Method for manufacturing separator for electrolytic capacitor, method for manufacturing electrolytic capacitor, separator for electrolytic capacitor, and electrolytic capacitor

By attaching the conductive polymer components to the fiber sheet in the electrolytic capacitor and compressing the polymer components, the problem of difficulty in entering the polymer components in the high-density fiber structure is solved, and the low ESR and short-circuit resistance of the electrolytic capacitor are improved.

CN118922901APending Publication Date: 2024-11-08PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030058.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When using high-density fiber structures in existing electrolytic capacitors, conductive polymer components are difficult to enter the fiber structure, resulting in a decrease in adhesion amount and an increase in equivalent series resistance (ESR), making it difficult to take into account both short-circuit resistance and ESR.

Method used

By adhering the conductive polymer components to the fiber sheet and compressing them, a composite sheet is formed to ensure that the polymer components are uniformly distributed on the outer surface and inside of the fiber sheet, ESR is reduced, and capacitor elements are formed through the lamination process.

Benefits of technology

The excellent short-circuit resistance and low ESR of the electrolytic capacitor are achieved, which reduces leakage current and improves the overall performance of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922901A_ABST
    Figure CN118922901A_ABST
Patent Text Reader

Abstract

A method for producing a separator for an electrolytic capacitor, the method comprising: a first step for obtaining a composite sheet by adhering a conductive polymer component to a fiber sheet; and a second step of compressing the composite sheet to obtain the diaphragm. The density of the composite sheet before compression is less than 0.60 g / cm < 3 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a diaphragm for an electrolytic capacitor, a method for manufacturing an electrolytic capacitor, a diaphragm for an electrolytic capacitor, and an electrolytic capacitor. Background Art

[0002] Capacitors used in electronic devices are required to have large capacitance and low equivalent series resistance (ESR) in the high-frequency region. As capacitors with large capacitance and low ESR, electrolytic capacitors using conductive polymers such as polypyrrole, polythiophene, polyfuran, and polyaniline as solid electrolytes are expected.

[0003] Patent document 1 proposes a method for manufacturing an electrolytic capacitor, which comprises the following steps: a step of preparing an anode foil, a cathode foil and a fiber structure having a dielectric layer; a step of preparing a conductive polymer dispersion containing a conductive polymer component and a dispersion medium; a step of applying the conductive polymer dispersion to the fiber structure and removing at least a portion of the dispersion medium to prepare a diaphragm; and a step of sequentially stacking the anode foil, the diaphragm and the cathode foil to prepare a capacitor element, wherein the dispersion medium contains water, the fiber structure contains 50% by mass or more of synthetic fibers, and the density of the fiber structure is 0.2 g / cm 3 Above and less than 0.45g / cm 3 .

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2020 / 158783 Pamphlet Summary of the invention

[0007] Problems to be solved by the invention

[0008] When a high-density fiber structure is used for the purpose of improving short-circuit resistance, the gaps between the fibers of the fiber structure are small, and when the conductive polymer dispersion is applied to the fiber structure, it becomes difficult for the particles of the conductive polymer component to enter the interior of the fiber structure. As a result, the amount of conductive polymer components attached to the interior of the fiber structure decreases and the ESR increases. In this way, it is difficult to achieve both improved short-circuit resistance and reduced ESR.

[0009] Means for solving problems

[0010] One aspect of the present invention relates to a method for manufacturing a separator for an electrolytic capacitor, including the following steps: a first step of attaching a conductive polymer component to a fiber sheet to obtain a composite sheet; and a second step of compressing the composite sheet to obtain a separator, wherein the density of the composite sheet before compression is less than 0.60 g / cm 3 .

[0011] Another aspect of the present invention relates to a method for manufacturing an electrolytic capacitor, including the following steps: a step of preparing an anode foil; a step of preparing a cathode foil; a step of obtaining a separator by the above-described method for manufacturing a separator for an electrolytic capacitor; and a step of sandwiching the separator between the anode foil and the cathode foil and laminating the anode foil and the cathode foil.

[0012] Still another aspect of the present invention relates to a separator for an electrolytic capacitor, which includes a composite sheet including a fiber sheet and a conductive polymer component attached to the fiber sheet, and the composite sheet has: a density of 0.33 g / cm 3 or more and less than 0.74 g / cm 3 , an air permeability of 0.5 seconds / 100 mL or more and less than 58 seconds / 100 mL, and a basis weight (Japanese: tsubome) of 19.0×10 -4 g / cm 2 or more.

[0013] Still another aspect of the present invention relates to an electrolytic capacitor, which includes an anode foil, a cathode foil, and a separator sandwiched between the anode foil and the cathode foil, and the separator is the above-described separator for an electrolytic capacitor.

[0014] Advantages of the Invention

[0015] According to the present invention, an electrolytic capacitor having excellent short-circuit resistance and low ESR can be obtained.

[0016] New features of the present invention are described in the appended claims, but regarding both the structure and content of the present invention, the following detailed description is made by combining other objects and features of the present invention and referring to the drawings, so as to be better understood. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is a cross-sectional view schematically showing an electrolytic capacitor according to an embodiment of the present invention.

[0018] Figure 2 is a perspective view obtained by unfolding a part of the wound body. DETAILED DESCRIPTION OF THE INVENTION

[0019] Hereinafter, examples are given to illustrate the embodiments of the present invention, but the present invention is not limited to the examples described below. In the following description, there are cases where specific numerical values ​​and materials are illustrated, but other numerical values ​​and materials may also be applied as long as the effect of the present invention can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be replaced by the statement "above numerical value A and below numerical value B". In the following description, when the lower limit and upper limit of numerical values ​​related to specific physical properties, conditions, etc. are illustrated, as long as the lower limit is not above the upper limit, any lower limit illustrated can be arbitrarily combined with any upper limit illustrated. When multiple materials are illustrated, one can be selected and used alone, or two or more can be used in combination.

[0020] [Method for producing diaphragm for electrolytic capacitor]

[0021] The method for manufacturing a separator for an electrolytic capacitor according to an embodiment of the present invention comprises the following steps: a first step of attaching a first conductive polymer component (hereinafter, also referred to as the first polymer component) to a fiber sheet to obtain a composite sheet; and a second step of compressing the composite sheet to obtain a separator. The density of the composite sheet before compression is less than 0.60 g / cm 3 .

[0022] In the first step, a low-density fiber sheet is used, so that the first polymer component can be attached to the inside of the fiber sheet. That is, the first polymer component can be arranged on the outer surface of the fiber sheet while being fully arranged in the gaps between the fibers inside the fiber sheet. In addition, by compressing the composite sheet in the second step, a thin diaphragm can be obtained while the first polymer component can be firmly attached to the fibers. When the long diaphragm is wound onto a roller, it is easy to maintain the state of the first polymer component attached to the fibers. In this way, the equivalent series resistance (ESR) of the electrolytic capacitor can be reduced.

[0023] The density of the composite sheet before compression is less than 0.60g / cm 3 , can be 0.59g / cm 3 Below, it can also be 0.22g / cm 3 Above (or 0.25g / cm 3 Above) and less than 0.60g / cm 3 (or 0.59g / cm 3 When the density of the composite sheet before compression is 0.60 g / cm 3 If the value is greater than this, the density of the fiber sheet increases, and the first polymer component may not be sufficiently attached to the inside of the fiber sheet, resulting in an increase in ESR.

[0024] The density of the composite sheet can be obtained by the following method.

[0025] A test piece of a specified size is cut out from the composite sheet, and a drying treatment is performed at 125°C for more than 3 hours to fully remove the first dispersion medium remaining in the test piece. Then, the length, width, thickness and weight of the test piece are measured, and the weight is divided by the volume obtained from the length, width and thickness to obtain the density of the composite sheet. Five test pieces are taken out, and the density of each of the five test pieces is obtained, and the average value thereof is obtained.

[0026] In the second step, the density of the composite sheet, that is, the density of the fiber sheet, can be increased by compressing the composite sheet, thereby improving the short-circuit resistance of the electrolytic capacitor and reducing the leakage current.

[0027] The above scheme can achieve both low ESR and improved short-circuit resistance of the electrolytic capacitor.

[0028] (1st step)

[0029] From the viewpoint of ensuring the impregnation of the fiber sheet with the first polymer component, the density of the fiber sheet used in the first step before compression may be 0.58 g / cm 3 Below (or 0.55g / cm 3 Below), it can also be 0.20g / cm 3 Above 0.58g / cm 3 Below (or 0.55g / cm 3 the following).

[0030] It should be noted that the density of the fiber sheet is determined based on JIS C2300-2 (Cellulose paper for electrical use - Part 2: Test methods). Specifically, a test piece of a predetermined size is cut out from the fiber sheet, dried at 105°C for more than 3 hours, and then determined by a weight method. That is, the length, width, thickness, and weight of the test piece are measured, and the weight is divided by the volume determined from the length, width, and thickness to determine the density of the fiber sheet. Five test pieces are taken out, and the density of each of the five test pieces is determined, and the average value thereof is determined.

[0031] The first step includes, for example, the following steps: a step 1a of preparing a conductive polymer dispersion (hereinafter, also referred to as the first polymer dispersion) containing a first polymer component and a first dispersion medium; and a step 1b of removing at least a portion of the dispersion medium after applying the first polymer dispersion to the fiber sheet or allowing the first polymer dispersion to penetrate into the fiber sheet. The first dispersion medium usually contains water. Removal of at least a portion of the first dispersion medium can be performed by drying.

[0032] As for the fiber sheet, a fiber sheet containing cellulose fibers can generally be used. Cellulose fibers are advantageous in terms of cost and electrolyte retention. Since cellulose fibers have hydroxyl groups, the fiber sheet containing cellulose fibers is prone to swelling in the first dispersion medium containing water, and the swollen fiber sheet is prone to shrinkage due to the subsequent drying process. In the first step, the above-mentioned fiber sheet sometimes produces wrinkles on the fiber sheet due to swelling and shrinkage, but by compressing the composite sheet in the second step, the unevenness caused by the wrinkles can be reduced. As a result, the unevenness of the thickness of the diaphragm caused by the unevenness and the increase in the deviation of the inter-electrode distance in the electrolytic capacitor caused by the unevenness of the thickness are suppressed.

[0033] Through step 1b, the first polymer component is attached to the surface of the fibers constituting the fiber sheet. In step 1b, a low-density fiber sheet is used, so that the first polymer component can be sufficiently attached to the inside of the fiber sheet. That is, the first polymer dispersion can smoothly penetrate into the inside of the fiber sheet, and the particles of the first polymer component can smoothly enter the gaps between the fibers.

[0034] The first polymer dispersion in step 1b may be applied to the fiber sheet by coating or spraying. Examples of coating machines include gravure coaters, knife coaters, comma coaters, roll coaters, die coaters, lip coaters, and other known devices.

[0035] The coating treatment may be performed on one side or both sides of the fiber sheet. The coating treatment may also be performed multiple times on the same side of the fiber sheet. In this case, the drying treatment may be performed after the multiple coating treatments are performed continuously, or the drying treatment may be performed after each coating treatment.

[0036] The impregnation of the fiber sheet with the first polymer dispersion in step 1b can be performed by immersing the fiber sheet in the first polymer dispersion contained in a container. The immersion treatment can also be performed multiple times. The drying treatment can be performed after the multiple immersion treatments are performed continuously, or the drying treatment can be performed after each immersion treatment.

[0037] The removal of the first dispersion medium in the 1b step can be carried out by drying. The drying process can be carried out, for example, by heating and drying at a temperature of 50°C or above and 150°C or below, or can be carried out under reduced pressure (for example, an atmosphere with a gauge pressure of -50kPa or above and -90kPa or below). In this case, the drying process can be carried out to the extent that the first dispersion medium is not completely removed, but it is preferred that, for example, a drying process is carried out to remove more than 80% by mass (or more than 90% by mass) of the first dispersion medium contained in the first polymer dispersion immediately after coating (impregnation). In this case, in the second step (compression process), the adhesion of the first polymer component contained in the composite sheet to the compression device (calendering roll, etc.) is suppressed, and the unevenness of the adhesion amount of the first polymer component of the composite sheet caused by the adhesion of the first polymer component to the compression device is suppressed.

[0038] The step 1b is preferably performed on a long fiber sheet. In this case, a roll-to-roll method can improve productivity. The step 1b can be performed, for example, by coating and drying one surface of the long fiber sheet and then winding the fiber sheet onto a roll. Furthermore, after that, the fiber sheet can be rolled out in the reverse direction while the other surface is coated using the same or another coating machine.

[0039] When the first polymer dispersion is impregnated into the long fiber sheet, a container for storing the first polymer dispersion is prepared, and the long fiber sheet is transported into the container by a transport roller and immersed in the first polymer dispersion. Thereafter, the fiber sheet is transported out of the container for drying, and the obtained composite sheet is wound onto a roller.

[0040] (Second step)

[0041] In the second step, the composite sheet is compressed in the thickness direction to obtain a separator. In the second step, the composite sheet is preferably roll-pressed. For a long composite sheet, a roll-to-roll method can be used to improve productivity.

[0042] The ratio of the thickness T1 of the composite sheet (separator) after compression to the thickness T0 of the composite sheet before compression: T1 / T0 is preferably greater than 0.50 and less than 0.95, and more preferably greater than 0.60 and less than 0.95. When T1 / T0 is less than 0.95, it is easy to obtain the effect of improving the short circuit resistance brought about by the high density of the fiber sheet. When T1 / T0 is greater than 0.50 (or greater than 0.60), it is easy to moderately control the pressing pressure to be smaller in the second step, and the adhesion of the first polymer component contained in the composite sheet to the pressing device (calendering roll, etc.) is suppressed, and the reduction and deviation of the amount of the first polymer component contained in the composite sheet accompanying the adhesion are suppressed. In addition, in this case, the electrolyte can be fully impregnated into the interior of the composite sheet in the electrolyte impregnation step of the subsequent step.

[0043] From the perspective of reducing ESR and improving short circuit resistance, the thickness T1 of the compressed composite sheet (diaphragm) can be, for example, 20 μm or more and 90 μm or less, or 25 μm or more and less than 60 μm (or 58 μm or less). It should be noted that the thickness T0 and thickness T1 of the composite sheet are the average values ​​of the thicknesses of any 10 points of the composite sheet before and after compression, respectively.

[0044] The composite sheet may also be compressed while being heated and / or humidified. In this case, the first polymer component can be more firmly attached to the fiber sheet, and the unevenness caused by wrinkles can be further reduced. In this case, it is desirable to adjust the degree of heating and / or humidification within a range in which the first polymer component contained in the composite sheet is inhibited from adhering to the pressing device (calender roll, etc.).

[0045] Hereinafter, the fiber sheet and the first polymer dispersion used in the first step will be described in detail.

[0046] (Fiber Sheet)

[0047] The fiber sheet is a porous sheet made of fiber material. The fiber sheet may be a woven fabric or a nonwoven fabric. The fiber sheet preferably contains at least cellulose fibers. The content of cellulose fibers in the fiber sheet is preferably 20% by mass or more, or may be 20% by mass or more and 80% by mass or less. In this case, the composite sheet can be easily compressed.

[0048] The fiber sheet may contain cellulose fibers and synthetic fibers, or may be a mixture of cellulose fibers and synthetic fibers. In this case, it is easy to ensure the strength of the fiber sheet, and the fiber sheet is difficult to swell due to water. Examples of synthetic fibers include nylon fibers, aramid fibers, acrylic fibers, polyester fibers, and polyphenylene sulfide fibers. The synthetic fibers may be used alone or in combination of two or more. The content of the synthetic fibers in the fiber sheet is, for example, 20% by mass or more and 80% by mass or less.

[0049] The fiber sheet may contain cellulose fibers and a paper strengthener at the same time. The paper strengthener may contain a wet paper strengthener and / or a dry paper strengthener. Examples of the wet paper strengthener include urea-formaldehyde resin, melamine-formaldehyde resin, polyamide polyamine epichlorohydrin, and polyvinylamine. Examples of the dry paper strengthener include polyacrylamide, polyvinyl alcohol, starch, and carboxymethyl cellulose. One type of the paper strengthener may be used alone, or two or more types may be used in combination.

[0050] The thickness of the fiber sheet used in the first step is not particularly limited. The thickness of the fiber sheet before compression may be, for example, 25 μm or more and 100 μm or more, or 30 μm or more and 95 μm or less. In this case, in the second step, the thickness of the separator (compressed fiber sheet) can be easily adjusted to a desired range from the viewpoint of improving short circuit resistance and reducing ESR.

[0051] (First polymer dispersion)

[0052] The first polymer dispersion includes a first polymer component and a first dispersion. The first polymer dispersion can be obtained, for example, by dispersing particles of the first polymer component in a first dispersion medium, polymerizing a precursor monomer of the first polymer component in the first dispersion medium to generate particles of the first polymer component in the first dispersion medium, or the like.

[0053] The content of the first polymer component in the first polymer dispersion may be, for example, 1 mass % or more (or 3 mass % or more) and 15 mass % or less. When the content of the first polymer component is within the above range, a sufficient amount of the first polymer component can be attached to the fiber sheet.

[0054] The viscosity of the first polymer dispersion can be, for example, 10 mPa·s or more (or 100 mPa·s or more) and 200 mPa·s or less. In this case, it is easy to apply the first polymer dispersion to the fiber sheet and to make the first polymer dispersion permeate into the fiber sheet. It should be noted that the viscosity of the polymer dispersion can be determined at room temperature (20° C.) using a vibration viscometer (e.g., VM-100A manufactured by SEKONIC Co., Ltd.).

[0055] (First polymer component)

[0056] The first polymer component includes a conductive polymer. Examples of the conductive polymer include polypyrrole, polythiophene, polyfuran, polyaniline, etc. The conductive polymer may be used alone or in combination of two or more, or may be a copolymer of two or more monomers.

[0057] It should be noted that, in this specification, polypyrrole, polythiophene, polyfuran, polyaniline, etc. respectively mean polymers with polypyrrole, polythiophene, polyfuran, polyaniline, etc. as basic skeletons. Therefore, polypyrrole, polythiophene, polyfuran, polyaniline, etc. may also include their respective derivatives. For example, polythiophene may include poly(3,4-ethylenedioxythiophene) and the like.

[0058] The first polymer component may further include a dopant. The dopant may be a polyanion. Specific examples of polyanions include polyethylene sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacryloyl sulfonic acid, polymethacryloyl sulfonic acid, poly(2-acrylamide-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, polyacrylic acid, etc. The dopant may be used alone or in combination of two or more. In addition, the dopant may be a polymer of a single monomer or a copolymer of two or more monomers. Among them, polystyrene sulfonic acid is preferred.

[0059] The weight average molecular weight of the polyanion contained in the first polymer component is not particularly limited. The weight average molecular weight of the polyanion is, for example, 1000 or more and 200000 or less. Such a conductive polymer component containing polyanions is easily dispersed uniformly in the first dispersion medium and easily adheres to the fiber sheet. In addition, the weight average molecular weight of the polyanion can be 1000 or more and 100000 or less. Even in the case of such a large amount of polyanions contained, the excessive increase in the viscosity of the dispersion is suppressed, and the amount attached to the fiber sheet is easily increased.

[0060] The first polymer component is dispersed in the first dispersion medium in the form of particles, for example. The mode particle size of the particles of the first polymer component is not particularly limited and can be appropriately adjusted by polymerization conditions, dispersion conditions, etc. The mode particle size of the particles of the first polymer component is, for example, 0.01 μm or more and 0.5 μm or less. When the density of the fiber sheet before compression is less than 0.6 g / cm 3 (or 0.55g / cm 3When the fiber sheet is compressed to a volume of 0.2 μm or less, the mode diameter of the particles of the first polymer component contained in the fiber sheet before compression may be, for example, 0.02 μm or more and 0.2 μm or less. In this case, it is easy to make the particles of the first polymer component adhere to the inside of the fiber sheet. Here, the mode diameter is the mode value (modal diameter) of the particle diameter in the volume particle size distribution measured by a particle diameter measuring device based on the dynamic light scattering method.

[0061] The conductivity of the diaphragm (compressed composite sheet) containing the first polymer component is, for example, 0.1 mS / cm or more, and may be 1 mS / cm or more. The higher the conductivity of the diaphragm containing the first polymer component, the more the ESR reduction effect can be obtained. The conductivity of the diaphragm containing the first polymer component can be adjusted by the type and molecular weight of the conductive polymer and the dopant, the amount of the first polymer component attached to the fiber sheet in the first step, the pressing pressure in the second step, etc. The conductivity of the diaphragm containing the first polymer component is measured by the four-probe method based on JIS K 7194:1994.

[0062] (First dispersion medium)

[0063] The first dispersion medium contains water. The first dispersion medium may also contain a non-aqueous solvent. Non-aqueous solvent is a general term for liquids other than water, including organic solvents and ionic liquids. The proportion of water in the first dispersion medium may be 50% by mass or more, 70% by mass or more, or 90% by mass or more. As non-aqueous solvents used together with water, polar solvents (protic solvents and / or non-protonic solvents) may be cited.

[0064] Examples of the protic solvent include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol (EG), propylene glycol, polyethylene glycol (PEG), diethylene glycol monobutyl ether, glycerol, 1-propanol, butanol, polyglycerol, sorbitol, mannitol, pentaerythritol, and formaldehyde. Examples of the aprotic solvent include amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone, esters such as methyl acetate and γ-butyrolactone (γBL), ketones such as methyl ethyl ketone, ethers such as 1,4-dioxane, sulfur-containing compounds such as dimethyl sulfoxide and sulfolane (SL), and carbonate compounds such as propylene carbonate.

[0065] When the first dispersion medium contains the above-mentioned alcohols (especially polyols and sugar alcohols), its conductivity and permeability to the separator are easily improved. On the other hand, polyols and sugar alcohols easily cause the fiber sheet to swell and wrinkle. Therefore, the method for manufacturing the electrolytic capacitor separator of this embodiment can achieve the effect of significantly suppressing the generation of wrinkles.

[0066] [Diaphragms for electrolytic capacitors]

[0067] The electrolytic capacitor separator according to the embodiment of the present invention comprises a composite sheet including a fiber sheet and a conductive polymer component (first polymer component) attached to the fiber sheet. The composite sheet has: 3 Above and less than 0.74g / cm 3 density, air permeability of 0.5 sec / 100 mL or more and less than 58 sec / 100 mL, and 19.0×10 -4 g / cm 2 The diaphragm can be obtained by the above-mentioned method for producing a diaphragm for an electrolytic capacitor.

[0068] When the density and basis weight of the composite sheet are within the above range, the short circuit resistance of the electrolytic capacitor is improved, the ESR is reduced, and the leakage current is reduced. The density of the composite sheet can be 0.34 g / cm 3 Above 0.53g / cm 3 In this case, the leakage current is reduced and excellent short circuit resistance is easily obtained. The basis weight of the composite sheet can be 19×10 -4 g / cm 2 Above and 35×10 -4 g / cm 2 The density of the fiber sheet contained in the separator may be 0.32 g / cm 3 Above and less than 0.72g / cm 3 , can also be 0.33g / cm 3 Above and 0.50g / cm 3 the following.

[0069] The density and basis weight of the composite sheet can be determined by the following method.

[0070] A test piece of a specified size is cut out from the composite sheet, and a drying treatment is performed at 125°C for more than 3 hours to fully remove the first dispersion medium remaining in the test piece. Then, the length, width, thickness, and weight of the test piece are measured, and the weight is divided by the volume obtained from the length, width, and thickness to obtain the density of the composite sheet. In addition, the weight is divided by the area obtained from the length and width to obtain the basis weight of the composite sheet. Take out 5 test pieces, and obtain the density and basis weight of the 5 test pieces, respectively, and obtain their average value.

[0071] When the air permeability of the composite sheet is within the above range, the first polymer component is fully arranged on the outer surface of the fiber sheet and the inside of the fiber sheet (in the gap between the fibers), and the ESR is reduced. The air permeability of the composite sheet can be 5 seconds / 100mL or more and 50 seconds / 100mL or less (or 10 seconds / 100mL or less). When the air permeability of the composite sheet is less than 58 seconds / 100mL (or 50 seconds / 100mL or less), it is easy to ensure the impregnation of the electrolyte, etc.

[0072] Here, air permeability (air resistance) is an index that indicates the time (seconds) required for a predetermined volume (100 mL) of air to pass through per unit area of ​​the diaphragm when a predetermined pressure difference is applied between the two sides of the diaphragm. The air permeability is based on JIS P8117:2009, and is calculated by setting the test area (permeable portion) of the diaphragm to 6.42 cm 2 , and the inner cylinder weight was set to 567 g using a Gurley tester method. Note that the air permeability was measured after the separator was dried at 125° C. for 3 hours or more to fully remove the first dispersion medium remaining in the separator.

[0073] The first polymer component is attached to the surface of the fibers constituting the fiber sheet. The first polymer component is disposed on the outer surface of the fiber sheet and inside the fiber sheet (in the gaps between the fibers).

[0074] From the viewpoint of reducing ESR, the adhesion amount of the first polymer component may be, for example, 0.02 mg / cm 2 Above, it can also be 0.05mg / cm 2 Above and 2.0mg / cm 2 It should be noted that the attachment amount of the first polymer component means the mass of the first polymer component attached per unit area of ​​the fiber sheet. The mass of the first polymer component attached per unit area of ​​the fiber sheet does not change before and after the composite sheet is compressed.

[0075] The adhesion amount of the first polymer component can be determined by the following method.

[0076] First, five first samples are prepared by cutting a predetermined area from a fiber sheet before the first polymer component is attached, and the average mass of the five first samples is calculated. Also, five second samples are prepared by cutting a predetermined area from a fiber sheet to which the first polymer component is attached, and the average mass of the five second samples is calculated. The difference between the average mass of the five second samples and the average mass of the five first samples is divided by the predetermined area to calculate the mass of the first polymer component attached per unit area of ​​the fiber sheet.

[0077] The coverage brought by the first polymer component of the diaphragm can be 60% or more, preferably 90% or more. The coverage means the area ratio of the first polymer component in the main surface of the diaphragm when the diaphragm is observed from the normal direction of the main surface (outer surface) of the diaphragm. The coverage can be obtained by using an optical microscope to obtain an image of the diaphragm when it is observed from the normal direction of the main surface of the diaphragm, and the image is binarized and obtained. In addition, the coverage can also be obtained by using a scanning or transmission electron microscope to obtain an image of the diaphragm when it is observed from the normal direction of the main surface of the diaphragm, and using this image to perform element scanning imaging (Japanese: Mapping) of the elements contained in the first polymer component using energy dispersive X-ray spectroscopy (EDX) to obtain. In addition, the coverage can also be obtained by using an optical microscope to obtain an image of the diaphragm when it is observed from the normal direction of the main surface of the diaphragm, and performing Raman scanning imaging using a molecular structure spectrum based on Raman spectroscopy.

[0078] [Method for manufacturing electrolytic capacitor]

[0079] The manufacturing method of the electrolytic capacitor of the embodiment of the present invention includes the following steps: a step of preparing an anode foil; a step of preparing a cathode foil; a step of obtaining a diaphragm by the above-mentioned method of manufacturing a diaphragm for an electrolytic capacitor; a step of sandwiching the above-mentioned diaphragm between the anode foil and the cathode foil and stacking the anode foil and the cathode foil (hereinafter also referred to as a stacking step).

[0080] Through the lamination process, a laminated body (hereinafter also referred to as a capacitor element) having an anode foil, a cathode foil, and a separator sandwiched between the anode foil and the cathode foil is obtained. In this process, the laminated body can also be wound. In this case, the end of the cathode foil located at the outermost layer is fixed by a winding stop tape.

[0081] The anode foil and cathode foil may be cut to a predetermined size. In this case, the capacitor element may be further subjected to chemical conversion treatment (re-chemical conversion treatment) in order to form a dielectric layer on the end surface (cut surface) of the anode foil.

[0082] The preparation process of the anode foil and / or cathode foil may also include the process of attaching the first polymer component to the anode foil and / or cathode foil. More first polymer components can be included in the capacitor element. When the first polymer component is attached to the cathode foil and the fiber sheet, a sufficient amount of conductive polymer components can be maintained without hindering the self-repairing performance of the anode foil. When the first polymer component is attached to the anode foil and the fiber sheet, the adhesion between the dielectric layer formed on the surface of the anode foil and the first polymer component is improved, and the ESR can be further reduced. The method of attaching the first polymer component to the electrode foil is not particularly limited, and it can be impregnation or coating.

[0083] (Second polymer dispersion liquid impregnation step)

[0084] The manufacturing method may also include: impregnating the capacitor element with a second polymer dispersion containing a second conductive polymer component (hereinafter, also referred to as the second polymer component) and a second dispersion medium, and then performing a drying process to remove at least a portion of the second dispersion medium. In this way, the capacitor element may also contain a first polymer component and a second polymer component. By using the second polymer component, it can be expected that the electrostatic capacitance will be further increased and the ESR will be reduced. In the case where the first dispersion medium remains in the diaphragm, the second polymer dispersion is induced by the first dispersion medium and is easily impregnated into the diaphragm.

[0085] The second polymer component can adhere to the surface of the electrode foil and the diaphragm in the capacitor element. The second polymer component adheres to the first polymer component contained in the diaphragm. However, since the density of the diaphragm (fiber sheet) increases due to the second step, it is difficult for the particles of the second polymer component to enter the interior of the diaphragm (the gaps between the fibers) and they are easily attached to the outer surface of the diaphragm.

[0086] When the electrode foil has a porous portion on the surface, the particles of the second polymer component may enter the depressions of the porous portion. When the first polymer component is attached to the electrode foil, the second polymer component may be attached to the first polymer component.

[0087] (Second polymer dispersion)

[0088] The second polymer dispersion comprises a second polymer component and a second dispersion medium. As the second dispersion medium, the same compound as the first dispersion medium can be cited. The second polymer component can also comprise a conductive polymer and a dopant the same as the first polymer component. The second polymer component can also comprise a polyanion (hereinafter referred to as the second polyanion) as a dopant.

[0089] From the viewpoint of reducing ESR, the weight average molecular weight of the second polyanion contained in the second polymer component may be greater than the weight average molecular weight of the first polyanion contained in the first polymer component. From the viewpoint of compatibility with the first polymer component and the impregnation of the second polymer dispersion, the weight average molecular weight of the second polyanion contained in the second polymer component may also be less than the weight average molecular weight of the first polyanion contained in the first polymer component. The weight average molecular weight of the second polyanion may be, for example, 1000 or more and 200000 or less, or 10000 or more and 150000 or less.

[0090] The content of the second polymer component in the second polymer dispersion may be less than the content of the first polymer component in the first polymer dispersion. Specifically, the content of the second polymer component in the second polymer dispersion is preferably 0.5 mass % or more and less than 3 mass %. The viscosity of the second polymer dispersion is preferably lower than the viscosity of the first polymer dispersion. The viscosity of the second polymer dispersion is preferably less than 100 mPa·s.

[0091] (Liquid component impregnation step)

[0092] The manufacturing process may include a step of impregnating the capacitor element with a liquid component. When the first dispersion medium remains in the separator, the liquid component is guided by the first dispersion medium and easily impregnates the separator.

[0093] The infiltration process of the liquid component can also be performed after the formation of the capacitor element. For example, the capacitor element can be housed in a bottom shell, and then the liquid component can be injected into the bottom shell. The infiltration process of the liquid component can also be performed under reduced pressure (for example, an atmosphere with a gauge pressure of more than -30kPa and less than -90kPa). In the case of performing the infiltration process of the second polymer dispersion, the infiltration process of the liquid component can be performed after the infiltration process of the second polymer dispersion. Through the infiltration process of the liquid component, the liquid component adheres to the surface of the electrode foil and the diaphragm. The liquid component enters the interior of the diaphragm (in the gap between the fibers), and when the electrode foil has a porous portion on the surface, the liquid component enters the depression of the porous portion.

[0094] The liquid component may include an electrolyte containing a solvent and a solute. The liquid component may also include an acid component, and may also include an acid component and an alkali component. In addition, the liquid component may also include only a solvent (e.g., a polyol such as a diol compound). By including a liquid component in the capacitor element, the self-healing performance of the dielectric layer is improved. In addition, by including an electrolyte in the capacitor element, it is advantageous in terms of reducing ESR and increasing electrostatic capacitance.

[0095] (Electrolyte)

[0096] As the solvent contained in the electrolyte, sulfone compounds, lactone compounds, carbonate compounds, polyols, etc. can be mentioned. As sulfone compounds, cyclopentane, dimethyl sulfoxide and diethyl sulfoxide can be mentioned. As lactone compounds, γ-butyrolactone, γ-valerolactone, etc. can be mentioned. As carbonate compounds, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC) and fluoroethylene carbonate (FEC) can be mentioned. As polyols, glycol compounds such as ethylene glycol (EG), diethylene glycol, triethylene glycol, propylene glycol and polyethylene glycol (PEG); glycerol, etc. can be mentioned. These can be used alone or in combination.

[0097] The solvent may also contain a compound having two or more hydroxyl groups. Examples of such compounds include polyols. The content of the compound having two or more hydroxyl groups may be 50% by mass or more of the total solvent, 60% by mass or more, or 70% by mass or more.

[0098] The electrolyte may also contain an acid component. The acid component in the electrolyte inhibits dedoping of the dopant from the polymer component, stabilizing the conductivity of the polymer component. In addition, even if the dopant is dedoped from the polymer component, the acid component of the electrolyte is re-doped to the site of the dedoping trace, so it is easy to maintain a low ESR.

[0099] The acid component in the electrolyte preferably does not excessively increase the viscosity of the electrolyte, is easily dissociated in the electrolyte, and generates anions that are easily mobile in the solvent. As such an acid component, for example, aliphatic sulfonic acids with 1 to 30 carbon atoms and aromatic sulfonic acids with 6 to 30 carbon atoms can be cited. Among aliphatic sulfonic acids, monovalent saturated aliphatic sulfonic acids (such as hexylsulfonic acid) are preferred. Among aromatic sulfonic acids, aromatic sulfonic acids having a hydroxyl group or a carboxyl group in addition to a sulfonic group are preferred, specifically, oxyaromatic sulfonic acids (such as phenol-2-sulfonic acid) and sulfoaromatic carboxylic acids (such as p-sulfobenzoic acid, 3-sulfophthalic acid, 5-sulfosalicylic acid) are preferred.

[0100] As other acid components, carboxylic acids can be mentioned. Carboxylic acids preferably include aromatic carboxylic acids (aromatic dicarboxylic acids) having more than two carboxyl groups. As aromatic carboxylic acids, for example, phthalic acid (ortho-body), isophthalic acid (meta-body), p-phthalic acid (para-body), maleic acid, benzoic acid, salicylic acid, trimellitic acid, pyromellitic acid can be mentioned. Among them, aromatic dicarboxylic acids such as phthalic acid (ortho-body) and maleic acid are more preferred. The carboxyl group of aromatic dicarboxylic acids is stable and is not easy to react with side reactions. Thus, the effect of stabilizing the conductive polymer for a long time is shown, which is conducive to the long life of the electrolytic capacitor. In addition, the carboxylic acid can also be an aliphatic carboxylic acid such as adipic acid.

[0101] The acid component may include a composite compound of an organic acid and an inorganic acid from the viewpoint of thermal stability. As the composite compound of an organic acid and an inorganic acid, heat-resistant boron disalicylic acid, boron dioxalic acid, boron diglycolic acid, etc. may be cited. The acid component may also include inorganic acids such as boric acid, phosphoric acid, phosphorous acid, hypophosphorous acid, and phosphonic acid.

[0102] From the viewpoint of enhancing the effect of suppressing the dedoping phenomenon, the concentration of the acid component may be 5% by mass or more and 50% by mass or less, or 15% by mass or more and 35% by mass or less.

[0103] The electrolyte may contain an acid component and an alkali component. At least a portion of the acid component is neutralized by the alkali component. Thus, the concentration of the acid component can be increased, and the corrosion of the electrode caused by the acid component can be suppressed. From the viewpoint of effectively suppressing dedoping, it is preferred that the acid component is excessive in terms of equivalent ratio compared to the alkali component. For example, the equivalent ratio of the acid component to the alkali component can be greater than 1 and less than 30. The concentration of the alkali component contained in the electrolyte can be greater than 0.1 mass % and less than 20 mass %, or can be greater than 3 mass % and less than 10 mass %.

[0104] The base component is not particularly limited. Examples of the base component include ammonium, primary amines, secondary amines, tertiary amines, quaternary ammonium compounds, and amidinium compounds. Examples of the amines include aliphatic amines, aromatic amines, and heterocyclic amines.

[0105] The pH of the electrolyte is preferably 4 or less, more preferably 3.8 or less, and even more preferably 3.6 or less. By setting the pH of the electrolyte to 4 or less, the degradation of the polymer component is further suppressed. The pH is preferably 2.0 or more.

[0106] (Capacitor element sealing process)

[0107] The manufacturing method may include a process of sealing the capacitor element. For example, the capacitor element is housed in a bottom shell, and then a lateral necking process is performed near the open end of the bottom shell, the open end is chiseled to the sealing member and curled, and a seat plate may be arranged on the curled portion. By operating in this way, an electrolytic capacitor can be obtained. Then, the electrolytic capacitor can be aged while applying the rated voltage. As the material of the bottom shell, metals such as aluminum, stainless steel, copper, iron, brass, or their alloys can be used.

[0108] [Electrolytic capacitors]

[0109] The electrolytic capacitor of the embodiment of the present invention comprises an anode foil, a cathode foil, and a diaphragm sandwiched between the anode foil and the cathode foil. That is, it comprises a capacitor element. The diaphragm is the above-mentioned diaphragm for electrolytic capacitors. The capacitor element may be a laminate of an anode foil, a diaphragm, and a cathode foil, or a winding body formed by winding the laminate. The capacitor element may also include a first polymer component as an electrolyte, and may further include a second polymer component and / or an electrolyte. In addition, the capacitor element may also include a solvent (for example, a polyol such as a diol compound) instead of an electrolyte. The electrolytic capacitor may have one capacitor element or multiple capacitor elements.

[0110] (Anode Foil)

[0111] The anode foil comprises a metal foil containing a valve metal, and a dielectric layer covering the surface of the metal foil. Examples of the valve metal include titanium, tantalum, aluminum, and niobium. The metal foil may contain the valve metal in the form of an alloy containing the valve metal or a compound containing the valve metal. The thickness of the anode foil is, for example, greater than 15 μm and less than 300 μm. The surface of the metal foil is usually roughened by etching or the like. For example, the metal foil whose surface has been roughened is subjected to a chemical conversion treatment to form a dielectric layer. In this case, the dielectric layer may contain an oxide of the valve metal.

[0112] (Cathode Foil)

[0113] The cathode foil may be a metal foil containing a valve-acting metal. The thickness of the cathode foil is, for example, greater than 15 μm and less than 300 μm. The surface of the metal foil may also be roughened by etching or the like. A chemical conversion film may also be formed on the surface of the metal foil by chemical conversion treatment. The cathode foil may also be a metal foil having a coating layer on the surface. The coating layer is configured to improve corrosion resistance, reduce ESR, etc. The coating layer may also contain at least one of carbon and metal M. In the coating layer, metal M may also be contained in the form of metal oxide, metal nitride, and metal carbide. Metal M may, for example, contain at least one selected from nickel, titanium, tantalum, and zirconium.

[0114] Here, Figure 1 1 is a cross-sectional view schematically showing an electrolytic capacitor according to an embodiment of the present invention. Figure 2 This is a perspective view of a part of the rolled body unfolded.

[0115] The electrolytic capacitor 200 includes a winding body 100 as a capacitor element. The winding body 100 is composed of an anode foil 10 and a cathode foil 20 wound with a separator 30 interposed therebetween. For the separator 30, the above-mentioned separator for electrolytic capacitors can be used. The winding body 100 contains an electrolyte, and the electrolyte is sandwiched between the anode foil 10 (dielectric layer) and the cathode foil. The electrolyte contains a first polymer component and may further contain a second polymer component and / or an electrolyte solution.

[0116] Anode foil 10 and cathode foil 20 are connected to one end of lead tabs 50A and 50B, respectively, and lead tabs 50A and 50B are wound around to form wound body 100. Leads 60A and 60B are connected to the other ends of lead tabs 50A and 50B, respectively.

[0117] The outer surface of the cathode foil 20 located at the outermost layer of the wound body 100 is provided with a stopper tape 40, and the end of the cathode foil 20 is fixed by the stopper tape 40. It should be noted that when the anode foil 10 is prepared by cutting from a large foil, the wound body 100 may be further subjected to a chemical conversion treatment in order to provide a dielectric layer on the cut surface.

[0118] The electrolytic capacitor 200 includes a sealing member 212 that seals the opening of the bottom case 211, and a seat plate 213 that covers the sealing member 212. The wound body 100 is housed in the bottom case 211 in such a manner that the leads 60A and 60B are located on the opening side of the bottom case 211. The leads 60A and 60B are led out from the sealing member 212 and pass through the seat plate 213. As a material for the bottom case 211, a metal such as aluminum, stainless steel, copper, iron, brass, or an alloy thereof can be used.

[0119] A sealing member 212 is disposed at the opening of the bottomed case 211 containing the wound body 100, the open end of the bottomed case 211 is riveted to the sealing member 212 and curled, and a seat plate 213 is disposed at the curled portion to seal the wound body 100 in the bottomed case 211. The sealing member 212 can be any insulating material, preferably an elastomer. Preferably, a material having excellent heat resistance, such as silicone rubber or fluororubber, is used.

[0120] Example

[0121] [Example]

[0122] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0123] 《Examples 1 to 7, Comparative Examples 6 to 7》>

[0124] Use the following method to make an electrolytic capacitor with a rated voltage of 35V.

[0125] (Fiber sheet preparation)

[0126] A fiber sheet (thickness: 60 μm) having a density shown in Table 1 was prepared. A nonwoven fabric containing cellulose fibers was used as the fiber sheet.

[0127] (Preparation of the first polymer dispersion)

[0128] 3,4-ethylenedioxythiophene and polystyrene sulfonic acid (PSS, weight average molecular weight 100,000) were dissolved in ion exchange water to prepare a mixed solution. Iron (III) sulfate (oxidant) was added while stirring the mixed solution to carry out a polymerization reaction. Then, the reaction solution was dialyzed to remove unreacted monomers and oxidants to obtain a first polymer dispersion containing polyethylenedioxythiophene (PEDOT / PSS, the first polymer component) doped with PSS (dopant). The concentration of the first polymer component in the first polymer dispersion was 2% by mass. The viscosity of the first polymer dispersion was 40 mPa·s.

[0129] (Step of applying the first polymer dispersion to the fiber sheet: first step)

[0130] The first polymer dispersion was applied to both sides of the fiber sheet using a gravure coater. Then, a drying process was performed to obtain a composite sheet (thickness T0: 60 μm) in which the first polymer component was attached to the fiber sheet. The mass of the first polymer component attached to each unit area of ​​the fiber sheet was 0.3 mg / cm 2 The area coverage of one main surface of the fiber sheet by the first polymer component was 98%. The fiber sheet was dried at 105° C. for 2 hours under atmospheric pressure.

[0131] (Compression step of composite sheet: second step)

[0132] The composite sheet is rolled to obtain a diaphragm. In this case, the pressing pressure is adjusted so that the thickness T1 of the pressed composite sheet (diaphragm) is the value shown in Table 1. The density, basis weight, and air permeability of the diaphragm obtained by the method already described are the values ​​shown in Table 1. The conductivity of the diaphragm (composite sheet after pressing) is 1.0 mS / cm. By operating in this way, diaphragms a1 to a7 and b6 to b7 of Examples 1 to 7 and Comparative Examples 6 to 7 are obtained.

[0133] [Table 1]

[0134]

[0135] (Fabrication of capacitor elements)

[0136] The anode lead connector and the cathode lead connector are connected to the anode foil and the cathode foil, and the anode foil and the cathode foil are wound with the lead connector wound in. It should be noted that for the anode foil, a foil obtained by cutting an etched foil having a dielectric layer on the surface into a specified size is used. The etched foil is obtained by etching an aluminum foil (thickness 100 μm). The dielectric layer is formed by chemically converting the surface of the etched foil. For the cathode foil, a foil obtained by cutting an etched foil obtained by etching an aluminum foil (thickness 50 μm) into a specified size is used.

[0137] The ends of each lead connector protruding from the winding body are connected to the anode lead and the cathode lead, respectively. The obtained winding body is chemically converted again to form a dielectric layer on the end surface of the anode foil. The end of the outer surface of the winding body is fixed with a stop tape. By operating in this way, a capacitor element is obtained.

[0138] (Impermeation of electrolyte)

[0139] After the capacitor element is housed in the bottomed case, an electrolyte is injected into the capacitor element in the bottomed case at room temperature under atmospheric pressure. This operation is performed so that the electrolyte is impregnated into the capacitor element. For the electrolyte, an electrolyte in which triethylamine phthalate is dissolved in a solvent having ethylene glycol as the main component is used.

[0140] (Sealing of capacitor elements)

[0141] A sealing member and a seat plate are arranged at the opening of the bottom shell to seal the capacitor element. The electrolytic capacitor is completed by operating in this way. Then, an aging treatment is performed at 105°C for 2 hours while applying the rated voltage. The electrolytic capacitors A1 to A7 and B6 to B7 of Examples 1 to 7 and Comparative Examples 6 to 7 are obtained by operating in this way.

[0142] Comparative Example 1 >>

[0143] The second step (compression step of the composite sheet) was not performed, and the composite sheet obtained in the first step was used as the separator b1. The electrolytic capacitor B1 of Comparative Example 1 was obtained in the same manner as in Example 1 except that the separator b1 was used instead of the separator a1.

[0144] The density, basis weight, and air permeability of the separator b1 were the values ​​shown in Table 1. The mass of the first polymer component per unit area of ​​the fiber sheet was 0.3 mg / cm 2 The area coverage of one main surface of the fiber sheet with the first polymer component was 98%.

[0145] Comparative Examples 2 to 5>>

[0146] The first step was performed in the same manner as in Example 1, except that a fiber sheet having a thickness and density shown in Table 1 was prepared, and the second step (compression step of the composite sheet) was not performed. The composite sheets obtained in the first step were used as separators b2 to b5. The electrolytic capacitors B2 to B5 of Comparative Examples 2 to 5 were obtained in the same manner as in Example 1, except that separators b2 to b5 were used instead of separator a1.

[0147] The density, basis weight, and air permeability of the separators b2 to b5 were the values ​​shown in Table 1. The mass of the first polymer component per unit area of ​​the fiber sheet was 0.3 mg / cm 2 The area coverage of the first polymer component on one main surface of the fiber sheet was 98%.

[0148] [evaluate]

[0149] The following evaluations were performed on each electrolytic capacitor.

[0150] (ESR measurement)

[0151] The ESR (Ω) of the electrolytic capacitor at a frequency of 100 kHz was measured in an environment of 20° C. The number of measurements was set to 100, and the average value thereof was calculated.

[0152] (Evaluation of short-circuit resistance)

[0153] In an environment of 20°C, the rated voltage is applied to the electrolytic capacitor, and the current value after 120 seconds is measured. If the current value is 1.0 mA or more, it is judged as a short-circuited product. The number of measurements is set to 100, and the ratio of the number of short-circuited products to the number of measurements is calculated as the short-circuit occurrence rate (%).

[0154] The evaluation results are shown in Table 2. In Table 2, A1 to A7 and B6 to B7 are electrolytic capacitors having separators a1 to a7 and b6 to b7, respectively. In Table 2, B1 to B5 are electrolytic capacitors having separators b1 to b5, respectively.

[0155] [Table 2]

[0156]

[0157] The electrolytic capacitors A1 to A7 had low ESR and good short-circuit resistance. Among them, the electrolytic capacitors A2 to A5 (particularly A3 to A5) had low ESR and excellent short-circuit resistance.

[0158] For electrolytic capacitor B1, the density of the composite sheet (fiber sheet) is small and the short-circuit resistance is poor. For electrolytic capacitors B2, B5 to B7, the amount of polymer components attached to the high-density fiber sheet is small and the ESR is increased. The diaphragms b3 and b4 obtained in Comparative Examples 3 and 4 have the same density and thickness as the fiber sheets of diaphragms a2 and a4 obtained in Examples 2 and 4, respectively, but are smaller in density and basis weight than diaphragms a2 and a4, and the amount of polymer components attached to the fiber sheet is small. Therefore, the ESR of electrolytic capacitors B3 and B4 is increased compared to electrolytic capacitors A2 and A4.

[0159] Industrial Applicability

[0160] The electrolytic capacitor separator of the present invention can be suitably used for an electrolytic capacitor that is required to have excellent short-circuit resistance and low ESR.

[0161] Although the present invention has been described with respect to the present preferred embodiments, it should not be limited to such disclosure. Upon reading the above disclosure, various modifications and changes will undoubtedly be apparent to those skilled in the art of the art to which the present invention belongs. Therefore, the scope of the additional claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention.

[0162] Description of Reference Numerals

[0163] 10: anode foil, 20: cathode foil, 30: separator, 40: anti-winding tape, 50A, 50B: lead terminals, 60A, 60B: lead wires, 100: winding body, 200: electrolytic capacitor, 211: bottom case, 212: sealing member, 213: seat plate

Claims

1. A method for manufacturing a diaphragm for an electrolytic capacitor, comprising the following steps: A first step of attaching a conductive polymer component to a fiber sheet to obtain a composite sheet; and A second step of compressing the composite sheet to obtain a separator, The density of the composite sheet before compression is less than 0.60 g / cm 3 .

2. The method for producing a diaphragm for an electrolytic capacitor according to claim 1, wherein: The first step includes the following steps: a step of preparing a conductive polymer dispersion liquid containing the conductive polymer component and a dispersion medium; as well as A step of applying the conductive polymer dispersion liquid to the fiber sheet or impregnating the fiber sheet with the conductive polymer dispersion liquid and then removing at least a portion of the dispersion medium.

3. The method for producing a diaphragm for an electrolytic capacitor according to claim 1 or 2, wherein: The density of the fiber sheet before compression is 0.58 g / cm 3 the following.

4. The method for producing a diaphragm for an electrolytic capacitor according to any one of claims 1 to 3, wherein: In the second step, the composite sheet is roll-pressed.

5. The method for producing a diaphragm for an electrolytic capacitor according to any one of claims 1 to 4, wherein: A ratio of a thickness T1 of the composite sheet after compression to a thickness T0 of the composite sheet before compression: T1 / T0 is greater than or equal to 0.50 and less than or equal to 0.

95.

6. The method for producing a diaphragm for an electrolytic capacitor according to any one of claims 1 to 5, wherein: The fiber sheet contains at least cellulose fibers.

7. The method for producing a diaphragm for an electrolytic capacitor according to claim 6, wherein: The fiber sheet comprises the cellulose fibers and synthetic fibers.

8. A method for manufacturing an electrolytic capacitor, comprising the following steps: The process of preparing anode foil; The process of preparing cathode foil; A step of obtaining a diaphragm by the method for producing a diaphragm for an electrolytic capacitor according to any one of claims 1 to 7; and A step of laminating the anode foil and the cathode foil with the separator interposed between the anode foil and the cathode foil.

9. A diaphragm for an electrolytic capacitor, comprising a composite sheet comprising a fiber sheet and a conductive polymer component attached to the fiber sheet, The composite sheet has: 0.33g / cm 3 Above and less than 0.74g / cm 3 density, air permeability of 0.5 sec / 100 mL or more and less than 58 sec / 100 mL, and 19.0×10 -4 g / cm 2 Basis weight above.

10. The diaphragm for electrolytic capacitor according to claim 9, wherein The thickness T1 of the composite sheet is greater than or equal to 20 μm and less than or equal to 90 μm.

11. An electrolytic capacitor comprising an anode foil, a cathode foil, and a separator interposed between the anode foil and the cathode foil, The separator is the separator for an electrolytic capacitor according to claim 9 or 10.