Method for regulating and controlling content of alloy elements in friction welding seam
By using modified material plates and constraint components to control the flow of alloying elements during friction welding, the problem of the inability to adjust the alloying element content in friction welds in existing technologies has been solved, thereby improving the performance of welded joints, especially the strength and toughness of titanium alloy welded joints.
Patent Information
- Application Number
- CN202411231870.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
Existing welding methods cannot adjust the alloy element content in friction welds, making it difficult to optimize the performance of welded joints.
During the welding process, modified material plates are placed on both sides of the workpiece to be welded and restraint components are used to control the flow of the modified material, so that it mixes with the base material interface to form a welded joint containing specific alloying elements.
This method enables the adjustment of weld metal element content during friction welding, thereby improving joint performance, particularly enhancing the strength and toughness of titanium alloy welded joints.
Smart Images

Figure CN118926672A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding, and more particularly to a method for regulating the content of alloy elements in a friction weld. Background Art
[0002] Materials with poor high-temperature plasticity, such as hard and brittle materials such as intermetallic compounds, are difficult to weld. Fusion welding is prone to cold cracks. Although friction welding can achieve welding, the process window is narrow. For the welding of titanium alloys, friction welding can obtain joints with higher strength than the parent material, but the plasticity and toughness are reduced. Continuous optimization and improvement of the mechanical properties of the joints is the development direction of welding technology.
[0003] When brazing / diffusion welding is used, the solder / intermediate layer composition can be adjusted to improve the joint performance; when fusion welding is used, the welding wire composition can be adjusted to improve the performance of the welded joint. Unlike these welding methods that can fill foreign materials in the weld, friction welding (mainly linear friction welding and inertia friction welding) is a process where two workpieces rub against each other to generate heat. After the interface reaches the welded state, the atoms on both sides of the welding interface diffuse under pressure to form a connection. The process of friction welding determines that the weld material can only be consistent with the parent material, which also leads to fewer variable factors in the linear friction welding process compared to other welding methods. For the welding of difficult-to-weld materials, performance can only be improved by optimizing the process parameters. For the welding of some materials, it may still be difficult to obtain a joint that meets the requirements by changing the process parameters. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The technical problem to be solved by the present invention is that the existing welding method cannot adjust the content of alloy elements in the friction weld.
[0006] (II) Technical solution
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] The present invention provides a method for regulating the content of alloy elements in a friction weld, which is used for friction welding a first plate and a second plate, and comprises the following steps:
[0009] A first modified material plate is disposed on one side of the first plate, and a first constraint portion is disposed on a side of the first modified material plate away from the first plate, so as to form a first workpiece to be welded;
[0010] A second modified material plate is laminated on one side of the second plate, and a second constraint portion is provided on a side of the second modified material plate away from the second plate, so as to form a second welded part; wherein both the first modified material plate and the second modified material plate contain specific alloy elements;
[0011] The end of the first workpiece to be welded and the second workpiece to be welded are mounted on a friction welding device, and the first workpiece to be welded and the second workpiece to be welded are friction welded. When the length shortening of the first workpiece to be welded or the second workpiece to be welded reaches a preset value, the welding is stopped to form a weld joint containing specific alloy elements.
[0012] Preferably, the first constraint portion is a third plate, the third plate is attached to the first constraint portion, and the first modified material plate is located between the first plate and the third plate;
[0013] Alternatively, the first constraint portion is a first cooling component, and the first cooling component is used to cool the first modifying material plate.
[0014] Preferably, when the first constraint portion is a third plate, the third plate is attached to the first modified material plate, and the first modified material plate is located between the first plate and the third plate, the first modified material plate is located at the geometric center of the first part to be welded.
[0015] Preferably, the second restraining portion is a fourth plate, the fourth plate is attached to the second modified material plate, and the second modified material plate is located between the second plate and the fourth plate;
[0016] Alternatively, the second constraint portion is a second cooling component, and the second cooling component is used to cool the second modified material plate.
[0017] Preferably, when the second constraint portion is a fourth plate, the fourth plate fits the second constraint portion, and the second modified material plate is located between the second plate and the fourth plate, the second modified material plate is located at the geometric center of the second part to be welded.
[0018] Preferably, the first constraint portion is a third modified material plate, the third modified material plate contains a specific alloy element, the third modified material plate is connected with the first modified material plate to form a first integrated structure, and the thickness of the first integrated structure is greater than the thickness of the first plate;
[0019] And / or, the second constraint portion is a fourth modified material plate, the fourth modified material plate contains specific alloy elements, the fourth modified material plate is connected to the second modified material plate to form a second integrated structure, and the thickness of the second integrated structure is greater than the thickness of the second plate.
[0020] Preferably, the first constraint portion is a third modified material plate, which contains specific alloy elements. The third modified material plate is connected to the first modified material plate to form a first integrated structure, and the thickness of the first integrated structure is greater than the thickness of the first plate; the second constraint portion is a limit plate, which is connected to the end face of the third modified material plate to form a limit groove for accommodating the second part to be welded.
[0021] Preferably, the friction welding device is a linear friction welding device, which has a moving end that moves along a first direction and a vibrating end that vibrates along a second direction, the first workpiece to be welded is clamped at the moving end, and the second workpiece to be welded is clamped at the vibrating end, wherein the first direction is perpendicular to the welding interface below the workpiece to be welded, and the second direction is perpendicular to the first direction.
[0022] Preferably, the friction welding device is an inertia friction welding device having a rotating end rotating about a third direction and a sliding end feeding along the third direction, the first workpiece to be welded is clamped at the rotating end, and the second workpiece to be welded is clamped at the sliding end.
[0023] Preferably, the first plate material and the second plate material are TC17 materials, and the first modified material plate and the second modified material plate are TC4 materials.
[0024] (III) Beneficial effects
[0025] The above technical solution of the present invention has at least the following advantages:
[0026] During the welding process, the first constraint part and the second constraint part can constrain the flow of the modified material in the plastic state generated on the welding interface, so that the outflow resistance of the metal toward the side where the first constraint part / the second constraint part is located increases, thereby causing the modified material in the plastic state to move toward the welding interface on the other side (i.e., the interface between the first plate and the second plate), thereby ensuring that the modified material in the plastic state (containing specific alloy elements) can be fully mixed with the base material in the plastic state at the welding interface to form a welded joint containing specific alloy elements. Through the above method, it is possible to adjust the content of alloy elements in the weld formed during friction welding, thereby adjusting and improving the performance of the joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 It is a schematic diagram of the implementation structure of the method for regulating the content of alloy elements in a friction weld provided in Example 1 of the present invention.
[0029] Figure 2 This is a metallographic diagram of a weld joint formed by the method for regulating the content of alloy elements in a friction weld provided in Example 1 of the present invention.
[0030] Figure 3 It is a schematic diagram of the implementation structure of the method for regulating the content of alloy elements in a friction weld provided in the second embodiment of the present invention.
[0031] Figure 4 This is a metallographic diagram of a weld joint formed by the method for regulating the content of alloy elements in a friction weld provided in the second embodiment of the present invention.
[0032] Figure 5 It is a schematic diagram of the implementation structure of the method for regulating the content of alloy elements in a friction weld provided in the third embodiment of the present invention.
[0033] Figure 6 It is a schematic diagram of the implementation structure of the method for regulating the alloy element content in the friction weld provided in the fourth embodiment of the present invention.
[0034] The reference numerals in the figures are:
[0035] 1. First plate; 2. Second plate; 3. First modified material plate; 4. Second modified material plate; 5. Third plate; 6. Fourth plate; 7. Third modified material plate; 8. Fourth modified material plate; 9. Limiting plate; 10. Limiting groove; A. First part to be welded; B. Second part to be welded; C. First integrated structure; D. Second integrated structure. DETAILED DESCRIPTION
[0036] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0037] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly located on the other element or indirectly located on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element.
[0038] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention, and do not indicate that a device or element must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0039] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating relative importance or indicating the number of technical features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The specific implementation of the present invention is described in more detail below in conjunction with specific embodiments:
[0040] like Figure 1 and Figure 2 As shown, an embodiment of the present invention provides a method for regulating the content of alloy elements in a friction weld, which is used for friction welding a first plate 1 and a second plate 2, and includes the following steps:
[0041] A first modified material plate 3 is laminated on one side of the first plate 1, and a first constraint portion is provided on a side of the first modified material plate 3 away from the first plate 1, so as to form a first welded part A;
[0042] A second modified material plate 4 is laminated on one side of the second plate 2, and a second constraint portion is provided on the side of the second modified material plate 4 away from the second plate 2, so as to form a second welded part B; wherein both the first modified material plate 3 and the second modified material plate 4 contain specific alloy elements;
[0043] The end of the first workpiece A to be welded and the second workpiece B to be welded are mounted on a friction welding device, and friction welding is performed on the first workpiece A to be welded and the second workpiece B to be welded. When the length shortening of the first workpiece A or the second workpiece B to be welded reaches a preset value, welding is stopped to form a weld joint containing specific alloy elements.
[0044] Linear friction welding is generally a joint formed by two metals with equal cross-sections rubbing against each other. The viscoplastic metal formed by friction on the interface continuously flows from the center of the interface to the outside to form flash. The metal flow follows the law of least resistance in plastic forming theory (the law that particles that may flow in different directions in a plastic deformation body only choose to flow in the direction with the least resistance), that is, for a sample with a certain contour, after entering a stable state during the welding process, each particle on the interface has a clear flow direction. For nearly homogeneous materials, the metal in the center flows to the surroundings, passing through other areas on the interface, and the material close to a certain edge will only flow to the side of the surface closer to it.
[0045] Based on the above principle, during the welding process, the first modified material plate 3 and the second modified material plate 4 generate heat by friction with each other, and a modified material in a plastic state is formed at the welding interface. The first constraint part and the second constraint part can constrain the flow of the modified material in a plastic state (having specific alloy elements), so that the modified material in a plastic state flows toward the welding interface between the first plate 1 and the second plate 2. As the welding process proceeds, under the action of the welding pressure, the modified material in a plastic state continuously flows along the welding interface between the first plate 1 and the second plate 2, and mixes with the plastic parent material formed by the friction heat generated by the first plate 1 and the second plate 2. After the welding is completed, a weld joint containing specific alloy elements is formed.
[0046] In one embodiment, if Figure 1 and Figure 2 As shown, the first constraint part is the third plate 5, the third plate 5 is attached to the first modified material plate 3, and the first modified material plate 3 is located between the first plate 1 and the third plate 5; in this embodiment, the first modified material plate 3 is located at the center of the first welded part A. During the welding process, the first modified material plate 3 and the second modified material plate 4 rub to form a modified material in a plastic state, and the modified material in a plastic state flows to the welding interface on both sides, and then fills the welding interface between the first plate 1 and the second plate 2, and the welding interface between the third plate 5 and the fourth plate 6. At the same time, the first plate 1 and the second plate 2 rub against each other, and the third plate 5 and the fourth plate 6 rub against each other to form a plastic state of the base material. The plastic state of the modified material (containing a specific alloy element) is mixed with the plastic state of the base material on the welding interface on both sides. After the welding is completed, a welded joint containing a specific alloy element is formed. In this embodiment, two required parts (i.e., two welded joints containing specific alloy elements) can be formed in the end, one of which is formed by welding the first plate 1 and the second plate 2, and the other is formed by welding the third plate 5 and the fourth plate 6. After welding is completed, machining cutting is performed along the center line of the first modified material plate 3 and the second modified material 4. After cutting, the first modified material plate 3 and the second modified material 4 are further machined to remove them, and the required parts can be obtained.
[0047] In another embodiment, Figure 5As shown, the first constraint part is a first cooling component, and the first cooling component is used to cool the first modified material plate 3. The second constraint part is a second cooling component, and the second cooling component is used to cool the second modified material plate 4. In this embodiment, the first cooling component and the second cooling component are both devices that can transport refrigerants, and can be specifically devices that can blow out cold air (refrigerant). The outlet of the cold air is toward the first modified material plate 3. The cold air is used to reduce the temperature of the first modified material plate 3, so that the interface temperature of the welded joint close to the first modified material plate 3 / second modified material plate 4 side is lower than the condition for generating burrs, and the metal outflow resistance is large, thereby causing the modified material in the plastic state to move toward the welding interface on the other side (i.e., the welding interface between the first plate 1 and the second plate 2), thereby ensuring that the modified material in the plastic state (containing specific alloy elements) can be mixed with the base material in the plastic state at the welding interface to form a welded joint containing specific alloy elements. Furthermore, the first cooling component and the second cooling component can also be pipes with coolant circulating inside, and the pipes are fitted on the first modified material plate 3 / the second modified material plate 4. The circulating coolant can exchange heat with the first modified material plate 3 / the second modified material plate 4, and take away the heat on the first modified material plate 3 / the second modified material plate 4, thereby cooling the first modified material plate 3 / the second modified material plate 4.
[0048] In one embodiment, if Figure 1 and Figure 2 As shown, the second constraint part is the fourth plate 6, the fourth plate 6 is attached to the second modified material plate 4, and the second modified material plate 4 is located between the second plate 2 and the fourth plate 6; the second modified material plate 4 is located at the geometric center of the second welded part B. In this embodiment, the function of the second constraint part is the same as that of the first constraint part mentioned above, and will not be repeated here; during the friction process, the modified material located at the geometric center position continues to flow to the outside of the joint, flowing through the welding interfaces on both sides, and as the welding process proceeds, the modified material covers the entire welding interface.
[0049] In one embodiment, if Figure 3 and Figure 4As shown, the first constraint part is the third modified material plate 7, which contains specific alloy elements. The third modified material plate 7 is connected with the first modified material plate 1 to form a first integrated structure C, and the thickness of the first integrated structure C is greater than the thickness of the first plate 1; the second constraint part is the fourth modified material plate 8, which contains specific alloy elements. The fourth modified material plate 8 is connected with the second modified material plate 4 to form a second integrated structure D, and the thickness of the second integrated structure D is greater than the thickness of the second plate 2. The second integrated structure D on the thicker side will produce greater resistance to the flow of the modified material in the plastic state, thereby making the modified material in the plastic state (containing specific alloy elements) more inclined to flow to the welding interface between the first plate 1 and the second plate 2, forming a welded joint containing specific alloy elements.
[0050] In one embodiment, if Figure 6 As shown, the first constraint part is the third modified material plate 7, which contains specific alloy elements. The third modified material plate 7 is connected to the first modified material plate 3 to form a first integrated structure C, and the thickness of the first integrated structure C is greater than the thickness of the first plate 1; the second constraint part is a limit plate 9, which is connected to the end face of the third modified material plate 7 to form a limit groove 10 for accommodating the second welded part B. The first modified material plate 3, the third modified material plate 7 and the limit plate 9 constitute a third integrated structure E. The third modified material plate 7 and the limit plate 9 can constrain the flow of the modified material in the plastic state, thereby making the modified material in the plastic state (containing specific alloy elements) more inclined to flow to the welding interface between the first plate 1 and the second plate 2, forming a welded joint containing specific alloy elements.
[0051] In one embodiment, the friction welding device is a linear friction welding device, which has a moving end that moves along a first direction and a vibrating end that vibrates along a second direction, a first workpiece to be welded is clamped at the moving end, and a second workpiece to be welded is clamped at the vibrating end, wherein the first direction is perpendicular to a welding interface below the workpieces to be welded, and the second direction is perpendicular to the first direction.
[0052] In one embodiment, the friction welding device is an inertia friction welding device having a rotating end rotating about a third direction and a sliding end feeding along the third direction, the first workpiece to be welded is clamped at the rotating end, and the second workpiece to be welded is clamped at the sliding end.
[0053] In one embodiment, the first plate 1 and the second plate 2 are made of TC17 material, and the first modified material plate 3 and the second modified material plate 4 are made of TC4 material.
[0054] In addition, the amount of modified layer material added to the material to be welded is related to the thickness of the modified material sample (i.e., the first modified material plate 3 and the second modified material plate 4) and the welding pressure. By adjusting the thickness and welding pressure of the modified material sample, the overall width of the weld and the amount of modified layer content therein can be regulated. The above measures are used to achieve modification and performance improvement of the joint of the material to be welded. After welding, the modified material sample is separated from the welded part by processing, or the modified material sample is removed to obtain a welded joint containing the modified layer alloy elements.
[0055] The following is a specific embodiment provided by the present invention:
[0056] In this embodiment, the part to be obtained is a TC17 titanium alloy welded joint. TC17 titanium alloy has high strength but low toughness. Compared with TC17 material, TC4 material has lower strength but significantly improved toughness. In certain applications, when it is necessary to improve the toughness of the welded joint, TC4 titanium alloy can be used as a modified material to improve the toughness of the joint.
[0057] Based on the above design ideas, in this embodiment, the first plate 1, the second plate 2, the third plate 5 and the fourth plate 6 are all made of TC17 titanium alloy plates with a length, width and height of 80mm×80mm×10mm. The requirements before welding are: the surface roughness of the two large surfaces of 80mm×80mm of the above plates is not greater than Ra1.6μm; the first modified material plate 3 and the second modified material plate 4 are made of TC4 titanium alloy plates with a length, width and height of 80mm×80mm×10mm, and it is also necessary to ensure that the surface roughness of the first modified material plate 3 and the second modified material plate 4 of 80mm×80mm is not greater than Ra1.6μm.
[0058] The first plate 1 and the third plate 5 are clamped on both sides of the first modified material plate 3, and the second plate 2 and the fourth plate 6 are clamped on both sides of the second modified material plate 4 to form two pairs of sandwich structures. After assembly, the layers need to be well fitted with a gap of less than 0.02 mm; Figure 1 The structure shown.
[0059] The first workpiece A to be welded is clamped at the vibrating end of the linear friction welding machine, and the second workpiece B to be welded is clamped at the moving end of the linear friction welding machine. The degree of freedom is fully constrained by the tooling, and the alignment accuracy error of the welding surfaces of the two pairs of test pieces is less than 0.1 mm.
[0060] The welding parameters can adopt the normal welding parameters of TC17, welding pressure 50MPa, frequency 40Hz, amplitude 3mm, shortening 5mm. During the welding process, TC4 material flows outward through the welding interface of TC17 material and is retained in the weld, making the weld material a mixture of TC17 and TC4 components. The addition of TC4 components can reduce the content of solid solution strengthening alloying elements of the original TC17 titanium alloy in the weld, increase the proportion of titanium and vanadium (specific alloying elements), and improve the toughness of the joint to a certain extent.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for regulating the content of alloying elements in a friction weld, characterized in that: For friction welding a first plate and a second plate, comprising the following steps: A first modified material plate is disposed on one side of the first plate, and a first constraint portion is disposed on a side of the first modified material plate away from the first plate, so as to form a first workpiece to be welded; A second modified material plate is laminated on one side of the second plate, and a second constraint portion is provided on a side of the second modified material plate away from the second plate, so as to form a second welded part; wherein both the first modified material plate and the second modified material plate contain specific alloy elements; The end of the first workpiece to be welded and the second workpiece to be welded are mounted on a friction welding device, and the first workpiece to be welded and the second workpiece to be welded are friction welded. When the length shortening of the first workpiece to be welded or the second workpiece to be welded reaches a preset value, the welding is stopped to form a weld joint containing specific alloy elements.
2. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The first constraint portion is a third plate, the third plate is attached to the first constraint portion, and the first modified material plate is located between the first plate and the third plate; Alternatively, the first constraint portion is a first cooling component, and the first cooling component is used to cool the first modifying material plate.
3. The method for controlling the alloying element content in a friction weld according to claim 2, characterized in that: When the first constraint portion is a third plate, the third plate is attached to the first modified material plate, and the first modified material plate is located between the first plate and the third plate, the first modified material plate is located at the geometric center of the first part to be welded.
4. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The second restraining portion is a fourth plate, the fourth plate is attached to the second modified material plate, and the second modified material plate is located between the second plate and the fourth plate; Alternatively, the second constraint portion is a second cooling component, and the second cooling component is used to cool the second modified material plate.
5. The method for controlling the alloying element content in a friction weld according to claim 4, characterized in that: When the second constraint portion is a fourth plate, the fourth plate fits the second constraint portion, and the second modified material plate is located between the second plate and the fourth plate, the second modified material plate is located at the geometric center of the second workpiece to be welded.
6. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The first constraint portion is a third modified material plate, the third modified material plate contains a specific alloy element, the third modified material plate is connected with the first modified material plate to form a first integrated structure, and the thickness of the first integrated structure is greater than the thickness of the first plate; And / or, the second constraint portion is a fourth modified material plate, the fourth modified material plate contains specific alloy elements, the fourth modified material plate is connected to the second modified material plate to form a second integrated structure, and the thickness of the second integrated structure is greater than the thickness of the second plate.
7. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The first constraint portion is a third modified material plate, which contains specific alloy elements. The third modified material plate is connected to the first modified material plate to form a first integrated structure, and the thickness of the first integrated structure is greater than the thickness of the first plate; the second constraint portion is a limiting plate, which is connected to the end face of the third modified material plate to form a limiting groove for accommodating the second part to be welded.
8. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The friction welding device is a linear friction welding device, which has a moving end that moves along a first direction and a vibrating end that vibrates along a second direction, the first workpiece to be welded is clamped at the moving end, and the second workpiece to be welded is clamped at the vibrating end, wherein the first direction is perpendicular to a welding interface below the workpiece to be welded, and the second direction is perpendicular to the first direction.
9. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The friction welding device is an inertia friction welding device having a rotating end rotating about a third direction and a sliding end feeding along the third direction, the first workpiece to be welded is clamped at the rotating end, and the second workpiece to be welded is clamped at the sliding end.
10. The method for controlling the alloying element content in a friction weld according to claim 1, characterized in that: The first plate material and the second plate material are TC17 materials, and the first modified material plate and the second modified material plate are TC4 materials.