Air filter element with lasting fragrance and preparation method of air filter element

By using fixed frame structure and semi-degradable water-based coating in the air filter element to coat the aromatherapy particles, forming a microporous structure, the problem of insufficient fragrance durability is solved, the slow release of fragrance and the long-lasting fragrance effect is achieved, and the air filter element is extended Service life and reduce production costs.

CN118925359APending Publication Date: 2024-11-12DONGGUAN AIR GUARD FILTER MANUFACTURING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411152907.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing car-mounted aroma air filter has insufficient fragrance durability and needs to be replaced frequently, which cannot effectively maintain a comfortable fragrance environment in the car.

Method used

Using a fixed frame structure, combined with the PET short fiber primary filter layer, meltblown PP layer, honeycomb carrier and second mesh cover, the honeycomb carrier is filled with activated carbon particles and aromatherapy particles, and the aromatherapy particles are coated with semi-degradable water-based coating to form micro Pore ​​structure to delay fragrance release.

Benefits of technology

It achieves the slow release of fragrance and lasting fragrance effect, extends the service life of the air filter element, avoids frequent replacement, and is simple in preparation and low in cost, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925359A_ABST
    Figure CN118925359A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of air filter elements, in particular to a lasting fragrance-retaining air filter element and a preparation method thereof.The air filter element comprises a fixed frame, a PET short fiber primary filter layer, a melt-blown PP layer, a first mesh enclosure, a honeycomb carrier and a second mesh enclosure, and the PET short fiber primary filter layer, the melt-blown PP layer, the first mesh enclosure, the honeycomb carrier and the second mesh enclosure are fixedly arranged in the fixed frame and sequentially bonded; honeycomb holes of the honeycomb carrier are filled with a plurality of activated carbon particles and a plurality of aromatherapy particles; the aromatherapy particles are composed of particle bodies and film layers wrapping the particle bodies, the film layers are formed by coating the surfaces of the particle bodies with semi-degradable water-based paint at least twice and then drying the semi-degradable water-based paint, the whole fragrance retention process lasts for 5-7 months, the more lasting fragrance retention effect is achieved, and frequent replacement of the air filter element due to short-term fragrance loss is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of air filter elements, and in particular to a long-lasting fragrance-retaining air filter element and a preparation method thereof. Background Art

[0002] When a car is driving, it usually inhales outside air into the car, but the outside air contains many different particles, such as dust, pollen, soot, abrasive particles, ozone, odor, nitrogen oxides, sulfur dioxide, carbon dioxide, benzene, etc. The air filter can separate solid impurities such as dust, pollen, and abrasive particles in the air, and can absorb moisture, soot, ozone, odor, carbon oxides, SO2, CO2, etc. in the air, playing a good protective role. For general urban family cars, the air filter is usually replaced once every six months.

[0003] The car aromatherapy air filter is a car product that combines air filtration and aromatherapy functions. It can improve the air quality in the car and provide a lasting fragrance. It attaches aroma molecules to the filter element and allows the air to enter the car, filling the entire car with fragrance. This product not only helps improve the air quality in the car and reduce odor, but also improves driving comfort.

[0004] However, since the fragrance of the aromatherapy filter will gradually weaken, the fragrance of the aromatherapy filter on the market is not long-lasting enough. Even if fragrance is added to the filter, the fragrance will usually be completely lost after 3 months of use, so it needs to be replaced frequently every 3 months. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide an air filter element with a long-lasting fragrance, and the fragrance of the air filter element is more lasting during actual use.

[0006] Another object of the present invention is to provide a method for preparing a long-lasting fragrance air filter element, which is simple to operate, convenient to control, high in production efficiency, low in production cost, and can be used for large-scale production.

[0007] The purpose of the present invention is achieved through the following technical scheme: a long-lasting fragrance air filter element, comprising a fixed frame, and a PET short fiber primary filter layer, a melt-blown PP layer, a first mesh cover, a honeycomb carrier and a second mesh cover, which are all fixedly installed in the fixed frame and bonded in sequence, and the honeycomb holes of the honeycomb carrier are filled with a plurality of activated carbon particles and a plurality of aromatherapy particles; the aromatherapy particles are composed of a particle body and a film layer coated on the particle body, and the film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body at least twice and then drying it.

[0008] The long-lasting fragrance air filter element of the present invention uses a fixed frame to fix the PET short fiber primary filter layer, the melt-blown PP layer, the first mesh cover, the honeycomb carrier and the second mesh cover. The PET short fiber primary filter layer, the melt-blown PP layer and the honeycomb carrier filled with activated carbon particles perform air filtration in sequence to ensure the filtering effect of the air filter element itself. The honeycomb holes of the honeycomb carrier are also filled with a number of aromatherapy particles, and the particle bodies of the aromatherapy particles are coated with a film layer to block the fragrance essential oils in the particle bodies to prevent the high concentration of fragrance essential oils from quickly diffusing and losing fragrance. In the initial stage of use when installed in the air filtration position of the automobile air conditioner, the intermolecular diffusion of the aromatherapy particles is used to slowly emit fragrance. A reasonable number of aromatherapy particles is conducive to ensuring that the space inside the car is slowly released in trace amounts and obtaining a fragrance concentration that is more comfortable for the human body. After the air filter element is used for 2-4 months, due to the particles The content of essential oil in the main body itself becomes less, and the diffusion effect of releasing fragrance through low-concentration essential oil molecules is reduced. The film layer is formed by coating the semi-degradable water-based paint on the surface of the particle body at least twice and then drying. At this time, the dried film layer of the semi-degradable water-based paint is affected by environmental microorganisms, temperature and humidity. The film layer is semi-degraded to form a microporous structure, that is, a channel for releasing fragrance is formed, allowing the essential oil to diffuse to maintain the fragrance. As time goes by, after the air filter element continues to be used for 1-2 months, the content of essential oil in the particle body itself is even less, and the microporous structure formed by the semi-degradation of the film layer is larger and more numerous, that is, the channels for releasing fragrance are larger and more numerous, so as to maintain the release of the lower concentration of essential oil in the particle body itself until the fragrance is lost. The entire fragrance retention process lasts for 5-7 months, achieving a more lasting fragrance retention effect and avoiding frequent replacement of the air filter element due to short-term loss of fragrance.

[0009] Preferably, the thickness of the film layer is 0.5-1.0 mm; in the honeycomb holes, the activated carbon particles and the aromatherapy particles are mixed in a weight ratio of 2:3-5.

[0010] By adopting the above technical scheme, the semi-degradable water-based paint is coated on the surface of the particle body at least twice to increase the thickness of the film layer, and the film layer thickness is controlled at 0.5-1.0mm, thereby improving the diffusion barrier effect of the essential oil of the particle body and avoiding the rapid diffusion of high-concentration essential oil and the loss of fragrance; the activated carbon particles and the aromatherapy particles are controlled to be mixed in a weight ratio of 2:3-5, and at the same time, affected by the barrier effect of the film layer thickness, it is more conducive to ensuring that the overall fragrance of the air filter element is moderate in the initial use.

[0011] Preferably, the particle body comprises the following components in parts by weight:

[0012] Ethylene-vinyl acetate copolymer 60-70 parts

[0013] 30-40 parts of perlite powder loaded with essential oil

[0014] 1-3 parts of lubricating dispersant

[0015] 1-3 parts of colorant.

[0016] By adopting the above technical scheme, the particle body uses ethylene-vinyl acetate copolymer as the main matrix, and under the action of the lubricating dispersant, the perlite powder loaded with the essential oil and the colorant are evenly dispersed in the particle body. On the one hand, the ethylene-vinyl acetate copolymer is used to cover most of the perlite powder loaded with the essential oil to avoid the rapid diffusion of the high concentration of the essential oil and the loss of fragrance. On the other hand, the perlite powder is used as a carrier to adsorb a large amount of essential oil, further avoiding the rapid diffusion of the high concentration of the essential oil and the loss of fragrance, and fully utilizing the intermolecular diffusion to slowly release the fragrance, so as to avoid the high concentration of the essential oil in the air filter element When it is initially used, it is not conducive to long-lasting fragrance due to the rapid diffusion, and at the same time, it is avoided that the high concentration of fragrance causes human discomfort.

[0017] Preferably, the density of the ethylene-vinyl acetate copolymer is 0.94-0.96 g / cm 3 , the melting temperature is 45-66°C; the perlite powder loaded with essential oil is mixed with essential oil and perlite powder in a weight ratio of 5-7:4-5.

[0018] By adopting the above technical scheme, ethylene-vinyl acetate copolymer with a melting temperature of 45-66°C is selected so that when preparing the particle body, a lower melting extrusion temperature is used for extrusion granulation to avoid excessive temperature, which accelerates the volatilization of the essential oil, increases the loss of the essential oil and reduces the fragrance retention effect, which is beneficial to reducing production costs and saving energy. The essential oil and perlite powder are controlled to be mixed in a weight ratio of 5-7:4-5, and the microporous adsorption characteristics of the perlite powder are used to adsorb the essential oil, thereby improving the reasonable utilization rate of the perlite powder and the essential oil, and improving the lasting fragrance retention effect of the aromatherapy particles. Furthermore, the model of the ethylene-vinyl acetate copolymer includes but is not limited to Arkema EVATANE42-60, EA33045 or Hanwha 1529; the particle size of the perlite micropowder is 10-30 μm; the category of the essential oil includes but is not limited to at least one of bergamot essential oil, lemon essential oil, lavender essential oil, jasmine essential oil, rose essential oil, ylang-ylang essential oil, citronella essential oil, peppermint essential oil, cedar essential oil or eucalyptus essential oil, more preferably, the essential oil is lemon essential oil.

[0019] Preferably, the lubricating dispersant is pentaerythritol stearate and / or carboxymethyl cellulose; and the colorant is at least one of titanium dioxide, carbon black, mica powder, yellow iron oxide or red iron oxide.

[0020] Adopting the above technical scheme, more preferably, the lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1, and the two act synergistically, which is more conducive to the uniform dispersion of the perlite powder and colorant loaded with the essential oil. Pentaerythritol stearate is conducive to maintaining the dispersed state of the solid particles, and the unique network structure of carboxymethyl cellulose becomes an excellent carrier for loading perlite powder and colorant, so that the perlite powder and colorant can be evenly and stably dispersed on the carrier, which can not only make the perlite powder and colorant well dispersed in the ethylene-vinyl acetate copolymer matrix, avoid the agglomeration of perlite powder and colorant, and improve the dispersion degree of perlite powder and colorant in the particle body, but also be more conducive to the sustained release of the essential oil and lasting fragrance.

[0021] Preferably, the preparation method of the particle body comprises the following steps: ethylene-vinyl acetate copolymer, perlite powder loaded with essential oil, lubricating dispersant and colorant are uniformly mixed by weight, and then extruded and granulated through a twin-screw extruder to obtain a particle body; wherein the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are respectively: 45-55°C, 55-65°C, 65-75°C, 65-80°C, 60-75°C, the head temperature is 60-75°C, the screw aspect ratio is 25:1, and the screw speed is 60-150r / min.

[0022] By adopting the above technical scheme, extrusion granulation is performed at a lower melt extrusion temperature, so as to avoid excessively high temperature which accelerates the volatilization of the essential oil, resulting in increased loss of the essential oil and reduced fragrance retention effect, which is beneficial to reducing production costs and saving energy.

[0023] Preferably, the semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0024]

[0025]

[0026] The above technical scheme is adopted, the semi-degradable water-based paint uses water-based acrylic resin and water-based polyurethane resin as the main resin, and polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water are added. The semi-degradable water-based paint has film-forming barrier and semi-degradation effects after curing. Among them, polylactic acid is fully mixed with other components and then coated to form a uniform film layer. When initially used, the air filter element has a good air filtration effect. After a period of use, due to the presence of dust, microorganisms, etc. in the air, there are cases where microorganisms are attached to the air filter element. Affected by environmental microorganisms, temperature and humidity, polylactic acid gradually degrades, thereby causing the film layer to semi-degrade to form a microporous structure, that is, to form a channel for releasing fragrance, so that the fragrance essential oil can diffuse to maintain the fragrance.

[0027] Preferably, the water-based acrylic resin is NeocryI XK-540 or DB3618; the water-based polyurethane resin is PU-3486 or H-34P; the average molecular weight of the polylactic acid is 30,000-50,000, and the molecular weight distribution is between 10,000-60,000.

[0028] The above technical scheme is adopted, wherein the average molecular weight of polylactic acid is controlled to be 30,000-50,000 and the molecular weight distribution is between 10,000-60,000, so that the polylactic acid with a lower molecular weight can be completely degraded in a shorter time to form local micropores for releasing fragrance, and the polylactic acid with a higher molecular weight is then completely degraded. The micropore structure formed by semi-degradation of the membrane layer is larger and more numerous, that is, the channels for releasing fragrance are larger and more numerous, so as to maintain the release of the lower concentration of essential oil in the particle body itself until the fragrance is lost. The entire fragrance retention process lasts for 6-7 months, achieving a more lasting fragrance retention effect, and avoiding the frequent replacement of the air filter element due to short-term loss of fragrance.

[0029] Preferably, the dispersant is BYK-190 or BYK192; the defoamer is BYK-028; the wetting agent is BASF WE3229 or TEGO WET280; the thickener is at least one of sodium carboxymethyl cellulose, propylene glycol alginate or sodium carboxymethyl starch; the film-forming aid is dipropylene glycol butyl ether or diethylene glycol monobutyl ether; and the cosolvent is isopropanol and / or ethanol.

[0030] More preferably, the preparation method of the semi-degradable water-based coating comprises the following steps:

[0031] (R1), taking water-based acrylic resin, water-based polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water by weight, and set aside;

[0032] (R2), adding polylactic acid to the cosolvent and mixing evenly to obtain a premixed solution;

[0033] (R3) Add water-based acrylic resin, water-based polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer into deionized water and mix evenly, then add thickener and film-forming aid and mix evenly to obtain semi-degradable water-based coating.

[0034] Another object of the present invention is achieved by the following technical solution: The preparation method of the above-mentioned long-lasting fragrance air filter element comprises the following steps:

[0035] (S1), bonding the PET staple fiber primary filter layer, the melt-blown PP layer, the first mesh cover, and the honeycomb carrier in sequence to form a multi-layer structure, and then bonding the outer periphery of the multi-layer structure to the inner wall of the fixed frame to obtain a semi-finished filter element;

[0036] (S2) After filling a plurality of activated carbon particles and a plurality of aroma particles into the honeycomb holes of the honeycomb carrier, a second mesh cover is bonded to a side of the honeycomb carrier away from the first mesh cover, and a long-lasting fragrance air filter element is obtained after packaging.

[0037] Wherein, in the honeycomb holes of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3-5.

[0038] The beneficial effects of the present invention are as follows: the long-lasting fragrance air filter element of the present invention uses a fixed frame to fix the PET short fiber primary filter layer, the melt-blown PP layer, the first mesh cover, the honeycomb carrier and the second mesh cover; the PET short fiber primary filter layer, the melt-blown PP layer and the honeycomb carrier filled with activated carbon particles perform air filtration in sequence to ensure the filtering effect of the air filter element itself; the honeycomb holes of the honeycomb carrier are also filled with a number of aromatherapy particles, and the particle body of the aromatherapy particles is coated with a film layer to block the fragrance essential oil of the particle body to prevent the high concentration of fragrance essential oil from quickly diffusing and losing the fragrance; in the initial stage of use when installed in the air filtration position of the automobile air conditioner, the intermolecular diffusion of the aromatherapy particles is used to slowly emit the fragrance; and a reasonable number of the fragrance particles is conducive to ensuring that the space inside the car is slowly released in trace amounts and obtaining a fragrance concentration that is more comfortable for the human body. After the air filter element is used for 2-4 months As the content of essential oil in the particle body itself decreases, the diffusion effect of releasing fragrance through low-concentration essential oil molecules is reduced. The film layer is formed by coating the surface of the particle body with semi-degradable water-based paint at least twice and then drying. At this time, the dried film layer of the semi-degradable water-based paint is affected by environmental microorganisms, temperature and humidity. The film layer semi-degrades to form a microporous structure, that is, a channel for releasing fragrance is formed, allowing the essential oil to diffuse to maintain the fragrance. As time goes by, after the air filter element continues to be used for 1-2 months, the content of essential oil in the particle body itself is even lower, and the microporous structure formed by the semi-degradation of the film layer is larger and more numerous, that is, the channels for releasing fragrance are larger and more numerous, so as to maintain the release of the lower concentration of essential oil in the particle body itself until the fragrance is lost. The entire fragrance retention process lasts for 6-7 months, achieving a more lasting fragrance retention effect and avoiding frequent replacement of the air filter element due to short-term loss of fragrance.

[0039] The preparation method of the invention has the advantages of simple operation, convenient control, high production efficiency and low production cost, and can be used for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the structure of the present invention;

[0041] Figure 2 is a SEM morphology image of the initial aromatherapy particles of Example 1 of the present invention;

[0042] Figure 3is a SEM morphology picture of the aromatherapy particles after being used for 3 months in Example 1 of the present invention;

[0043] Figure 4 This is a SEM morphology picture of the aromatherapy particles of Example 1 of the present invention after being used for 5 months.

[0044] The figures are marked as follows: 1. fixed frame; 2. PET short fiber primary filter layer; 3. melt-blown PP layer; 4. first mesh cover; 5. honeycomb carrier; 6. second mesh cover; 7. activated carbon particles; 8. aromatherapy particles. DETAILED DESCRIPTION

[0045] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments and drawings. The contents mentioned in the implementation modes are not intended to limit the present invention.

[0046] Example 1

[0047] like Figure 1 As shown, a long-lasting fragrance air filter element includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5 and a second mesh cover 6, which are all fixedly installed in the fixed frame 1 and bonded in sequence, and the honeycomb holes of the honeycomb carrier 5 are filled with a plurality of activated carbon particles 7 and a plurality of aroma particles 8; the aroma particles 8 are composed of a particle body and a film layer coated on the particle body, and the film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body twice and then drying it.

[0048] The thickness of the membrane layer is 0.6 mm; in the honeycomb holes of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:4.

[0049] The particle body comprises the following components in parts by weight:

[0050]

[0051] The perlite powder loaded with essential oil is mixed with the essential oil and the perlite powder in a weight ratio of 6:4.5. The particle size of the perlite powder is 20 μm; and the essential oil is lemon essential oil.

[0052] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; and the colorant is red iron oxide.

[0053] The preparation method of the particle body comprises the following steps: uniformly mixing ethylene-vinyl acetate copolymer EA33045, perlite powder loaded with essential oil, a lubricating dispersant and a colorant by weight, extruding and granulating through a twin-screw extruder to obtain the particle body; wherein the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are respectively 50°C, 60°C, 70°C, 75°C and 65°C, the head temperature is 62°C, the screw aspect ratio is 25:1, and the screw speed is 120r / min.

[0054] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0055]

[0056] The water-based acrylic resin is NeoCryI XK-540; the water-based polyurethane resin is PU-3486; the average molecular weight of the polylactic acid is 40,000, and the molecular weight distribution is between 10,000 and 60,000.

[0057] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0058] The preparation method of the semi-degradable water-based coating comprises the following steps:

[0059] (R1), taking water-based acrylic resin, water-based polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water by weight, and set aside;

[0060] (R2), adding polylactic acid to the cosolvent and mixing evenly to obtain a premixed solution;

[0061] (R3) Add water-based acrylic resin, water-based polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer into deionized water and mix evenly, then add thickener and film-forming aid and mix evenly to obtain semi-degradable water-based coating.

[0062] The method for preparing the long-lasting fragrance air filter element comprises the following steps:

[0063] (S1), bonding the PET staple fiber primary filter layer 2, the melt-blown PP layer 3, the first mesh cover 4, and the honeycomb carrier 5 in sequence to form a multi-layer structure, and then bonding the outer periphery of the multi-layer structure to the inner wall of the fixed frame 1 to obtain a semi-finished filter element;

[0064] (S2) After filling a plurality of activated carbon particles 7 and a plurality of aroma particles 8 into the honeycomb holes of the honeycomb carrier 5, the second mesh cover 6 is bonded to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after packaging, a long-lasting fragrance air filter element is obtained.

[0065] Example 2

[0066] like Figure 1 As shown, a long-lasting fragrance air filter element includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5 and a second mesh cover 6, which are all fixedly installed in the fixed frame 1 and bonded in sequence, and the honeycomb holes of the honeycomb carrier 5 are filled with a plurality of activated carbon particles 7 and a plurality of aroma particles 8; the aroma particles 8 are composed of a particle body and a film layer coated on the particle body, and the film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body twice and then drying it.

[0067] The thickness of the membrane layer is 0.5 mm; in the honeycomb holes of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3.

[0068] The particle body comprises the following components in parts by weight:

[0069]

[0070] The perlite powder loaded with essential oil is prepared by mixing the essential oil and the perlite powder in a weight ratio of 5:5. The particle size of the perlite powder is 10 μm; and the essential oil is lemon essential oil.

[0071] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; and the colorant is red iron oxide.

[0072] The preparation method of the particle body comprises the following steps: uniformly mixing ethylene-vinyl acetate copolymer EA33045, perlite powder loaded with essential oil, a lubricating dispersant and a colorant by weight, extruding and granulating through a twin-screw extruder to obtain the particle body; wherein the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are respectively 50°C, 60°C, 70°C, 75°C and 65°C, the head temperature is 62°C, the screw aspect ratio is 25:1, and the screw speed is 120r / min.

[0073] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0074]

[0075] The water-based acrylic resin is NeoCryI XK-540; the water-based polyurethane resin is PU-3486; the average molecular weight of the polylactic acid is 30,000, and the molecular weight distribution is between 10,000 and 60,000.

[0076] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0077] The preparation method of the semi-degradable water-based coating comprises the following steps:

[0078] (R1), taking water-based acrylic resin, water-based polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water by weight, and set aside;

[0079] (R2), adding polylactic acid to the cosolvent and mixing evenly to obtain a premixed solution;

[0080] (R3) Add water-based acrylic resin, water-based polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer into deionized water and mix evenly, then add thickener and film-forming aid and mix evenly to obtain semi-degradable water-based coating.

[0081] The method for preparing the long-lasting fragrance air filter element comprises the following steps:

[0082] (S1), bonding the PET staple fiber primary filter layer 2, the melt-blown PP layer 3, the first mesh cover 4, and the honeycomb carrier 5 in sequence to form a multi-layer structure, and then bonding the outer periphery of the multi-layer structure to the inner wall of the fixed frame 1 to obtain a semi-finished filter element;

[0083] (S2) After filling a plurality of activated carbon particles 7 and a plurality of aroma particles 8 into the honeycomb holes of the honeycomb carrier 5, the second mesh cover 6 is bonded to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after packaging, a long-lasting fragrance air filter element is obtained.

[0084] Example 3

[0085] like Figure 1As shown, a long-lasting fragrance air filter element includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5 and a second mesh cover 6, which are all fixedly installed in the fixed frame 1 and bonded in sequence, and the honeycomb holes of the honeycomb carrier 5 are filled with a plurality of activated carbon particles 7 and a plurality of aroma particles 8; the aroma particles 8 are composed of a particle body and a film layer coated on the particle body, and the film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body twice and then drying it.

[0086] The thickness of the membrane layer is 1.0 mm; in the honeycomb holes of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:5.

[0087] The particle body comprises the following components in parts by weight:

[0088]

[0089]

[0090] The perlite powder loaded with essential oil is prepared by mixing the essential oil and the perlite powder in a weight ratio of 7:5. The particle size of the perlite powder is 30 μm; and the essential oil is lemon essential oil.

[0091] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; and the colorant is red iron oxide.

[0092] The preparation method of the particle body comprises the following steps: uniformly mixing ethylene-vinyl acetate copolymer EA33045, perlite powder loaded with essential oil, a lubricating dispersant and a colorant by weight, extruding and granulating through a twin-screw extruder to obtain the particle body; wherein the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are respectively 50°C, 60°C, 70°C, 75°C and 65°C, the head temperature is 62°C, the screw aspect ratio is 25:1, and the screw speed is 120r / min.

[0093] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0094]

[0095] The water-based acrylic resin is NeoCryI XK-540; the water-based polyurethane resin is PU-3486; the average molecular weight of the polylactic acid is 50,000, and the molecular weight distribution is between 10,000 and 60,000.

[0096] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0097] The preparation method of the semi-degradable water-based coating comprises the following steps:

[0098] (R1), taking water-based acrylic resin, water-based polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water by weight, and set aside;

[0099] (R2), adding polylactic acid to the cosolvent and mixing evenly to obtain a premixed solution;

[0100] (R3) Add water-based acrylic resin, water-based polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer into deionized water and mix evenly, then add thickener and film-forming aid and mix evenly to obtain semi-degradable water-based coating.

[0101] The method for preparing the long-lasting fragrance air filter element comprises the following steps:

[0102] (S1), bonding the PET staple fiber primary filter layer 2, the melt-blown PP layer 3, the first mesh cover 4, and the honeycomb carrier 5 in sequence to form a multi-layer structure, and then bonding the outer periphery of the multi-layer structure to the inner wall of the fixed frame 1 to obtain a semi-finished filter element;

[0103] (S2) After filling a plurality of activated carbon particles 7 and a plurality of aroma particles 8 into the honeycomb holes of the honeycomb carrier 5, the second mesh cover 6 is bonded to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after packaging, a long-lasting fragrance air filter element is obtained.

[0104] Example 4

[0105] like Figure 1 As shown, a long-lasting fragrance air filter element includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5 and a second mesh cover 6, which are all fixedly installed in the fixed frame 1 and bonded in sequence, and the honeycomb holes of the honeycomb carrier 5 are filled with a plurality of activated carbon particles 7 and a plurality of aroma particles 8; the aroma particles 8 are composed of a particle body and a film layer coated on the particle body, and the film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body twice and then drying it.

[0106] The thickness of the membrane layer is 0.7 mm; in the honeycomb holes of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:4.

[0107] The particle body comprises the following components in parts by weight:

[0108]

[0109] The perlite powder loaded with essential oil is prepared by mixing the essential oil and the perlite powder in a weight ratio of 6:5. The particle size of the perlite powder is 10 μm; and the essential oil is lemon essential oil.

[0110] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; and the colorant is red iron oxide.

[0111] The preparation method of the particle body comprises the following steps: uniformly mixing ethylene-vinyl acetate copolymer EA33045, perlite powder loaded with essential oil, a lubricating dispersant and a colorant by weight, extruding and granulating through a twin-screw extruder to obtain the particle body; wherein the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are respectively 50°C, 60°C, 70°C, 75°C and 65°C, the head temperature is 62°C, the screw aspect ratio is 25:1, and the screw speed is 120r / min.

[0112] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0113]

[0114]

[0115] The water-based acrylic resin is NeoCryI XK-540; the water-based polyurethane resin is PU-3486; the average molecular weight of the polylactic acid is 40,000, and the molecular weight distribution is between 10,000 and 60,000.

[0116] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0117] The preparation method of the semi-degradable water-based coating comprises the following steps:

[0118] (R1), taking water-based acrylic resin, water-based polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water by weight, and set aside;

[0119] (R2), adding polylactic acid to the cosolvent and mixing evenly to obtain a premixed solution;

[0120] (R3) Add water-based acrylic resin, water-based polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer into deionized water and mix evenly, then add thickener and film-forming aid and mix evenly to obtain semi-degradable water-based coating.

[0121] The method for preparing the long-lasting fragrance air filter element comprises the following steps:

[0122] (S1), bonding the PET staple fiber primary filter layer 2, the melt-blown PP layer 3, the first mesh cover 4, and the honeycomb carrier 5 in sequence to form a multi-layer structure, and then bonding the outer periphery of the multi-layer structure to the inner wall of the fixed frame 1 to obtain a semi-finished filter element;

[0123] (S2) After filling a plurality of activated carbon particles 7 and a plurality of aroma particles 8 into the honeycomb holes of the honeycomb carrier 5, the second mesh cover 6 is bonded to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after packaging, a long-lasting fragrance air filter element is obtained.

[0124] Comparative Example 1

[0125] The difference between this comparative example and Example 1 is:

[0126] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0127]

[0128] 8 parts of deionized water; that is, the semi-degradable water-based paint does not contain polylactic acid.

[0129] Comparative Example 2

[0130] The difference between this comparative example and Example 1 is:

[0131] The film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body once and then drying it. The thickness of the film layer is 0.2 mm.

[0132] Comparative Example 3

[0133] The difference between this comparative example and Example 1 is:

[0134] The particle body comprises the following components in parts by weight:

[0135]

[0136] The titanium dioxide doped with essential oil is prepared by mixing the essential oil and titanium dioxide in a weight ratio of 6:4.5. The particle size of the titanium dioxide is 20 μm.

[0137] The preparation method of the particle body comprises the following steps: uniformly mixing ethylene-vinyl acetate copolymer EA33045, titanium dioxide doped with essential oil, lubricating dispersant and colorant by weight, extruding and granulating through a twin-screw extruder to obtain the particle body.

[0138] Comparative Example 4

[0139] An air filter element is taken from a commercially available brand: Qingxi, with a product name: automobile aromatherapy air conditioning filter element and a product number: 10054267311135.

[0140] Example 5

[0141] Performance Test:

[0142] I. Take multiple groups of air filter elements of Example 1, assemble them in the same car (Great Wall C50) and use them in the urban area, take the initial aromatherapy particles, the aromatherapy particles after 3 months of use and the aromatherapy particles after 5 months of use, respectively, use SEM to scan and image them, and obtain the SEM morphology images of the initial aromatherapy particles, the aromatherapy particles after 3 months of use and the aromatherapy particles after 5 months of use, respectively, as shown in FIG. Figure 2-4 As shown, it can be seen that during actual use, the membrane layer of the aromatherapy particles can be semi-degraded to obtain a microporous structure. As time goes by, the microporous structure formed by the semi-degradation of the membrane layer is larger and more numerous, that is, the channels for releasing fragrance are larger and more numerous.

[0143] II. Take multiple groups of air filter elements of Examples 1-4 and Comparative Examples 1-4, assemble them in the same car (Great Wall C50) and use them in the urban area. Take the initial air filter element, the air filter element after one month of use, the air filter element after three months of use, the air filter element after five months of use and the air filter element after seven months of use respectively, and use the odor detector XP-329IIIR to test the grade value of the fragrance. During the test, the detection probe of the odor detector is against the middle of the second mesh cover, and the value is recorded. The test results are shown in Table 1 below:

[0144]

[0145]

[0146] As can be seen from Table 1 above, the long-lasting fragrance air filter of the present application has a better fragrance retention effect and fragrance persistence. From the use results of Examples 1-4, the air filter after 3 months of use has a stronger fragrance than the air filter after 1 month of use. The main reason is that the semi-degradation of the membrane layer to form microporous channels promotes the diffusion and release of the fragrance essential oil, so as to maintain the fragrance retention effect of the air filter; and the fragrance of the air filter after 5 months of use is weakened to a certain extent. The main reason is that the concentration of the residual fragrance essential oil is lower, but the microporous channels are larger and more numerous, which further promotes the diffusion and release of the fragrance essential oil to maintain the fragrance intensity to a certain extent, and the fragrance is weakened. The amplitude is not low and it is not difficult for consumers to detect, so it can still reflect its fragrance retention effect; and the air filter after 7 months of use, its fragrance essential oil is almost evaporated, and consumers are not able to smell the fragrance; for Example 3, because its film layer is thicker, the fragrance particles are more, and the average molecular weight of polylactic acid is larger, therefore, the fragrance retention effect and fragrance persistence are better. Compared with Comparative Example 1, the film layer of Example 1 has a certain amount of polylactic acid, which is conducive to the degradation of polylactic acid to form a microporous structure after a period of use, so as to release the essential oil. Otherwise, the low concentration of essential oil only relies on the intermolecular diffusion effect under the condition of the barrier between the film layer and the particle body. Although the fragrance is more lasting, the released fragrance is weak and the fragrance effect is poor. Compared with Comparative Example 2, the film layer of Example 1 is controlled at 0.5-1mm to improve its effect of blocking the fragrance release, which is conducive to the slow release of the essential oil in the early stage of use, avoiding the release of too high concentration and too heavy fragrance to cause discomfort to consumers. Compared with Comparative Example 3, Example 1 uses perlite micropowder to load the essential oil, and uses the adsorption characteristics of perlite micropowder to avoid the rapid volatilization and diffusion of the essential oil, resulting in insufficient fragrance effect in the later stage of use. Compared with Comparative Example 4, Example 1 adopts the specific air filter element of the present invention, and the fragrance effect and fragrance persistence are better.

[0147] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A long-lasting fragrance air filter element, characterized in that: It includes a fixed frame, and a PET short fiber primary filter layer, a melt-blown PP layer, a first mesh cover, a honeycomb carrier and a second mesh cover, which are all fixedly installed in the fixed frame and bonded in sequence. The honeycomb holes of the honeycomb carrier are filled with a plurality of activated carbon particles and a plurality of aromatherapy particles. The aromatherapy particles are composed of a particle body and a film layer coated on the particle body, and the film layer is formed by coating a semi-degradable water-based paint on the surface of the particle body at least twice and then drying it.

2. The long-lasting fragrance air filter element according to claim 1, characterized in that: The thickness of the film layer is 0.5-1.0 mm; in the honeycomb holes, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3-5.

3. The air filter element with a long-lasting fragrance according to claim 1, characterized in that: The particle body comprises the following components in parts by weight: Ethylene-vinyl acetate copolymer 60-70 parts 30-40 parts of perlite powder loaded with essential oil 1-3 parts of lubricating dispersant 1-3 parts of colorant.

4. The air filter element with a long-lasting fragrance according to claim 3, characterized in that: The density of the ethylene-vinyl acetate copolymer is 0.94-0.96 g / cm 3 , the melting temperature is 45-66°C; the perlite powder loaded with essential oil is mixed with essential oil and perlite powder in a weight ratio of 5-7:4-5.

5. The air filter element with a long-lasting fragrance according to claim 3, characterized in that: The lubricating dispersant is pentaerythritol stearate and / or carboxymethyl cellulose; the colorant is at least one of titanium dioxide, carbon black, mica powder, yellow iron oxide or red iron oxide.

6. The air filter element with a long-lasting fragrance according to claim 3, characterized in that: The preparation method of the particle body comprises the following steps: uniformly mixing ethylene-vinyl acetate copolymer, perlite powder loaded with essential oil, lubricating dispersant and colorant by weight, extruding and granulating through a twin-screw extruder to obtain the particle body; wherein the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are respectively 45-55°C, 55-65°C, 65-75°C, 65-80°C and 60-75°C, the head temperature is 60-75°C, the screw aspect ratio is 25:1, and the screw speed is 60-150r / min.

7. The air filter element with a long-lasting fragrance according to claim 1, characterized in that: The semi-degradable water-based coating comprises the following raw materials in parts by weight:

8. The air filter element with a long-lasting fragrance according to claim 7, characterized in that: The water-based acrylic resin is NeoCryI XK-540 or DB3618; the water-based polyurethane resin is PU-3486 or H-34P; the average molecular weight of the polylactic acid is 30,000-50,000, and the molecular weight distribution is between 10,000-60,000.

9. The air filter element with a long-lasting fragrance according to claim 7, characterized in that: The dispersant is BYK-190 or BYK192; the defoamer is BYK-028; the wetting agent is BASF WE3229 or TEGO WET280; the thickener is at least one of sodium carboxymethyl cellulose, propylene glycol alginate or sodium carboxymethyl starch; the film-forming aid is dipropylene glycol butyl ether or diethylene glycol monobutyl ether; and the cosolvent is isopropanol and / or ethanol.

10. A method for preparing a long-lasting fragrance air filter element according to any one of claims 1 to 9, characterized in that: The steps include: (S1) The PET short fiber primary filter layer, the melt-blown PP layer, the first mesh cover, and the honeycomb carrier are sequentially bonded to form a multi-layer structure, and then the periphery of the multi-layer structure is bonded to the inner wall of the fixed frame to obtain a semi-finished filter element; (S2) After filling a plurality of activated carbon particles and a plurality of aroma particles into the honeycomb holes of the honeycomb carrier, the second mesh cover is bonded to the side of the honeycomb carrier away from the first mesh cover, and after packaging, a long-lasting fragrance air filter element is obtained.

Citation Information

Patent Citations

  • High-concentration polyolefin aromatic master batch and its preparation method

    CN102766294A

  • Honeycomb activated carbon filter and manufacturing method thereof

    CN108993025A

  • Aroma-enhancing and cooling particles for cigarettes as well as preparation method and application thereof

    CN112273717A

  • DETERGENT COMPOSITIONS WITH ENHANCED OLFACTORY PROPERTIES

    FR3091877A1

  • Making process of perfume sheet type patch

    KR1020000026387A