Reverse flotation desilicication collector as well as preparation method and application thereof
The antiflotation desilica collector prepared by combining alkyl polyamines, amide betaines and alkyl polyethers in silicone calcyl gel phosphite, the siliceous veins in acidic reverse flotation demagnesium return water were solved. The problem of separating stones has achieved efficient desiliconization and low-cost return water treatment, and improved the stability and efficiency of the double reverse flotation process of silicon calcareous phosphate ore.
Patent Information
- Application Number
- CN202410981622.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The lack of high-efficiency desilicate collectors for brittle foam adapted to acidic reverse flotation demagnesium return water in the prior art, resulting in difficult to solve the interaction of return water in the double reverse flotation process of silicon calcareous gel phosphate, resulting in low production efficiency and cost high.
The antiflotation desilase collector is prepared by compounding alkyl polyamines, amide betaines and alkyl polyethers, so as to achieve efficient separation of siliceous ganglite in an acidic environment, and is compatible with acidic reverse flotation demagnesium return water. Reduce the cost of return water treatment and improve sorting efficiency.
Under the conditions of acidic reverse flotation demagnesium return water, the effective removal of siliceous gangue in phosphate phosphate of silicone , reduced the cost of return water treatment, improved the efficiency of reverse flotation desilicon sorting, and ensured that High-value utilization of phosphate ore resources.
Smart Images

Figure CN118925940A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to calci-silicon colloid phosphate, and in particular to a reverse flotation desiliconizing collector, a preparation method and uses thereof, and in particular to a brittle-bubble high-efficiency reverse flotation desiliconizing collector suitable for acidic reverse flotation demagnesium return water, a preparation method and uses thereof. Background Art
[0002] At present, the research on the flotation technology of medium and low-grade calcareous siliceous colloid phosphate mainly focuses on direct-reverse flotation and double-reverse flotation, but few of these two processes have been industrialized.
[0003] An important difficulty in the industrialization of the double reverse flotation process of silico-calcium collophosphate is the mutual accumulation between the return water of reverse flotation desiliconization and the return water of reverse flotation demagnesiumization, which causes the deterioration of the foam fluidity and flotation separation efficiency of each operation, making it difficult for the industrial production of double reverse flotation to operate stably. At present, in response to this difficulty, the main methods disclosed include quality-based utilization and pretreatment-reuse of the return water of double reverse flotation.
[0004] CN112237993A discloses a method for recycling wastewater from the double reverse flotation process of collophanite, wherein the overflow of the collophanite after grinding and classification is subjected to reverse flotation to obtain tailings and coarse concentrate, and the tailings are thickened and filtered to obtain tailings; the coarse concentrate is thickened and the filter cake obtained by pressure filtration is slurried and reverse flotated again to obtain tailings and concentrate slurry; the tailings are thickened and filtered to obtain tailings; the concentrate slurry is thickened and filtered to obtain concentrate. This method is a conventional means to deal with the serious cross-effect of flotation reagents, but the investment cost and floor space of the thickening tank construction are large, and it cannot completely solve the problem of cross-effect of anions and cations in wastewater.
[0005] CN115594353A discloses a method for treating wastewater from the double reverse flotation of collophanite. The method comprises adjusting the pH value of wastewater containing anionic and cationic collectors generated in the double reverse flotation of collophanite, introducing an eliminator to eliminate the cationic collector, and removing the anionic collector and the eliminator in the wastewater by adsorption. Finally, the concentrations of the residual cationic collector and the anionic collector in the wastewater are reduced to a lower level, thereby avoiding the cross-influence of anionic and cationic collectors in the double reverse flotation operation, resulting in excessive viscosity of mineralized foam in each operation, reduced sorting efficiency, and failure of normal production, thereby achieving zero discharge of mineral processing wastewater and the cost of pretreatment of return water is not low.
[0006] From the above, it can be seen that at present, there is a lack of a desiliconization collector that is compatible with the return water of acidic reverse flotation demagnesiumization. It is difficult to fundamentally solve the adverse effects of the interaction between the two return waters with very different properties. In addition, the cost of return water utilization is high and the sorting indicators are unstable. At the same time, the mainstream mineral processing technology adopted by phosphorus chemical industrial parks or phosphate mines is reverse flotation demagnesiumization. The water used for reverse flotation desiliconization basically uses the return water of acidic reverse flotation demagnesiumization, and the reverse flotation demagnesiumization operation must face the problem of desiliconization collector mixing. Therefore, whether the interactive influence of return water from different operations in the industrialization process of double reverse flotation of silico-calcium colloidal phosphate can be solved, fundamentally, it is necessary to provide a brittle foaming and efficient desiliconization collector that is suitable for the return water of acidic reverse flotation demagnesiumization. Summary of the invention
[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a reverse flotation desiliconization collector and a preparation method and use thereof, which can realize an economical and efficient reverse flotation desiliconization process in an acidic, complex, multi-type and high-concentration impurity ion environment, which not only saves the return water treatment cost, reduces the adverse effects of the interaction of return waters of different properties on the double reverse flotation operations, but also ensures a relatively high reverse flotation desiliconization separation efficiency, laying a foundation for the large-scale application of double reverse flotation of silico-calcium collophosphate.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a reverse flotation desiliconization collector, which comprises an alkyl polyamine, an amide betaine and an alkyl polyether.
[0010] The reverse flotation desiliconizing collector provided by the present invention is compounded with specific alkyl polyamines, amide betaines and alkyl polyethers, and can realize the removal of siliceous gangue in silico-calcium colloidal phosphate by reverse flotation process in an acidic reverse flotation demagnesium return water environment. Under the premise of good fluidity of silicon-containing foam, efficient separation of phosphate minerals and silicon-containing gangue is achieved, which is conducive to the high-value utilization of phosphate resources.
[0011] As a preferred technical solution of the present invention, the amine groups of the alkyl polyamine include tertiary amine groups and quaternary amine groups;
[0012] Preferably, the amide betaine includes one or a combination of at least two of myristic amide hydroxysulfopropyl betaine, lauryl amide hydroxysulfopropyl betaine or demeryl amide hydroxysulfopropyl betaine;
[0013] Preferably, the alkyl polyether includes dodecyl polyoxyethylene ether and / or hexadecyl polyoxyethylene ether.
[0014] As a preferred technical solution of the present invention, the reverse flotation desiliconization collector comprises, by weight: 5-7 parts of alkyl polyamine, 1-2 parts of amide betaine and 2-4 parts of alkyl polyether.
[0015] In a second aspect, the present invention provides a method for preparing the reverse flotation desiliconization collector as described in the first aspect, the preparation method comprising: mixing alkyl polyamine, amide betaine, and alkyl polyether according to a formula to obtain a reverse flotation desiliconization collector.
[0016] In a third aspect, the present invention provides a use of the reverse flotation desiliconization collector as described in the first aspect, wherein the use comprises using the reverse flotation desiliconization collector to reverse flotation desiliconize calcareous collophane ore.
[0017] As a preferred technical solution of the present invention, the use includes: mixing and stirring the silico-calcium colloidal phosphate slurry with a reverse flotation desiliconizing collector, and then performing reverse flotation operations to obtain silicon tailings and phosphate concentrate.
[0018] As a preferred technical solution of the present invention, the calci-silico-colloid phosphate slurry is obtained by mixing calci-silico-colloid phosphate ore with acidic reverse flotation demagnesized return water and then grinding the mixture.
[0019] Preferably, the calci-silico-collophane ore comprises, by mass percentage, the following: P2O5 20-28%, SiO2 10-30%, and MgO 1.0-4.0%.
[0020] Preferably, the acidic reverse flotation demagnesium return water comprises: 4000-7000 mg / L sulfate ions, 1500-4000 mg / L phosphate ions, 300-700 mg / L calcium ions and 500-1200 mg / L magnesium ions.
[0021] As a preferred technical solution of the present invention, the slurry concentration of the calcium-silicon collophanite slurry is 20-40wt%.
[0022] Preferably, the pH value of the calci-silico-collophane slurry is 5-7.
[0023] Preferably, solid particles with a diameter of -0.074 mm in the calci-silico-collophane slurry account for 60-85% of the mass of all solid particles.
[0024] As a preferred technical solution of the present invention, the mixing and stirring time is 3-5 minutes.
[0025] Preferably, the stirring speed of the mixing and stirring is 1.5-2 m / s.
[0026] As a preferred technical solution of the present invention, the reverse flotation operation performs at least one roughing operation and one scavenging operation.
[0027] Preferably, the addition amount of the reverse flotation desiliconization collector is 100-500 g / t.
[0028] Preferably, the reverse flotation operation is a closed-circuit reverse flotation.
[0029] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0030] (1) In the return water of acidic reverse flotation demagnesiumization, a specific compound reagent is used to remove the siliceous gangue through one or more reverse flotation operations without affecting the fluidity of the desiliconization foam and the desiliconization separation efficiency, thereby achieving good compatibility between the desiliconization collector and the return water of acidic reverse flotation demagnesiumization.
[0031] (2) After desiliconization, the phosphate concentrate can be demagnesized by reverse flotation with the addition of a small amount of acid and anion collector. The pH values of reverse flotation desiliconization and reverse flotation demagnesium are similar, both under acidic conditions, which greatly reduces the cost of reagents for adjusting the flotation pH.
[0032] (3) The return water from each operation of double reverse flotation can be fully reused without separation and special treatment, which saves the cost of return water treatment and water resource consumption, and does not pollute the environment.
[0033] (4) Under acidic backwater conditions, the combination of reverse flotation de-magnesium collector and reverse flotation de-silicon collector can improve the floating speed of siliceous gangue and the collection capacity of siliceous gangue; the residual reverse flotation de-silicon collector and reverse flotation de-magnesium collector can, to some extent, achieve the simultaneous floating of magnesium-containing gangue and silicon-containing gangue, thereby ensuring the quality of phosphate concentrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a flow chart of the use of a reverse flotation desiliconization collector according to an embodiment of the present invention;
[0035] Figure 2 This is a flow chart of the use of reverse flotation desiliconization collector in Example 1 of the present invention.
[0036] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0037] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0038] This embodiment provides a reverse flotation desiliconization collector, which includes alkyl polyamine, amide betaine and alkyl polyether.
[0039] Wherein, the amine groups of the alkyl polyamine include tertiary amine groups and quaternary amine groups.
[0040] In the present invention, the alkyl polyamine is a single substance, i.e., a polyamine with a long carbon chain containing a tertiary amine group and a quaternary ammonium group, rather than a mixture of a tertiary amine and a quaternary ammonium group. For example, it can be a conventional commercially available agent such as BK432, or an alkyl polyamine synthesized according to the prior art and meeting the requirements of the present invention can be selected.
[0041] The amide betaine includes one or a combination of at least two of myristic amide hydroxysulfopropyl betaine, lauryl amide hydroxysulfopropyl betaine or demeryl amide hydroxysulfopropyl betaine.
[0042] Wherein, the alkyl polyether includes dodecyl polyoxyethylene ether and / or hexadecyl polyoxyethylene ether.
[0043] The reverse flotation desiliconization collector comprises, by weight: 5-7 parts of alkyl polyamine, 1-2 parts of amide betaine and 2-4 parts of alkyl polyether.
[0044] In the present invention, the alkyl polyamine in the reverse flotation desiliconization collector is 5-7 parts by weight, for example, it can be 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6 parts, 6.2 parts, 6.4 parts, 6.6 parts, 6.8 parts or 7 parts, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0045] In the present invention, the amide betaine in the reverse flotation desiliconization collector is 1-2 parts by weight, for example, it can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts or 2 parts, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0046] In the present invention, the amide betaine in the reverse flotation desiliconization collector is 2-4 parts by weight, for example, it can be 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts or 4 parts, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0047] Furthermore, this embodiment provides a method for preparing the aforementioned reverse flotation desiliconization collector, the preparation method comprising: mixing alkyl polyamine, amide betaine, and alkyl polyether according to a formula to obtain a reverse flotation desiliconization collector.
[0048] Further, this embodiment provides the use of the aforementioned reverse flotation desiliconization collector, the process is as follows Figure 1 As shown, the use includes using the reverse flotation desiliconization collector to reverse flotation desiliconize calcareous collophane ore.
[0049] The use includes: mixing and stirring the silico-calcium colloidal phosphate slurry with a reverse flotation desiliconizing collector, and then performing reverse flotation operations to obtain silicon tailings and phosphate concentrate.
[0050] The calci-silico-colloid phosphate slurry is obtained by mixing calci-silico-colloid phosphate ore with acidic reverse flotation magnesium removal return water and then grinding the mixture;
[0051] The siliceous-calcium collophosphate ore comprises, by mass percentage, 20-28% P2O5, 10-30% SiO2, and 1.0-4.0% MgO.
[0052] In the present invention, the mass percentage of P2O5 in the calcisilicate collophosphate ore is 20-28%, for example, it can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0053] In the present invention, the mass percentage of SiO2 in the calci-silico-collophane ore is 10-30%, for example, it can be 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28% or 30%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0054] In the present invention, the mass percentage of MgO in the calcisilicate collophanite ore is 1.0-4.0%, for example, it can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8% or 4.0%, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0055] The acidic reverse flotation demagnesium return water contains 4000-7000 mg / L sulfate ions, 1500-4000 mg / L phosphate ions, 300-700 mg / L calcium ions and 500-1200 mg / L magnesium ions.
[0056] Among them, the slurry concentration of the siliceous calcium colloidal phosphate slurry is 20-40wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wy%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0057] In the present invention, wt% refers to mass percentage.
[0058] In the present invention, the solid-liquid ratio of the silico-calcium collophosphate ore and the acidic reverse flotation demagnesizing return water in the grinding is based on the concentration of the slurry obtained by the grinding.
[0059] The pH value of the calci-silico-colloid phosphate slurry is 5-7, for example, it can be 5, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9 or 7, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0060] Among them, the solid particles of -0.074mm in the silico-calcium colloidal phosphate slurry account for 60-85% of the mass of all solid particles, for example, it can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84% or 85%, etc., but are not limited to the listed values, and other values not listed within the range are also applicable.
[0061] In the present invention, -0.074 mm refers to the undersize product obtained by sieving with a 0.074 mm sieve.
[0062] The mixing and stirring time is 3-5 min, for example, it can be 3 min, 3.2 min, 3.4 min, 3.6 min, 3.8 min, 4 min, 4.2 min, 4.4 min, 4.6 min, 4.8 min or 5 min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0063] The stirring speed of the mixed stirring is 1.5-2 m / s, for example, it can be 1.5 m / s, 1.6 m / s, 1.7 m / s, 1.8 m / s, 1.9 m / s or 2 m / s, but is not limited to the listed values, and other values not listed in the range are also applicable.
[0064] Wherein, the reverse flotation operation performs at least one roughing operation and one scavenging operation.
[0065] Wherein, the addition amount of the reverse flotation desiliconization collector is 100-500g / t, for example, it can be 100g / t, 150g / t, 200g / t, 250g / t, 300g / t, 350g / t, 400g / t, 450g / t or 500g / t, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0066] In the present invention, g / t refers to adding a flotation agent of corresponding mass g to a certain amount of calci-silico-colloid phosphate ore, and the specific mixing ratio with water can be designed according to the conventional requirements in the field, that is, the amount of g / t flotation agent in the present invention is the mass before mixing with water.
[0067] In the present invention, the number of times the reverse flotation operation is performed can be designed according to the content of siliceous gangue in the siliceous-calcium collophosphate ore. In multiple reverse flotations, the phosphate concentrate product obtained is obtained by mixing the phosphate concentrate obtained from each reverse flotation roughing operation.
[0068] Wherein, the reverse flotation operation is a closed-circuit reverse flotation.
[0069] According to the above scheme, the silico-calcium colloidal phosphate is added to the acidic reverse flotation demagnesium return water for grinding. After grinding, the slurry flows into the stirring tank, and then the reverse flotation collector is added to the stirring tank for stirring and selective adsorption. The slurry-adjusted material enters the reverse flotation desiliconization system, and the mineralized foam scraped out by the scraper is the silicon tailings, which are discharged after dense pressure filtration and stacked. The product in the tank is the desiliconized phosphate concentrate, and enters the reverse flotation demagnesium system. The mineralized foam scraped out by the scraper is the magnesium tailings, which are discharged after dense pressure filtration and stacked. The product in the tank is the final phosphate concentrate. The return water generated by the tailings and phosphate concentrate does not need additional treatment and can be fully returned for use, reducing the consumption of reagents and water resources.
[0070] Further, in order to illustrate the good desiliconization effect that can be achieved by the reverse flotation desiliconization collector provided by the present invention, an actual example is used for exemplary description, as follows:
[0071] Example 1
[0072] This embodiment provides a brittle foam high-efficiency reverse flotation desiliconization collector suitable for acidic reverse flotation demagnesium return water, the collector comprises, by weight: 5 parts of alkyl polyamine, 1 part of amide betaine and 3 parts of alkyl polyether;
[0073] The alkyl polyamine is commercially available BK432, the amide betaine is tetradecylamide hydroxysulfopropyl betaine, and the alkyl polyether is dodecyl polyoxyethylene ether;
[0074] The above reagents are mixed according to the formula.
[0075] Example 2
[0076] This embodiment provides a brittle foam high-efficiency reverse flotation desiliconization collector suitable for acidic reverse flotation demagnesium return water, the collector comprises 6 parts of alkyl polyamine, 1 part of amide betaine and 2 parts of alkyl polyether in parts by weight;
[0077] The alkyl polyamine is commercially available BK432, the amide betaine is dodecylamide hydroxysulfopropyl betaine, and the alkyl polyether is hexadecyl polyoxyethylene ether;
[0078] The above reagents are mixed according to the formula.
[0079] Example 3
[0080] This embodiment provides a brittle foam high-efficiency reverse flotation desiliconization collector suitable for acidic reverse flotation demagnesium return water, the collector comprises 7 parts of alkyl polyamine, 2 parts of amide betaine and 4 parts of alkyl polyether in parts by weight;
[0081] The alkyl polyamine is commercially available BK432, the amide betaine is decylamide hydroxysulfopropyl betaine, and the alkyl polyether is dodecyl polyoxyethylene ether;
[0082] The above reagents are mixed according to the formula.
[0083] Application Example 1
[0084] This embodiment provides a use of a brittle foam high-efficiency reverse flotation desiliconization collector suitable for acidic reverse flotation demagnesium return water, such as Figure 2 As shown, the siliceous-calcium collophanite used is a medium-low grade collophanite produced in Xingshan, Hubei. The silicon-containing minerals in the ore are mainly feldspar and quartz, with a P2O5 mass fraction of 24.24%, a SiO2 mass fraction of 20.12%, and a MgO mass fraction of 1.4%. The specific process is as follows:
[0085] (1) mixing the collophanite ore and the acidic reverse flotation demagnesized return water and grinding the ore, and adjusting the slurry to control the slurry concentration to 25% and the slurry pH to 5.0 after grinding;
[0086] (2) the ore pulp obtained in step (1) enters a mixing tank and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 1 to obtain silicon tailings 1 and phosphate concentrate 1; the phosphate concentrate 1 enters an intermediate box of a flotation machine and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 2 to obtain silicon tailings 2 and phosphate concentrate 2;
[0087] (3) The silicon tailings 1 and silicon tailings 2 obtained in step (2) are combined and enter the reverse flotation desiliconization scavenging operation 1 to obtain silicon tailings 3 and middlings 1; the middlings 1 are returned to the roughing operation 1;
[0088] (4) The silicon tailings 3 obtained in step (3) enter the reverse flotation desiliconization scavenging operation 2 to obtain silicon tailings 4 and middlings 2; the middlings 2 are returned to the scavenging operation 1;
[0089] Phosphate concentrate 2 is the final desiliconized phosphate concentrate, and silicon tailings 4 is the final silicon tailings.
[0090] Wherein, the amount of reverse flotation desiliconization collector added in the roughing 1 process of step (2) is 360 g / t; the amount of reverse flotation desiliconization collector added in the roughing 2 process is 120 g / t;
[0091] The desiliconized phosphate concentrate finally obtained in this application example has a P2O5 mass fraction of 32.15%, a SiO2 mass fraction of 6.51%, and a P2O5 recovery rate of 88.36%.
[0092] Application Example 2
[0093] This embodiment provides a use of a brittle bubble high-efficiency reverse flotation desiliconization collector suitable for acidic reverse flotation demagnesium return water. The siliceous calcium collophanite used is a medium-low grade collophanite produced in Hubei. The silicon-containing minerals in the ore are mainly feldspar and quartz, with a P2O5 mass fraction of 26.62%, a SiO2 mass fraction of 16.36%, and a MgO mass fraction of 2.4%. The specific process is as follows:
[0094] (1) mixing the collophanite ore and the acidic reverse flotation demagnesized return water and grinding the ore, and adjusting the slurry to control the slurry concentration to 30% and the slurry pH to 5.2 after grinding;
[0095] (2) The slurry obtained in step (1) enters a mixing tank and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation to obtain silicon tailings 1 and phosphate concentrate 1; the phosphate concentrate 1 enters an intermediate box of a flotation machine and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 2 to obtain silicon tailings 2 and phosphate concentrate 2;
[0096] (3) The silicon tailings 1 and silicon tailings 2 obtained in step (2) are combined and enter the reverse flotation desiliconization scavenging operation 1 to obtain silicon tailings 3 and middlings; the middlings are returned to the roughing operation;
[0097] Phosphate concentrate 2 is the final desiliconized phosphate concentrate, and silicon tailings 3 is the final silicon tailings.
[0098] Wherein, the amount of reverse flotation desiliconization collector added in the roughing 1 process of step (2) is 300 g / t; the amount of reverse flotation desiliconization collector added in the roughing 2 process is 80 g / t;
[0099] The desiliconized phosphate concentrate finally obtained in this application example has a P2O5 mass fraction of 32.45%, a SiO2 mass fraction of 5.87%, and a P2O5 recovery rate of 89.32%.
[0100] Application Example 3
[0101] This embodiment provides a use of a brittle bubble high-efficiency reverse flotation desiliconization collector suitable for acidic reverse flotation demagnesium return water. The siliceous calcium collophanite used is a medium-low grade collophanite produced in Yunnan. The silicon-containing minerals in the ore are mainly feldspar, muscovite and quartz. The mass fraction of P2O5 is 21.37%, the mass fraction of SiO2 is 24.68%, and the mass fraction of MgO is 2.6%. The specific process is as follows:
[0102] (1) mixing the collophanite ore and the acidic reverse flotation demagnesized return water and grinding the ore, and adjusting the slurry to control the slurry concentration to 25% and the slurry pH to 5.0 after grinding;
[0103] (2) The ore pulp obtained in step (1) enters a mixing tank and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation to obtain silicon tailings 1 and phosphate concentrate 1; the phosphate concentrate 1 enters an intermediate box of the flotation machine and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 2 to obtain silicon tailings 2 and phosphate concentrate 2; the phosphate concentrate 2 enters an intermediate box of the flotation machine and is mixed with a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 3 to obtain silicon tailings 3 and phosphate concentrate 3;
[0104] (3) The silicon tailings 1, 2 and 3 obtained in step (2) are combined and enter the reverse flotation desiliconization scavenging operation 1 to obtain silicon tailings 4 and middlings 1; the middlings 1 are returned to the roughing operation;
[0105] (4) The silicon tailings 4 obtained in step (3) enter the reverse flotation desiliconization scavenging operation 2 to obtain silicon tailings 5 and middlings 2; the middlings 2 are returned to the scavenging operation 1;
[0106] Phosphate concentrate 3 is the final desiliconized phosphate concentrate, and silicon tailings 5 is the final silicon tailings.
[0107] Wherein, in step (2), the amount of reverse flotation desiliconization collector added during roughing 1 is 300 g / t; the amount of reverse flotation desiliconization collector added during roughing 2 is 100 g / t; the amount of reverse flotation desiliconization collector added during roughing 3 is 100 g / t;
[0108] The desiliconized phosphate concentrate finally obtained in this application example has a P2O5 mass fraction of 32.25%, a SiO2 mass fraction of 5.87%, and a P2O5 recovery rate of 86.13%.
[0109] Application Example 4
[0110] The only difference from Application Example 3 is that the alkyl polyamine in the collector used in the reverse flotation process is replaced by an equal amount of dodecyl ether diamine.
[0111] The final phosphate concentrate obtained in this application example has a P2O5 mass fraction of 30.18%, a SiO2 mass fraction of 9.85%, and a P2O5 recovery rate of 66.37% in the desiliconized phosphate concentrate. The desiliconized foam is very sticky and difficult to industrialize.
[0112] Application Example 5
[0113] The only difference from Application Example 3 is that the amide betaine in the collector used in the reverse flotation process is replaced by dodecyltrimethylammonium chloride.
[0114] The final P2O5 mass fraction obtained in this application example is 31.36%, the SiO2 mass fraction is 7.85%, the P2O5 recovery rate of the desiliconized phosphate concentrate is 80.32%, and the fluidity of the desiliconized foam is average.
[0115] Application Example 6
[0116] The only difference from Application Example 3 is that the alkyl polyether in the collector used in the reverse flotation process is replaced by an equal amount of butyl ether.
[0117] The final P2O5 mass fraction obtained in this application example is 30.32%, the SiO2 mass fraction is 10.35%, the P2O5 recovery rate of the desiliconized phosphate concentrate is 82.37%, and the fluidity of the desiliconized foam is average.
[0118] Application Example 7
[0119] The only difference from Application Example 3 is that the amide betaine in the collector is replaced with an equal amount of dodecyl sulfopropyl betaine.
[0120] The final P2O5 mass fraction obtained in this application example is 30.75%, the SiO2 mass fraction is 10.05%, the P2O5 recovery rate of the desiliconized phosphate concentrate is 81.37%, and the fluidity of the desiliconized foam is average.
[0121] Application Example 8
[0122] The only difference from Application Example 3 is that the amide betaine in the collector is replaced with an equal amount of dodecyl dimethyl betaine.
[0123] The final P2O5 mass fraction obtained in this application example is 31.05%, the SiO2 mass fraction is 9.56%, the P2O5 recovery rate of the desiliconized phosphate concentrate is 78.67%, and the fluidity of the desiliconized foam is average.
[0124] Application Example 9
[0125] The only difference from Application Example 1 is that the alkyl polyamine in the collector is replaced by tetradecyl dimethyl tertiary amine and alkyl dimethyl benzyl ammonium chloride in a mass ratio of 1:1.
[0126] The final P2O5 mass fraction obtained in this application example is 31.68%, the SiO2 mass fraction is 8.67%, the P2O5 recovery rate of the desiliconized phosphate concentrate is 82.69%, and the fluidity of the desiliconized foam is average.
[0127] It can be seen from the results of the above embodiments and application examples that the composite collector provided by the present invention can effectively remove siliceous gangue in silico-calcium collophosphate under the conditions of acidic reverse flotation demagnesium return water, the desiliconization foam has good fluidity, and the desiliconization collector and acidic reverse flotation demagnesium return water are well compatible. Furthermore, the return water can be fully reused without separation and special treatment, saving the return water treatment cost and water resource consumption, and is pollution-free to the environment. Furthermore, the low flotation pH value difference between the reverse flotation desiliconization operation and the reverse flotation demagnesium operation in double reverse flotation is achieved, saving the cost of flotation pH adjuster reagents.
[0128] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0129] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0130] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0131] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A reverse flotation desiliconization collector, characterized in that: The reverse flotation desiliconization collector includes alkyl polyamine, amide betaine and alkyl polyether.
2. The reverse flotation desiliconization collector according to claim 1, characterized in that: The amine groups of the alkyl polyamines include tertiary amine groups and quaternary amine groups; Preferably, the amide betaine includes one or a combination of at least two of myristic amide hydroxysulfopropyl betaine, lauryl amide hydroxysulfopropyl betaine or demeryl amide hydroxysulfopropyl betaine; Preferably, the alkyl polyether includes dodecyl polyoxyethylene ether and / or hexadecyl polyoxyethylene ether.
3. The reverse flotation desiliconization collector according to claim 1, characterized in that: The reverse flotation desiliconizing collector comprises, by weight: 5-7 parts of alkyl polyamine, 1-2 parts of amide betaine and 2-4 parts of alkyl polyether.
4. The method for preparing the reverse flotation desiliconization collector according to any one of claims 1 to 3, characterized in that: The preparation method comprises: mixing alkyl polyamine, amide betaine and alkyl polyether according to a formula to obtain a reverse flotation desiliconizing collector.
5. The use of the reverse flotation desiliconization collector according to any one of claims 1 to 3, characterized in that: The use includes using the reverse flotation desiliconization collector to reverse flotation desiliconize calcareous collophane ore.
6. The use according to claim 5, characterized in that The use includes: mixing and stirring the silico-calcium colloidal phosphate slurry with a reverse flotation desiliconizing collector, and then performing reverse flotation operations to obtain silicon tailings and phosphate concentrate.
7. The use according to claim 6, characterized in that The silico-calcium collophanite slurry is obtained by mixing silico-calcium collophanite ore and acidic reverse flotation magnesium removal return water and then grinding the mixture; Preferably, the calci-silico-collophane ore comprises, by mass percentage, P2O5 20-28%, SiO2 10-30%, and MgO 1.0-4.0%; Preferably, the acidic reverse flotation demagnesium return water comprises: 4000-7000 mg / L sulfate ions, 1500-4000 mg / L phosphate ions, 300-700 mg / L calcium ions and 500-1200 mg / L magnesium ions.
8. The use according to claim 6, characterized in that The slurry concentration of the calci-silico-collophane slurry is 20-40wt%; Preferably, the pH value of the calcium-silicon collophanite slurry is 5-7; Preferably, solid particles with a diameter of -0.074 mm in the calci-silico-collophane slurry account for 60-85% of the mass of all solid particles.
9. The use according to claim 6, characterized in that The mixing time is 3-5min; Preferably, the stirring speed of the mixing and stirring is 1.5-2 m / s.
10. The use according to claim 6, characterized in that: The reverse flotation operation performs at least one roughing operation and one scavenging operation; Preferably, the amount of the reverse flotation desiliconization collector added is 100-500 g / t; Preferably, the reverse flotation operation is a closed-circuit reverse flotation.