.

[0041] Fig.19B is a SEM image of the solid component of suspension Y.

[0042] Fig. 20 This is a graph showing the relationship between the temperature during spraying and the peeling critical temperature difference.

[0043] Fig.21 This is a graph showing the relationship between the unmelted particle mixing rate and the peeling critical temperature difference.

[0044] Fig. 22 This is a graph showing the relationship between the pH of a suspension and the Zeta potential of ceramic powder in the suspension.

[0045] Fig.23 is a SEM image of a test piece produced from suspension X.

[0046] Fig.24 This is a SEM image of a test piece produced from suspension Y.

[0047] Explanation of symbols

[0048] 1- heat-resistant component, 3- thermal barrier coating, 5- heat-resistant alloy substrate (parent material), 7- metal bonding layer (bonding coating), 9- top coating. DETAILED DESCRIPTION

[0049] Hereinafter, some embodiments of the present invention will be described with reference to the accompanying drawings. However, the dimensions, materials, shapes, and relative arrangements of the components described in the embodiments or shown in the accompanying drawings are not intended to limit the scope of the present invention, but are merely illustrative examples.

[0050] For example, expressions such as "in a certain direction", "along a certain direction", "parallel", "orthogonal", "center", "concentric" or "coaxial" indicating relative or absolute configuration not only indicate such configuration in a strict sense, but also indicate a state of relative displacement at an angle or distance with a tolerance or a degree to which the same function can be achieved.

[0051] For example, expressions such as “same”, “equal” and “homogeneous” indicating that things are in an equal state not only indicate a state of being equal in a strict sense, but also indicate a state of having a tolerance or a difference in the degree to which the same function can be obtained.

[0052] For example, expressions indicating shapes such as a quadrilateral or a cylinder not only indicate shapes such as a quadrilateral or a cylinder in a strict geometric sense, but also indicate shapes including concave and convex portions or chamfered portions within a range that can obtain the same effect.

[0053] On the other hand, the expression “have”, “complete”, “include”, “includes” or “has” a constituent element is not an exclusive expression that excludes the existence of other constituent elements.

[0054] (About Thermal Barrier Coating 3)

[0055] Figure 1 Schematic diagram of a cross section of a heat-resistant component 1 provided with a thermal barrier coating 3 applied by a thermal barrier coating application method according to some embodiments.

[0056] Figure 2 This is a diagram showing the appearance of a burner panel 1A for an aircraft engine as an example of the heat-resistant member 1 .

[0057] A thermal barrier coating (TBC) 3 for the heat-resistant component 1 is formed on a heat-resistant component 1 such as a combustor panel 1A for an aircraft engine, a turbine blade, a turbine blade or a split ring for an industrial gas turbine.

[0058] In some embodiments, the heat-resistant component 1 includes a heat-resistant alloy substrate (parent material) 5 having a metal bonding layer (bonding coating) 7 and a top coating 9 as a thermal barrier layer. That is, in some embodiments, the thermal barrier coating 3 includes the bonding coating 7 and the top coating 9.

[0059] The bonding coating layer 7 according to some embodiments is made of MCrAlY alloy (M represents a metal element such as Ni, Co, Fe, or a combination of two or more thereof) or the like.

[0060] The top coating layer 9 in some embodiments may be made of a ZrO2-based material, for example, YSZ (yttrium-stabilized zirconia), which is partially or fully stabilized ZrO2 in Y2O3. In addition, the top coating layer 9 in some embodiments may be made of any one of DySZ (dysprosium oxide stabilized zirconia), ErSZ (erbium oxide stabilized zirconia), Gd2Zr2O7 or Gd2Hf2O7.

[0061] Thereby, a thermal barrier coating 3 having excellent thermal barrier properties can be obtained.

[0062] In the top coating 9 involved in some embodiments, the longitudinal cracks Cv extending in the thickness direction of the top coating 9 are in the surface direction, that is, Figure 1 In addition, in the top coat layer 9 according to some embodiments, transverse cracks Ch extending in the surface direction are dispersed.

[0063] In the thermal barrier coating 3 according to some embodiments, the structure having a plurality of longitudinal cracks Cv in the top coat layer 9 can alleviate thermal stress generated by the difference in linear expansion coefficient with the heat-resistant alloy substrate 5 , thereby achieving excellent thermal cycle durability.

[0064] (flow chart)

[0065] Figure 3 The flowchart shows the procedure of the thermal barrier coating construction method according to some embodiments. The thermal barrier coating construction method according to some embodiments includes a step S10 of forming the bonding coating 7 and a step S20 of forming the top coating 9.

[0066] In some embodiments, the step S10 of forming the bonding coating 7 is a step of forming the bonding coating 7 by spraying on the heat-resistant alloy substrate 5. In some embodiments, the step S10 of forming the bonding coating 7 can be, for example, a step of forming the bonding coating by high-velocity flame spraying (HVOF) on the heat-resistant alloy substrate 5. In the following description, it is assumed that the step S10 of forming the bonding coating 7 is a step of forming the bonding coating 7 by high-velocity flame spraying on the heat-resistant alloy substrate 5.

[0067] That is, in some embodiments, in step S10 of forming the bonding coating layer 7 , powder of MCrAlY alloy or the like as a spraying material is sprayed onto the surface of the heat-resistant alloy substrate 5 by high-velocity flame spraying.

[0068] In some embodiments, in order to improve adhesion with the top coat layer 9 , the surface roughness of the adhesive coat layer 7 may be 8 μm or more in terms of arithmetic mean roughness Ra.

[0069] In some embodiments, the step S20 of forming the top coating 9 is a step of forming the top coating 9 on the bonding coating 7 formed on the heat-resistant alloy substrate 5 of the heat-resistant component 1 as the object. In some embodiments, in the step S20 of forming the top coating 9, the top coating is formed by spraying a suspension containing ceramic powder using high-speed flame spraying. That is, in some embodiments, the spraying performed in the step S20 of forming the top coating 9 is suspension-based high-speed flame spraying (S-HVOF). In some embodiments, in the step S20 of forming the top coating 9, a suspension in which ceramic powder as a spraying material is dispersed in a solvent is sprayed onto the surface of the bonding coating 7 by high-speed flame spraying. In the suspension-based high-speed flame spraying, the spraying material TM supplied as a suspension is sprayed onto the surface of the spraying target by the combustion flame jet CF (refer to the later-described Figure 4B ).

[0070] The conditions for spraying in step S20 of forming the top coat layer 9 will be described in detail later.

[0071] Figure 4A It is a diagram for explaining the outline of an apparatus involved in a method for applying a thermal barrier coating according to some embodiments.

[0072] like Figure 4AAs shown, in the construction method of the thermal barrier coating according to some embodiments, the thermal barrier coating 3 is constructed using a spray gun 30, a moving device 50 of the spray gun 30, and a dust collecting hood 70. In addition, in the construction method of the thermal barrier coating according to some embodiments, in addition to Figure 4A In addition to these devices shown, although not shown in the figure, a coating control panel, a control device for controlling the driving of the moving device 50, a supply device for coating material, etc. are also included in the device structure.

[0073] When the thermal barrier coating 3 is applied, if the heat-resistant member 1 to be applied with the thermal barrier coating 3 needs to be fixed, a fixing jig 91 may be used. If the heat-resistant member 1 needs to be continuously rotated, a rotation drive device (not shown) may be used.

[0074] The moving device 50 according to some embodiments is, for example, an industrial robot, but may also be, for example, a scanning device having a slide axis that can move in multiple directions like an NC device.

[0075] like Figure 4A As shown, in the construction method of the thermal barrier coating involved in some embodiments, for example, the spray gun 30, the mobile device 50 and the dust collecting hood 70 are arranged inside a spray chamber 20. The spray hood 20 forms a space separated from the surroundings for sound insulation or preventing dust from scattering to the surroundings. For example, the spray hood 20 can be a box-shaped spray hood arranged in the working room, or it can be an area divided by a part of the working room with a wall, or it can be a dedicated room set in a building.

[0076] The thermal barrier coating 3 is formed on the heat-resistant component 1 as the object to be coated with the thermal barrier coating 3 in the spraying room 20 .

[0077] In the construction method of the thermal barrier coating involved in some embodiments, as described above, in the step S10 of forming the bonding coating 7, spraying based on high-velocity flame spraying (HVOF) is performed, and in the step S20 of forming the top coating 9, spraying based on high-velocity flame spraying (S-HVOF) of a suspension is performed. Therefore, in the construction method of the thermal barrier coating involved in some embodiments, for example, by changing the spray gun 30 and the supply device of the spray material in the step S10 of forming the bonding coating 7 and the step S20 of forming the top coating 9, the step S10 of forming the bonding coating 7 and the step S20 of forming the top coating 9 can be implemented in the same spray chamber 20.

[0078] In the construction method of the thermal barrier coating involved in some embodiments, when the step S20 of forming the top coating 9 is performed after the step S10 of forming the bonding coating 7, the heat-resistant component 1 may not be moved to a spraying room different from the spraying room 20 in which the step S10 of forming the bonding coating 7 is performed. As a result, the step of moving the heat-resistant component 1 to a different spraying room or the step of setting the heat-resistant component 1 after moving it to before the start of spraying can be omitted.

[0079] (Construction Conditions in Step S20 of Forming Top Coat Layer 9)

[0080] Conventionally, in order to ensure thermal cycle durability, the topcoat layer is sometimes formed by electron beam physical vapor deposition (EB-PVD) so as to include cracks called longitudinal cracks extending in the thickness direction of the topcoat layer in the layer.

[0081] However, the initial cost of the device for electron beam physical vapor deposition is more than 10 times that of the spraying device, etc., which is relatively expensive. In addition, the operating cost for forming a layer by electron beam physical vapor deposition is about 10 times the operating cost for forming a layer by spraying, etc., which is relatively expensive. In addition, the formation speed of the layer formed by electron beam physical vapor deposition is about a fraction of the formation speed of the layer formed by spraying, etc., which is relatively low. Therefore, a method for forming a top coating at a lower cost while ensuring the thermal barrier properties or thermal cycle durability of the top coating as a thermal barrier coating is desired.

[0082] As a result of in-depth research conducted by the inventors, it was found that in step S20 of forming the top coating 9, by maintaining the temperature of the top coating 9 at above 300°C and below 450°C while spraying a suspension containing ceramic powder by high-speed flame spraying, it is possible to ensure the same thermal barrier properties or thermal cycle durability as when the top coating is formed on the bonding coating by electron beam physical vapor deposition.

[0083] Therefore, in the construction method of the thermal barrier coating involved in some embodiments, in the step S20 of forming the top coating 9, the top coating 9 is formed by spraying a suspension containing ceramic powder by high-speed flame spraying while maintaining the temperature of the top coating 9 at above 300°C and below 450°C.

[0084] In addition, the research results of the inventors will be described later.

[0085] Thus, the top coat 9 can be formed at a lower running cost and in a shorter time than when the top coat 9 is formed on the bonding coat 7 by electron beam physical vapor deposition. Furthermore, if the top coat 9 is formed by suspension-based high-velocity flame spraying, the introduction cost of the equipment for forming the top coat 9 can also be greatly suppressed.

[0086] Furthermore, the heat-resistant component 1 according to some embodiments has a top coating layer 9 formed by the thermal barrier coating application method according to some embodiments.

[0087] Thereby, the manufacturing cost of the heat-resistant member 1 can be suppressed.

[0088] In step S20 of forming top coat layer 9 , top coat layer 9 may be formed by spraying a suspension containing ceramic powder by high velocity flame spraying while keeping the temperature of top coat layer 9 at 300° C. or higher and 400° C. or lower.

[0089] As a result, the performance of the thermal barrier coating, such as the thermal barrier property and the thermal cycle durability, becomes further improved.

[0090] For example, whether the temperature of the top coating layer 9 is maintained within the above-mentioned temperature range can be measured and confirmed by a non-contact thermometer such as a thermal imager that detects temperature using infrared rays.

[0091] Furthermore, appropriate cooling may be performed so that the temperature of the top coating layer 9 is maintained within the above-mentioned temperature range.

[0092] That is, in the thermal barrier coating construction method according to some embodiments, in step S20 of forming top coating layer 9 , the temperature of top coating layer 9 can be controlled by cooling with a cooling medium.

[0093] This makes it easy to control the temperature of the top coating layer 9 within the above-mentioned temperature range, so that the performance of the thermal barrier coating 3 such as the thermal barrier property and the thermal cycle durability is stabilized.

[0094] Figure 4B This is a diagram showing an example of a cooling method for maintaining the temperature of the top coating layer 9 within the above-mentioned temperature range.

[0095] exist Figure 4B In the example shown, the heat-resistant member 1 is a shaft-shaped member. Figure 4B In the example shown, the heat-resistant member 1 is rotated by a rotation drive device (not shown) for continuously rotating the heat-resistant member 1 while the top coating layer 9 is formed. Figure 4B In the illustrated example, the heat-resistant member 1 is gripped by a gripping portion 92 of a rotation drive device (not shown) and rotates together with the gripping portion 92 .

[0096] exist Figure 4B In the example shown, the heat-resistant component 1 is cooled by the cooling medium CM blown out from the cooling nozzle 81, for example. Figure 4BIn the example shown, in order to suppress the combustion flame jet flow CF from being affected by the cooling medium CM blown out from the cooling nozzle 81, the cooling medium CM can be set to be blown not toward the surface of the surface coating 9, but toward the area 1a in the heat-resistant part 1 where the surface coating 9 is not formed or the holding portion 92 that holds the heat-resistant part 1.

[0097] Regarding the cooling of the heat-resistant member 1 Figure 4B Embodiments other than the illustrated example and types of the cooling medium CM will be described later.

[0098] Figure 5 1 is a diagram schematically showing the change in the temperature of the top coating 9 after the start of spraying. From the moment when the spraying for forming the top coating 9 is started, the temperature of the top coating 9 rises as time passes. Figure 4B In the example shown, the temperature of the top coating layer 9 during spraying can be stably maintained within the above-mentioned temperature range by performing cooling with the cooling medium CM.

[0099] That is, in the thermal barrier coating construction method involved in some embodiments, in the step S20 of forming the top coating 9, it is sufficient that the average temperature of the coating 9 in a stable state after the temperature rises after the start of spraying is maintained within the above temperature range.

[0100] In the following description, this average value is also referred to as the spraying temperature Ta.

[0101] In addition, in the thermal barrier coating application method according to some embodiments, it is not necessary to preheat the heat-resistant member 1 on which the bonding coating 7 is formed before starting the spraying for forming the top coating 9 .

[0102] Hereinafter, the research results of the inventors will be described.

[0103] Figure 6 It is a graph showing the relationship between the thermal conductivity (relative value) of the topcoat layer 9 and the spraying temperature Ta for test piece A with a spraying temperature Ta of 413°C, test piece B with a spraying temperature Ta of 477°C, and test piece C with a spraying temperature Ta of 586°C.

[0104] Figure 7 This is a graph showing the relationship between the peeling limit temperature difference ΔT (relative value) and the spraying temperature Ta for the test pieces A, B, and C.

[0105] Figure 8 This is a graph showing the relationship between the peeling limit temperature difference ΔT (relative value) and the length of the transverse crack Ch (transverse crack length) for the test pieces A, B, and C.

[0106] Fig. 9 This is a graph showing the relationship between the deposited film thickness (relative value) per spraying stroke and the spraying temperature Ta for the test pieces A, B, C, and the test piece D whose spraying temperature Ta is 678°C.

[0107] Fig. 10A This is a table showing the measurement results of the density of longitudinal cracks Cv dispersed in the surface direction for the test pieces A, B, and C.

[0108] Fig. 10B This is a table showing the measurement results of the maximum length of the transverse crack Ch for the test pieces A, B, and C.

[0109] In addition, Figure 6 In FIG. 1 , the thermal conductivity of the top coat layer 9 is expressed as a relative value with the thermal conductivity of the top coat layer formed by electron beam physical vapor deposition (EB-PVD) being set to 1.

[0110] Similarly, in Figure 7 and Figure 8 In the figure, the peeling limit temperature difference ΔT of the top coating layer 9 is expressed as a relative value when the peeling limit temperature difference ΔT of the top coating layer formed by electron beam physical vapor deposition is set to 1. Figure 7 and Figure 8 The delamination critical temperature difference ΔT in ΔT is a temperature difference estimated to cause delamination in the thermal barrier coating 3 when a test in which the temperature difference ΔT is applied is repeated for 1000 cycles.

[0111] exist Fig. 9 In the figure, the deposited film thickness of the top coat layer 9 per one pass is expressed as a relative value, with the deposited film thickness per one pass when the spraying temperature Ta is 450° C. being set as 1.

[0112] In addition, when obtaining Fig. 10A and Fig. 10B The data shown were obtained by observing a microscope photograph of a cut surface obtained by cutting each test piece along the thickness direction of the top coat 9. Fig. 10A and Fig. 10B In the embodiment, each data is acquired at 6 positions (6 fields of view) in which the observation part (field of view) on the cut surface is changed.

[0113] In addition, when obtaining Fig. 10A and Fig. 10B The data shown are as follows: Figure 1 The size of the visual field corresponding to the left and right directions of the figure is 1.09 mm, so the number of longitudinal cracks Cv and the maximum length of transverse cracks Ch observed in this visual field are obtained.

[0114] The spraying conditions other than the spraying temperature Ta for the test pieces A, B, C, and D are as follows.

[0115] Test pieces A to D are as follows Figure 4B In the cylindrical test pieces shown, a top coat 9 is formed on the bonding coat 7 formed on the outer periphery of the test pieces A to D by high velocity flame spraying using a suspension.

[0116] The traverse speed of the spray gun 30 was 100 mm / sec. The film thickness of the top coat 9 was 0.5 mm. The rotation speed of the cylindrical test piece was 1200 rpm.

[0117] In addition, when spraying the test piece, the spray gun 30 is Figure 4B The film is formed by moving the film forming start position on one side in the vertical direction of the figure to the other side. After the spray gun 30 reaches the film forming end position on the other side, the spray gun 30 is moved along Figure 4B The combustion flame jet CF moves in the depth direction of the paper surface in the figure so that it does not contact the test piece and avoids it, and then moves it toward Figure 4B Then, the spray gun 30 is moved along the vertical direction of the figure. Figure 4B The top coating layer 9 is formed by moving in the paper depth direction and returning to the film formation start position, and then repeating the above-mentioned operation.

[0118] like Figure 6 As shown, by setting the spraying temperature Ta to 450° C. or lower, the thermal conductivity of the top coat layer 9 can be reduced to a value equal to or lower than that of the top coat layer 9 formed by electron beam physical vapor deposition.

[0119] In addition, if Figure 6 As shown, by setting the spraying temperature Ta to 400° C. or less, the thermal conductivity of the top coat layer 9 can be further reduced.

[0120] like Figure 7 As shown, by setting the spraying temperature Ta to 400° C. or less, the peeling limit temperature difference ΔT of the top coat layer 9 can be made equal to or higher than that in the case of formation by electron beam physical vapor deposition.

[0121] In addition, as Figure 7 The relative value in the peeling limit temperature difference ΔT of the top coating 9 can be about 0.8. Therefore, by setting the spraying temperature Ta to below 450°C, the peeling limit temperature difference ΔT of the top coating 9 can be set to be above the required temperature difference.

[0122] Therefore, the temperature Ta during spraying is preferably 450° C. or lower, more preferably 400° C. or lower.

[0123] like Figure 8 and Fig. 10BAs shown, it can be seen that the higher the temperature Ta during spraying, the longer the transverse crack Ch tends to be. Moreover, it can be seen that the longer the transverse crack Ch is, the lower the peeling limit temperature difference ΔT of the top coating 9 tends to be. Since the growth of the transverse crack Ch causes the peeling of the top coating 9, which leads to a decrease in thermal cycle durability, the shorter the length of the transverse crack Ch, the better. In addition, Figure 8 The plots shown are based on Fig. 10B Data shown.

[0124] In addition, if Fig. 10A As shown in FIG. 1 , the higher the temperature Ta during spraying, the greater the density of the longitudinal cracks Cv dispersed in the plane direction. The greater the density of the longitudinal cracks Cv dispersed in the plane direction, the higher the thermal cycle durability. However, if the density of the longitudinal cracks Cv dispersed in the plane direction is increased, the length of the transverse cracks Ch tends to increase. Therefore, the density of the longitudinal cracks Cv dispersed in the plane direction only needs to be about 4 / mm.

[0125] like Fig. 9 As shown in FIG. 1 , if the temperature Ta during spraying is lowered, the thickness of the deposited film per spraying stroke becomes smaller. Therefore, if the temperature Ta during spraying is lowered, the productivity of the top coat 9 is reduced.

[0126] like Fig. 9 As shown, when the spraying temperature Ta is lower than 300°C, the deposited film thickness per spraying stroke becomes less than 1 / 2 compared with the case where the spraying temperature Ta is 450°C.

[0127] Therefore, the temperature Ta during spraying is preferably 300°C.

[0128] (Regarding Cooling of Heat-Resistant Component 1)

[0129] Fig.11 It is a diagram for explaining an embodiment related to cooling of the heat-resistant member 1 .

[0130] Fig. 12A This is a diagram for explaining an embodiment related to cooling of a plurality of heat-resistant members 1 .

[0131] Fig. 12B This is a diagram for explaining another embodiment related to cooling of a plurality of heat-resistant members 1 .

[0132] Fig.13 It is a diagram for explaining an embodiment related to cooling of the heat-resistant member 1 .

[0133] Fig.14 It is a diagram for explaining an embodiment related to cooling of the heat-resistant member 1 .

[0134] like Fig.11As shown, for example, when the topcoat layer 9 is formed on one surface of the plate-shaped heat-resistant member 1 , the heat-resistant member 1 can be cooled by blowing the cooling medium CM toward the other surface on the opposite side to the one surface.

[0135] like Fig. 12A and Fig. 12B As shown, in the step S20 of forming the top coat 9 , the top coat 9 may be formed by spraying the plurality of heat-resistant members 1 mounted on the jigs 93 and 94 in sequence.

[0136] Thus, the top coating layer 9 can be efficiently formed on the plurality of heat-resistant members 1 .

[0137] That is, Fig. 12A As shown, a plurality of heat-resistant members 1 may be arranged in a row, and sprayed in one spraying stroke. In this case, for example, a plurality of heat-resistant members 1 arranged in a straight line or in a plane may be held by a jig 93.

[0138] like Fig. 12A As shown, each heat-resistant member 1 may be cooled by blowing the cooling medium CM toward the surface of the heat-resistant member 1 arranged in plurality on the opposite side to the surface on which the top coating layer 9 is formed.

[0139] In addition, if Fig. 12A As shown in FIG. 1 , when a plurality of heat-resistant components 1 are arranged in a row and sprayed in one spraying stroke, the interval between the spraying stroke and the next spraying stroke becomes longer than when spraying one heat-resistant component 1, so it is difficult for the temperature of the top coating 9 to rise. Therefore, if the temperature Ta during spraying can be maintained within the above-mentioned temperature range even without cooling each heat-resistant component 1 by blowing the cooling medium CM, cooling by the cooling medium CM is not necessary.

[0140] like Fig. 12B As shown, the plurality of heat-resistant components 1 arranged in a ring shape and the spray gun 30 may be rotated relative to each other to spray the plurality of heat-resistant components 1. In this case, for example, the plurality of heat-resistant components 1 arranged in a ring shape may be held by a fixture 94. That is, the fixture 94 may hold the plurality of heat-resistant components 1 arranged in a ring shape. Moreover, in the step S20 of forming the top coating layer 9, the plurality of heat-resistant components 1 held by the fixture 94 and the spray gun 30 may be rotated relative to each other, and the plurality of heat-resistant components 1 may be sprayed sequentially.

[0141] Alternatively, the plurality of heat-resistant members 1 arranged in a ring shape may be fixed and sprayed by rotating the spray gun 30 , or the plurality of heat-resistant members 1 arranged in a ring shape may be fixed and sprayed by rotating the spray gun 30 .

[0142] When the plurality of heat-resistant members 1 are rotated, a speed difference occurs between each heat-resistant member 1 and the surrounding air, so that the same cooling effect as when air is blown toward each heat-resistant member 1 can be obtained, and each heat-resistant member 1 can be cooled efficiently.

[0143] For example Fig.13 and Fig.14 As shown, when the heat-resistant component 1 has a plurality of holes 110 opened on the surface of the heat-resistant alloy substrate 5 , such as so-called film cooling holes, the top coating layer 9 can be formed while ejecting gas (cooling medium CM) from the plurality of holes 110 .

[0144] This makes it easy to control the temperature Ta during spraying within the above-mentioned temperature range, so that the performance of the thermal barrier coating 3, such as the thermal barrier property and thermal cycle durability, is stabilized.

[0145] In addition, for example Figure 2 As shown in the burner panel 1A, as long as a plurality of holes communicating with one side and the other side of the burner panel 1A are provided, for example, Fig.13 As shown, the gas may be ejected from the plurality of holes 110 by injecting the gas toward the surface opposite to the surface on which the top coat layer 9 is formed.

[0146] Furthermore, for example, in the case where the plurality of holes 110 in the turbine blade communicate with the cooling passage inside the blade in the turbine blade, in the case where the plurality of holes 110 communicate with the passage 120 inside the heat-resistant component 1 (see Fig.14 ) can also be caused to eject gas from the plurality of holes 110 by supplying gas (cooling medium CM) to the channel 120 connected to the plurality of holes 110.

[0147] (About cooling medium CM)

[0148] In some embodiments, the cooling medium CM may be compressed air compressed by a compressor.

[0149] As long as the compressed air is compressed by a compressor, it is easy to secure the cooling medium CM, and it is possible to suppress an increase in the cost for cooling.

[0150] The compressed air serving as the cooling medium CM may be compressed air compressed by a compressor for generating compressed air for power of a factory, or may be compressed air compressed by a compressor provided for cooling the heat-resistant member 1 .

[0151] Also, in some embodiments, the cooling medium CM may include dry ice.

[0152] That is, the cooling medium CM may be dry ice particles or powder having a relatively small particle size conveyed by compressed air, or may be carbon dioxide having a relatively low temperature obtained by vaporizing dry ice.

[0153] As a result, when forming the top coat layer 9 , the possibility of excessive temperature rise of the top coat layer 9 is reduced, and the performance of the thermal barrier property and thermal cycle durability of the thermal barrier coating 3 is stabilized.

[0154] (Regarding Suppression of Clogging of the Multiple Holes 110 Opened on the Surface of the Heat-Resistant Alloy Base Material 5)

[0155] As described above, in the heat-resistant component 1 according to some embodiments, for example, in order to perform film cooling, a plurality of holes 110 (hereinafter also referred to as cooling holes 110) are opened on the surface of the heat-resistant component 1. In the case of such a heat-resistant component 1, it is necessary to prevent the material of the thermal barrier coating (spraying material) from invading the cooling holes 110 and blocking the cooling holes 110 during the formation process of the thermal barrier coating. Therefore, for example, if a shielding pin is inserted into each cooling hole 110 in advance, it is possible to prevent the material of the thermal barrier coating from invading each cooling hole 110 during the formation process of the thermal barrier coating.

[0156] However, when shielding pins are used, the shielding pins must be removed from each cooling hole 110 after forming the thermal barrier coating. Therefore, the greater the number of cooling holes 110 in the heat-resistant component 1, the greater the workload of removing the shielding pins. Therefore, it is desirable to prevent the cooling holes 110 from being blocked during the formation process of the thermal barrier coating by a simpler method.

[0157] Therefore, in the construction method of the thermal barrier coating involved in some embodiments, for example, in the step S10 of forming the bonding coating 7, the bonding coating 7 can be formed on the heat-resistant alloy substrate 5 by spraying while ejecting gas from a plurality of holes 110 opened on the surface of the heat-resistant alloy substrate 5. That is, in the construction method of the thermal barrier coating involved in some embodiments, for example, the step S10 of forming the bonding coating 7 can be a step of forming the bonding coating 7 on the heat-resistant alloy substrate 5 by spraying while ejecting gas from a plurality of holes 110.

[0158] Thus, by forming the adhesive coating 7 while ejecting gas from the plurality of holes 110, the material of the adhesive coating 7 (spraying material) is prevented from intruding into the plurality of holes 110. Thus, in the step S10 of forming the adhesive coating 7, the plurality of holes 110 can be prevented from being clogged by the material of the adhesive coating 7.

[0159] In addition, as described above, for example, in the step S10 of forming the bonding coating 7 , the bonding coating 7 may be formed on the heat-resistant alloy substrate 5 by high-velocity flame spraying while ejecting gas from the plurality of holes 110 .

[0160] Thus, the adhesive coating layer 7 can be formed by high-velocity flame spraying while preventing the plurality of holes 110 from being clogged with the material of the adhesive coating layer 7 .

[0161] Furthermore, in the construction method of the thermal barrier coating involved in some embodiments, for example, in the step S20 of forming the top coating 9, the top coating 9 can be formed on the bonding coating 7 formed on the heat-resistant alloy substrate 5 by spraying while ejecting gas from a plurality of holes 110 opened on the surface of the heat-resistant alloy substrate 5. That is, in the construction method of the thermal barrier coating involved in some embodiments, for example, the step S20 of forming the top coating 9 can be a step of forming the top coating 9 on the bonding coating 7 formed on the heat-resistant alloy substrate 5 by spraying while ejecting gas from a plurality of holes 110.

[0162] In this way, by forming the topcoat layer 9 while ejecting gas from the plurality of holes 110, the material of the topcoat layer 9 (spraying material, i.e., ceramic powder) is suppressed from intruding into these plurality of holes 110. Thus, in the step S20 of forming the topcoat layer 9, it is possible to suppress the plurality of holes 110 from being clogged by the material of the topcoat layer 9.

[0163] Furthermore, in step S20 of forming topcoat layer 9 , when the above-mentioned inconvenience such as excessive temperature rise of topcoat layer 9 due to spraying may occur, by spraying gas from multiple holes 110 , excessive temperature rise of topcoat layer 9 can be suppressed.

[0164] As described above, for example, in step S20 of forming top coat layer 9 , top coat layer 9 may be formed by spraying a suspension containing ceramic powder by high-velocity flame spraying while ejecting gas from a plurality of holes 110 .

[0165] Thus, the top coat 9 can be formed at a lower running cost and in a shorter time than when the top coat 9 is formed on the bonding coat 7 by electron beam physical vapor deposition. Furthermore, if the top coat 9 is formed by suspension-based high-velocity flame spraying, the introduction cost of the equipment for forming the top coat 9 can also be greatly suppressed.

[0166] In addition, as mentioned above, for example Figure 2 In the case where a plurality of holes communicating with one surface and the other surface of the burner panel 1A are provided, for example, Fig.13 As shown, the gas may be ejected from the plurality of holes 110 by injecting the gas to the surface opposite to the surface on which the top coat layer 9 is formed. In this way, the gas can be easily ejected from the plurality of holes.

[0167] And, if Fig.14As shown, when the plurality of holes 110 are connected to the channel 120 inside the heat-resistant component 1, as described above, the gas (cooling medium CM) can be supplied to the channel 120 connected to the plurality of holes 110 to eject the gas from the plurality of holes 110. By supplying the gas to the channel 120, the gas can be easily ejected from the plurality of holes 110.

[0168] As described above, in the thermal barrier coating formation process, spraying gas from a plurality of holes to suppress clogging of the cooling holes 110 by the spray material is effective regardless of the spraying method, that is, for example, in atmospheric pressure plasma spraying (APS), high velocity oxygen fuel spraying (HVOF), atmospheric pressure plasma spraying based on suspension (S-APS), and high velocity oxygen fuel spraying based on suspension (S-HVOF).

[0169] Fig.15 It is a schematic diagram for explaining the construction angle when spraying the plurality of holes 110 .

[0170] In some embodiments, the construction angle θa when spraying the hole 110 refers to the angle difference between the extension direction of the hole 110 and the spray direction of the spray material (the extension direction of the nozzle 31 of the spray gun 30 ).

[0171] In some embodiments, the inclination angle θb of the hole 110 refers to the difference in angle between the extending direction of the surface 5 a of the heat-resistant alloy substrate 5 and the extending direction of the hole 110 .

[0172] When the construction angle θa is near 90 degrees, the hole 110 is clogged with the spray material. As the construction angle θa gradually decreases from 90 degrees to approach 0 degrees, the hole 110 tends to be less likely to be clogged.

[0173] In addition, for example, in atmospheric pressure plasma spraying (APS), a high-temperature plasma is sprayed to melt the spray material and attach it to the substrate. In contrast, for example, in high-velocity flame spraying (HVOF) or high-velocity flame spraying based on a suspension (S-HVOF), the spray material is made to collide with the substrate at an ultrasonic speed and attach. Therefore, as the construction angle θa gradually decreases from 90 degrees, for example, high-velocity flame spraying (HVOF) or high-velocity flame spraying based on a suspension (S-HVOF) has a tendency to be more difficult to block the hole 110 than atmospheric pressure plasma spraying (APS).

[0174] In addition, in the construction method of the thermal barrier coating involved in some embodiments, in the step S20 of forming the top coating 9, the angle difference between the extension direction of the hole and the injection direction of the spraying material, that is, the construction angle θa, can be set to be greater than 0 degrees and less than 80 degrees for spraying.

[0175] Therefore, the inventors conducted intensive studies and found that, in order to suppress clogging of the hole 110 by the material of the top coat 9 , it is more preferable to perform spray coating with the application angle θa set to 0 degrees or more and 80 degrees or less.

[0176] Therefore, in the thermal barrier coating application method according to some embodiments, by setting the application angle θa to be greater than 0 degrees and less than 80 degrees for spraying, it is possible to effectively prevent the holes 110 from being clogged by the material of the top coating layer.

[0177] In the thermal barrier coating construction method according to some embodiments, the diameter of the hole 110 may be greater than 0.5 mm (eg, greater than 0.533 mm).

[0178] Therefore, the inventors conducted intensive studies and found that, as described later, in order to suppress clogging of the hole 110 by the material of the top coat 9 , the diameter of the hole 110 is preferably larger than 0.5 mm (for example, 0.533 mm or more).

[0179] Therefore, in the thermal barrier coating construction method according to some embodiments, by setting the diameter of the hole 110 to be larger than 0.5 mm (eg, 0.533 mm or larger) and performing spraying, it is possible to effectively prevent the hole 110 from being clogged by the material of the top coating layer 9 .

[0180] Fig.16 This is a graph showing the experimental results of the relationship between the hole size (diameter) of the hole 110 and the clogging rate of the hole 110 by the sprayed material.

[0181] Fig.16 The results shown show that the clogging rate of the hole 110 changes depending on the spraying method or the presence or absence of gas (air) ejection from the hole 110 when the inclination angle θb of the hole 110 is 30 degrees and the construction angle θa is 60 degrees.

[0182] exist Fig.16 In the experiment showing the results, a bonding coating 7 and a top coating 9 were sequentially formed on the surface of a test piece of a heat-resistant alloy corresponding to the heat-resistant alloy substrate 5 described above. Fig.16 In the experiment showing the results, the top coat 9 was formed by high-velocity flame spraying using a suspension, with the target value of the film thickness being set to be the same as the film thickness in the actual machine.

[0183] Fig.16 The clogging rate of the vertical axis of the graph shown is the percentage of the value obtained by dividing the pore diameter Da of the hole 110 after the top coating 9 is formed by the pore diameter Db of the hole 110 after the bonding coating 7 is formed. In addition, since a portion of the hole 110 is blocked by the spraying material of the bonding coating 7, the pore diameter Db of the hole 110 after the bonding coating 7 is formed tends to be smaller than the pore diameter of the hole 110 before the bonding coating 7 is formed.

[0184] Fig.16 The pore diameter on the horizontal axis of the graph shown is the pore diameter of the pore 110 before the bonding coating layer 7 is formed.

[0185] like Fig.16 As shown, when spraying is performed without ejecting air from hole 110, if the hole diameter of hole 110 is less than 0.5 mm, the clogging rate becomes 100%, but if the hole diameter of hole 110 is greater than 0.5 mm (for example, greater than 0.533 mm), the clogging rate is less than about 50%.

[0186] And, if Fig.16 As shown, when spraying is performed without ejecting air from the hole 110, the clogging rate is smaller when the top coat 9 is formed by atmospheric pressure plasma spraying based on a suspension than when the top coat 9 is formed by atmospheric pressure plasma spraying. Fig.16 As shown, when spraying is performed without ejecting air from the holes 110, the clogging rate is smaller when the top coat 9 is formed by high-velocity flame spraying based on a suspension than when the top coat 9 is formed by atmospheric pressure plasma spraying based on a suspension.

[0187] like Fig.16 As shown, in the case of forming the top coating 9 by atmospheric pressure plasma spraying based on a suspension and in the case of forming the top coating 9 by high-speed flame spraying based on a suspension, the clogging rate becomes smaller when spraying is performed while spraying air from the hole 110, compared with the case of spraying without spraying air from the hole 110.

[0188] (Regarding the influence of the area where the unmelted ceramic powder aggregates)

[0189] As described above, as a result of in-depth research conducted by the inventors, it was discovered that, in the process of forming a top coat on a bonding coating, by maintaining the temperature of the top coat at above 300°C and below 450°C while spraying a suspension containing ceramic powder by high-velocity flame spraying, it is possible to ensure the same thermal barrier properties or thermal cycle durability as in the case of forming the top coat on the bonding coating by electron beam physical vapor deposition.

[0190] Furthermore, the inventors conducted in-depth research and found that in the step S20 of forming the topcoat layer 9, even if the temperature of the topcoat layer 9 is maintained at 300°C or more and 450°C or less while spraying the suspension containing the ceramic powder by high-speed flame spraying, if there is an area where the unmelted ceramic powder is aggregated in the topcoat layer 9, the area may become the starting point of peeling cracks and affect the thermal cycle durability. Then, the inventors conducted in-depth research and found that as long as the ratio of the area of ​​the unmelted ceramic powder aggregated area to the area of ​​the cross section of the topcoat layer 9 is 0.15% or less, it is possible to ensure the same thermal barrier properties or thermal cycle durability as when the topcoat layer 9 is formed on the bonding coating 7 by electron beam physical vapor deposition.

[0191] Therefore, in the construction method of the thermal barrier coating involved in some embodiments, in the step S20 of forming the top coating 9, the temperature of the top coating 9 is maintained at above 300°C and below 450°C while a suspension containing ceramic powder is sprayed by high-speed flame spraying, thereby forming a top coating 9 in which the area of ​​the region where the unmelted ceramic powder is condensed is less than 0.15% relative to the area of ​​the cross-section of the top coating 9.

[0192] In addition, the research results of the inventors will be described later.

[0193] Thus, the top coating 9 can be formed at a lower running cost and in a shorter time compared to the case where the top coating 9 is formed on the bonding coating 7 by electron beam physical vapor deposition. In addition, according to the construction method of the thermal barrier coating involved in some embodiments, the introduction cost of the equipment for forming the top coating 9 can also be greatly suppressed.

[0194] In the following description, the ratio of the area of ​​the region where the unmelted ceramic powder is aggregated to the area of ​​the cross section of the topcoat layer 9 is also referred to as the unmelted particle mixing rate. The unmelted particle mixing rate is a value obtained by dividing the area of ​​the region where the unmelted ceramic powder is aggregated by the area of ​​the cross section of the topcoat layer 9 as a percentage. Specifically, the unmelted particle mixing rate is calculated as follows.

[0195] For example, a cross section of the surface coating 9 is polished to obtain an image observed by a scanning electron microscope (SEM). Then, an area where unmelted ceramic powder aggregates within a specified area of ​​the obtained image is determined, and its area is calculated. Then, the calculated area is divided by the area of ​​the specified area to calculate the unmelted particle mixing rate.

[0196] In addition, as described above, the ceramic powder may contain any one of yttria-stabilized zirconia, dysprosia-stabilized zirconia, erbium oxide-stabilized zirconia, Gd2Zr2O7, or Gd2Hf2O7.

[0197] Thereby, a thermal barrier coating 3 having excellent thermal barrier properties can be obtained.

[0198] In the construction method of the thermal barrier coating involved in some embodiments, in the step S20 of forming the top coating 9, the top coating 9 can be formed by maintaining the temperature of the top coating 9 at above 300°C and below 450°C while spraying a suspension containing ceramic powder by high-speed flame spraying to form a top coating 9 with an unmelted particle mixing rate of less than 0.02%.

[0199] As a result, the performance of the thermal barrier coating 3, such as the thermal barrier property and the thermal cycle durability, becomes further improved.

[0200] (About the Zeta potential of ceramic powder in suspension)

[0201] As described above, the lower the temperature of the top coating layer 9 during spraying, the higher the peeling limit temperature difference ΔT of the top coating layer 9 (refer to Figure 7 However, the lower the temperature of the top coating 9 during spraying, the more easily the agglomerated state of the ceramic powder in the suspension is reflected in the structure of the top coating 9, and the more easily the unmelted particles enter the top coating 9.

[0202] In order to facilitate dispersion of the ceramic powder in the suspension, it is preferable to increase the absolute value of the Zheda potential of the ceramic powder in the suspension.

[0203] As described later, the inventors conducted intensive studies and found that when the absolute value of the Zhe potential of the ceramic powder in the suspension is 40 mV or more, the ceramic powder in the suspension is less likely to aggregate, and as a result, intrusion of unmelted particles into the topcoat layer 9 can be suppressed.

[0204] Therefore, in the thermal barrier coating construction method according to some embodiments, in step S20 of forming the topcoat layer 9, a suspension having an absolute value of the Zheda potential of ceramic powder in the suspension of 40 mV or more may be sprayed by high velocity flame spraying.

[0205] This can reduce the area where the unmelted ceramic powder in the top coat layer 9 aggregates, so that the performance of the thermal barrier coating 3 such as the thermal barrier property and the thermal cycle durability becomes good.

[0206] (About pH of suspension)

[0207] As a result of in-depth research conducted by the inventors, it was found that in the ceramic powder used to form the top coating 9, if the pH of the suspension is below 2 or above 9, the absolute value of the zeta potential of the ceramic powder in the suspension becomes above 40 mV, so that the ceramic powder in the suspension is difficult to agglomerate, and as a result, the unmelted particles can be inhibited from entering the top coating 9.

[0208] Therefore, in the construction method of the thermal barrier coating involved in some embodiments, in the step S20 of forming the top coating layer 9, water or ethanol can be used as a dispersion medium to spray a suspension with a pH of 2 or less or 9 or more by high-velocity flame spraying.

[0209] This can reduce the area where the unmelted ceramic powder in the top coat layer 9 aggregates, so that the performance of the thermal barrier coating 3 such as the thermal barrier property and the thermal cycle durability becomes good.

[0210] In addition, as described above, in the construction method of the thermal barrier coating involved in some embodiments, in the step S20 of forming the top coating 9, the top coating 9 can be formed by spraying a suspension containing ceramic powder by high-speed flame spraying while maintaining the temperature of the top coating 9 at above 300°C and below 400°C.

[0211] As a result, the performance of the thermal barrier coating 3, such as the thermal barrier property and the thermal cycle durability, becomes further improved.

[0212] As described above, in the thermal barrier coating application method according to some embodiments, in step S20 of forming top coating layer 9 , the temperature of top coating layer 9 may be controlled by cooling with cooling medium CM.

[0213] Thus, by cooling with the cooling medium CM, the temperature of the top coating layer 9 can be easily controlled within the above-mentioned temperature range, so that the performance of the thermal barrier property and thermal cycle durability of the thermal barrier coating 3 is stabilized.

[0214] In addition, as described above, the cooling medium CM may be compressed air compressed by a compressor. The cooling medium CM may include dry ice.

[0215] Hereinafter, based on the research results of the inventors, the influence of the region where the unmelted ceramic powder aggregates will be described.

[0216] Fig.17 This is a table showing the compositions of the suspension X and the suspension Y used to examine the influence of the region where the unmelted ceramic powder aggregates.

[0217] Fig.18A Graph showing the particle size distribution of the solid component of the suspension X.

[0218] Fig.18B Graph showing the particle size distribution of the solid component of the suspension Y.

[0219] Fig.19A is a SEM image of the solid component of suspension X.

[0220] Fig.19B is a SEM image of the solid component of suspension Y.

[0221] Fig. 20 This is a graph showing the relationship between the spraying temperature Ta and the peeling limit temperature difference ΔT (relative value) for each test piece.

[0222] Fig.21 This is a graph showing the relationship between the unmelted particle mixing ratio and the peeling critical temperature difference ΔT (relative value).

[0223] Fig. 22 This is a graph showing the relationship between the pH of a suspension and the Zeta potential of ceramic powder in the suspension.

[0224] Fig.23 is a SEM image of a test piece produced from suspension X.

[0225] Fig.24 This is a SEM image of a test piece produced from suspension Y.

[0226] In addition, Fig. 20 and Fig.21 In FIG. 1 , the peeling limit temperature difference ΔT of the top coat layer 9 represents a relative value when the peeling limit temperature difference ΔT of the top coat layer formed by electron beam physical vapor deposition is set to 1. Fig. 20 and Fig.21 The delamination critical temperature difference ΔT in ΔT is a temperature difference estimated to cause delamination in the thermal barrier coating 3 when a test in which the temperature difference ΔT is applied is repeated for 1000 cycles.

[0227] like Fig.17 As shown in FIG. 1 , there is no significant difference in the solid component composition between suspension X and suspension Y, but the dispersant components are different. It is presumed that this is caused by the difference in the dispersant components, but as shown in FIG. Fig.18A and Fig.18B As shown, the particle size distribution of the solid components in the suspension X and the suspension Y is different. Specifically, the particle size distribution of the solid components in the suspension Y is lower in peak value and wider in distribution width than the particle size distribution of the solid components in the suspension X.

[0228] like Fig.19A and Fig.19B As shown, the solid components in suspension Y are more aggregated than the solid components in suspension X.

[0229] In addition, the dispersion medium of the suspension X and the suspension Y is water. However, the dispersion medium of the suspension may be ethanol or a mixed solution of water and ethanol.

[0230] exist Fig. 20In the figure, the test pieces A, B, C, F, and G shown in the black filled drawings are the test pieces sprayed with the suspension X, and the test piece E shown in the blank drawings is the test piece sprayed with the suspension Y. Figures 6 to 10B The test pieces A, B, and C shown are the same test pieces.

[0231] As described above, the spraying temperature Ta of the test piece A was 413°C, and the spraying temperature Ta of the test piece E was 412°C. The spraying temperature Ta of the test piece F was 349°C, and the spraying temperature Ta of the test piece G was 268°C.

[0232] The spraying conditions other than the spraying temperature Ta for the test pieces E, F, and G were the same as those for the test pieces A, B, C, and D (reference Fig. 9 ) are the same as the above spraying conditions except for the spraying temperature Ta.

[0233] In addition, the film thickness of the test piece A, that is, the total thickness of the adhesive coating 7 and the top coating 9, is 0.60 mm, the film thickness of the test piece B is 0.51 mm, and the film thickness of the test piece C is 0.54 mm. The film thickness of the test piece E is 0.49 mm, the film thickness of the test piece F is 0.59 mm, and the film thickness of the test piece G is 0.53 mm.

[0234] In the construction method of the thermal barrier coating according to some embodiments, as described above, the top coating layer 9 is preferably formed at a relatively low temperature by cooling with the cooling medium CM. However, as a disadvantage when the top coating layer 9 is formed at a relatively low temperature, the coagulation state of the suspension is easily reflected in the structure of the top coating layer 9. Therefore, if the dispersion state of the suspension is poor, the region where the unmelted ceramic powder is coagulated appears on the top coating layer 9, and this region becomes the starting point of peeling cracks, etc., thereby adversely affecting the mechanical properties of the top coating layer 9.

[0235] like Fig.21 As shown, in the test piece A sprayed with the suspension X, the unmelted particle mixing rate is approximately 0%. In contrast, in the test piece E sprayed with the suspension Y, the unmelted particle mixing rate is approximately 0.24%, which is higher than the unmelted particle mixing rate of the test piece A.

[0236] For example, in Fig.23 In the SEM image of the test piece A shown, no region where the unmelted ceramic powder aggregated was found.

[0237] exist Fig.24 In the SEM image of the test piece E shown, regions where the unmelted ceramic powder aggregated are seen everywhere. Fig.24The area enclosed by the dotted line is shown in the figure. Fig.23 and Fig.24 In the figure, the magnification of SEM images is the same, and the SEM images at 5000 times are cited.

[0238] like Fig. 20 and Fig.21 As shown in FIG. 1 , in the peeling limit temperature difference ΔT of the test piece E sprayed with the suspension Y, the temperature Ta during spraying is substantially the same and is significantly lower than that of the test piece A sprayed with the suspension X. If the SEM images of the cross sections of the test pieces A and E and the particle size distribution of the solid components in the suspension are examined together, it is estimated that the dispersion state of the solid components in the suspension has a significant influence on the peeling limit temperature difference ΔT.

[0239] like Fig.21 As shown, by setting the unmelted particle mixing rate to 0.02% or less, the peeling critical temperature difference ΔT of the top coat layer 9 can be set to be equal to or higher than that in the case of formation by electron beam physical vapor deposition.

[0240] In addition, as Fig.21 The relative value in the peeling limit temperature difference ΔT of the top coating layer 9 can be about 0.8. Therefore, by setting the unmelted particle mixing rate to 0.15% or less, the peeling limit temperature difference ΔT of the top coating layer 9 can be set to be greater than the required temperature difference.

[0241] Therefore, the unmelted particle mixing ratio is preferably set to 0.15% or less, and more preferably set to 0.02% or less.

[0242] like Fig. 22 As shown in FIG. 1 , the zeta potential of the ceramic powder in the suspension X is below -40 mV. In addition, since the zeta potential of the ceramic powder in the suspension X was measured twice, Fig. 22 , a plot of the Zed potential of ceramic powders in two suspensions X is shown.

[0243] The Z-potential of the ceramic powder in the suspension Y is about 35 mV.

[0244] The dispersion state of the suspension is affected by the absolute value of the Zheda potential of the ceramic powder in the suspension. Therefore, the absolute value of the Zheda potential of the ceramic powder in the suspension may be 40 mV or more.

[0245] The Zheda potential of ceramic powder in suspension is affected by the pH of the suspension. Fig. 22 It can be seen that when the pH of the suspension is set to 2 or less or 9 or more, the absolute value of the Zheda potential of the ceramic powder in the suspension becomes 40 mV or more.

[0246] Therefore, the pH of the suspension may be below 2 or above 9.

[0247] The present invention is not limited to the above-described embodiments, and includes modified embodiments of the above-described embodiments or appropriate combinations thereof.

[0248] The contents described in each of the above-mentioned embodiments can be understood, for example, as follows.

[0249] (1) The construction method of a thermal barrier coating according to at least one embodiment of the present invention comprises a step S20 of forming a topcoat layer 9 on a bonding coating layer 7 formed on a heat-resistant alloy substrate 5 of a heat-resistant component 1 as an object. In the step S20 of forming the topcoat layer 9, a suspension containing ceramic powder is sprayed by high-velocity flame spraying while the temperature of the topcoat layer 9 is maintained at 300° C. or higher and 450° C. or lower, thereby forming a topcoat layer 9 in which the ratio of the area of ​​the region where the unmelted ceramic powder is aggregated to the area of ​​the cross section of the topcoat layer 9 (unmelted particle mixing ratio) is 0.15% or less.

[0250] According to the method of (1) above, the top coat 9 can be formed at a lower running cost and in a shorter time than when the top coat 9 is formed on the bonding coat 7 by electron beam physical vapor deposition. In addition, according to the method of (1) above, the introduction cost of the equipment for forming the top coat 9 can also be greatly reduced.

[0251] (2) In some embodiments, in the method of (1) above, in step S20 of forming the top coating 9, the temperature of the top coating 9 can be maintained at above 300°C and below 450°C while a suspension containing ceramic powder is sprayed by high-speed flame spraying, thereby forming a top coating 9 in which the ratio of the area of ​​the region where the unmelted ceramic powder is condensed to the area of ​​the cross-section of the top coating 9 (unmelted particle mixing rate) is less than 0.02%.

[0252] According to the method (2) above, the performance of the thermal barrier coating 3, such as the thermal barrier property and the thermal cycle durability, becomes further improved.

[0253] (3) In some embodiments, in the method of (1) or (2) above, in step S20 of forming the top coating 9, a suspension in which the absolute value of the zeta potential of the ceramic powder in the suspension becomes greater than 40 mV can be sprayed by high-speed flame spraying.

[0254] According to the method (3) described above, the region where the unmelted ceramic powder aggregates in the top coat layer 9 can be reduced, so that the performance of the thermal barrier coating 3 such as the thermal barrier property and the thermal cycle durability becomes good.

[0255] (4) In some embodiments, in the method of (1) or (2) above, in step S20 of forming the top coating 9, water or ethanol can be used as a dispersion medium to spray a suspension with a pH of less than 2 or greater than 9 by high-speed flame spraying.

[0256] According to the method (4) described above, the region where the unmelted ceramic powder aggregates in the top coat layer 9 can be reduced, so that the performance of the thermal barrier coating 3 such as the thermal barrier property and the thermal cycle durability becomes good.

[0257] (5) In some embodiments, in any of the methods (1) to (4) above, in step S20 of forming the top coating 9, the top coating 9 can be formed by spraying a suspension containing ceramic powder by high-speed flame spraying while maintaining the above-mentioned temperature at above 300°C and below 400°C.

[0258] According to the method (5) above, the performance of the thermal barrier coating 3, such as the thermal barrier property and the thermal cycle durability, becomes further improved.

[0259] (6) In some embodiments, in any of the methods (1) to (5) above, in step S20 of forming the top coat layer 9 , the temperature may be controlled by cooling with a cooling medium CM.

[0260] According to the method (6) above, by cooling with the cooling medium CM, the temperature can be easily controlled within the range described in (1) or (5) above, so that the performance of the thermal barrier coating 3 such as the thermal barrier property and thermal cycle durability is stabilized.

[0261] (7) In some embodiments, in the method of (6) above, the cooling medium CM may be compressed air compressed by a compressor.

[0262] According to the method of (7) above, it is easy to secure the cooling medium CM, and it is possible to suppress an increase in the cost for cooling.

[0263] (8) In some embodiments, in the method of (6) above, the cooling medium CM may contain dry ice.

[0264] According to the method (8) above, when forming the top coat layer 9, the possibility of excessive temperature rise of the top coat layer 9 is reduced, and the performance of the thermal barrier property and thermal cycle durability of the thermal barrier coating 3 is stabilized.

[0265] (9) In some embodiments, in any of the methods (1) to (8) above, the ceramic powder may contain any one of yttrium-stabilized zirconia, dysprosium-stabilized zirconia, erbium-stabilized zirconia, Gd2Zr2O7 or Gd2Hf2O7.

[0266] According to the method of (9) above, a thermal barrier coating 3 having excellent thermal barrier properties can be obtained.

[0267] (10) The heat-resistant member 1 according to at least one embodiment of the present invention includes the top coating layer 9 formed by the thermal barrier coating application method according to any one of the methods (1) to (9) above.

[0268] According to the above-mentioned structure (10), the manufacturing cost of the heat-resistant member 1 can be suppressed.

Claims

1. A method for applying a thermal barrier coating, comprising the step of forming a topcoat layer on a bonding coating layer formed on a heat-resistant alloy substrate of an object, In the process of forming the top coating, while maintaining the temperature of the top coating at above 300°C and below 450°C, a suspension containing ceramic powder is sprayed by high-speed flame spraying, thereby forming the top coating in which the area of ​​the region where the unmelted ceramic powder is condensed is less than 0.15% relative to the area of ​​the cross-section of the top coating.

2. The construction method of the thermal barrier coating according to claim 1, in, In the process of forming the top coating, a suspension containing ceramic powder is sprayed by high-speed flame spraying while maintaining the temperature of the top coating at above 300°C and below 450°C, thereby forming the top coating in which the area of ​​the region where the unmelted ceramic powder is condensed is less than 0.02% relative to the area of ​​the cross-section of the top coating.

3. The construction method of the thermal barrier coating according to claim 1 or 2, in, In the step of forming the top coat layer, the suspension in which the absolute value of the Zheda potential of the ceramic powder in the suspension is 40 mV or more is sprayed by high-velocity flame spraying.

4. The construction method of the thermal barrier coating according to claim 1 or 2, in, In the process of forming the top coat layer, water or ethanol is used as a dispersion medium, and the suspension having a pH of 2 or less or 9 or more is sprayed by high-velocity flame spraying.

5. The construction method of the thermal barrier coating according to claim 1 or 2, in, In the step of forming the top coat layer, a suspension containing ceramic powder is sprayed by high-velocity flame spraying while the temperature is maintained at 300° C. or higher and 400° C. or lower, thereby forming the top coat layer.

6. The construction method of the thermal barrier coating according to claim 1 or 2, in, In the step of forming the top coat layer, the temperature is controlled by cooling with a cooling medium.

7. The construction method of the thermal barrier coating according to claim 6, in, The cooling medium is compressed air compressed by a compressor.

8. The construction method of thermal barrier coating according to claim 6, in, The cooling medium includes dry ice.

9. The construction method of the thermal barrier coating according to claim 1 or 2, in, The ceramic powder comprises yttrium-stabilized zirconia, dysprosium-stabilized zirconia, erbium-stabilized zirconia, Gd 2 Zr 2 O 7 or Gd 2 Hf 2 O 7 Any of . 10 . A heat-resistant component comprising the top coating layer formed by the method for applying a thermal barrier coating according to claim 1 or 2.