Method for coating inner surface of glass bottle

Silica and copper oxide films are successively coated on the inner surface of the glass bottle by spraying, and laser curing technology is used to form a composite film layer, which solves the problem of low coating efficiency in the prior art and achieves efficient metal ion precipitation and Improved production efficiency and is suitable for storage bottles for microelectronics industrial reagents.

CN118930068AActive Publication Date: 2024-11-12CNBM RESEARCH INSTITUTE FOR ADVANCED GLASS MATERIALS GROUP CO LTD

Patent Information

Application Number
CN202410976462.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-20
Publication Date
2024-11-12
Estimated Expiration
2044-07-20

AI Technical Summary

Technical Problem

The existing glass bottle coating technology has low energy utilization efficiency and low processing efficiency, making it difficult to meet the high requirements of microelectronic industrial reagents for metal ion precipitation.

Method used

The inner surface of the glass bottle is coated with silica and copper oxide films in turn by spraying, and curing them at low temperatures through laser curing equipment to form a composite film layer, which improves laser energy absorption efficiency, reduces the temperature difference of the glass bottle, and improves production efficiency.

Benefits of technology

It realizes efficient metal ion precipitation, meets the requirements of microelectronics industrial reagent storage, improves the energy utilization efficiency and production efficiency of the coating process, and reduces the risk of glass bottle bursting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The invention relates to a method for coating the inner surface of a glass bottle. The method is characterized by comprising the following steps: (1) cleaning and drying the glass bottle; (2) coating the inner surface of the glass bottle with a silicon dioxide film by adopting a spraying method, taking out and drying at low temperature, coating the silicon dioxide film with a copper oxide film by adopting a spraying method, taking out and drying at low temperature, then coating the copper oxide film with a silicon dioxide film by adopting a spraying method, taking out and drying at low temperature; and (3) performing laser curing by adopting laser curing equipment, and cleaning after curing to obtain the glass bottle with the inner surface coated with the film. The method has the advantages that the copper oxide film layer is introduced into the composite structure film layer, the absorption efficiency of laser energy is improved, compared with a conventional high-temperature heating mode, laser curing has the advantages of being high in efficiency and energy utilization efficiency and capable of directly heating the film layer through glass, the temperature difference of the glass bottle before and after curing is reduced, the glass bottle is prevented from bursting, and the service life of the glass bottle is prolonged. The production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass bottle coating, and in particular to a method for coating the inner surface of a glass bottle. Background Art

[0002] Glass bottles are traditional packaging containers used to package beverages, alcoholic beverages, chemicals, medicines, etc. They have stable chemical properties, good barrier properties and sealing properties, and can effectively protect the contents from the influence of the external environment. Coating of glass bottles is a process of coating a metal or other compound film on the surface of the glass to change the optical, thermal, and electromagnetic properties of the glass bottle to meet specific usage requirements.

[0003] Reagents in the microelectronics industry have extremely high requirements for the precipitation of metal ions and other impurities in packaging materials, and glass materials have excellent optical, mechanical, thermal stability, chemical stability and other properties, and are excellent materials for the storage and packaging of reagents in the microelectronics industry. Reagents in the microelectronics industry are prone to react with alkali metals, so their storage conditions have very high requirements for the precipitation of metal ions in glass storage bottles. Surface treatment of glass bottles, such as coating their inner surfaces with functional films, can enable glass bottles to achieve the performance required by the application environment and meet the storage conditions of reagents. Due to the large size, heavy weight, and special shape of glass storage bottles (especially some special-shaped parts of the bottle mouth), coating is difficult. At present, the industrial coating of glass bottles adopts spraying and immersion methods, but conventional curing processes have disadvantages such as low energy utilization efficiency and low processing efficiency. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of low energy utilization efficiency and low processing efficiency in the process of coating glass in the prior art, and to provide a method for coating the inner surface of a glass bottle.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for coating the inner surface of a glass bottle, characterized by comprising the following steps: (1) Clean and dry the glass bottles to make the inner surface of the glass bottles suitable for coating; (2) coating the inner surface of the glass bottle with a silicon dioxide film by spraying, drying the glass bottle at low temperature after taking it out, coating the copper oxide film on the silicon dioxide film by spraying, drying the glass bottle at low temperature after taking it out, and coating the silicon dioxide film on the copper oxide film by spraying again, drying the glass bottle at low temperature after taking it out; (3) The glass bottle with the multi-layer film structure coated on the inner surface is subjected to laser curing by a laser curing device, and after the curing is completed, the glass bottle with the film coated on the inner surface is obtained by cleaning.

[0006] Furthermore, the cleaning and drying process in step (1) is as follows: the glass bottle is ultrasonically treated in pure water, alkaline cleaning agent, acidic cleaning agent and pure water for 20 to 60 minutes respectively, and then placed in a 75 to 85°C oven for drying.

[0007] Furthermore, the alkaline cleaning agent is 1-3% potassium hydroxide, 1-10% ethylenediaminetetraacetic acid, 1-5% gluconic acid, 2-5% isopropyl alcohol, 75-90% deionized water, and 2-10% surfactant, wherein the surfactant is one of sodium α-olefin sulfonate, sodium dodecylbenzene sulfonate, stearic acid, and the like.

[0008] Furthermore, the acidic cleaning agent is 5-15% citric acid, 10-25% acetic acid, 75-85% deionized water, and 2-10% non-ionic surfactant, wherein the non-ionic surfactant is one of alkyl glycoside, fatty acid glyceride, polyethylene glycol octylphenyl ether, etc.

[0009] Furthermore, the process of coating the thin film on the inner surface of the glass bottle by spraying in step (2) is as follows: placing the glass bottle mouth downward, atomizing the silicon dioxide coating liquid and the copper oxide particle dispersion liquid to obtain an atomized liquid, and then using a pressure nozzle device to spray the atomized liquid onto the inner surface of the glass bottle, so that the inner surface is evenly coated with a thin film.

[0010] Furthermore, the silica coating solution is composed of the following raw materials in mass percentage: 2-10% silica sol, 10-20% deionized water, and 75-85% alcohol, wherein the alcohol is one or a mixture of two or more of ethanol, ethylene glycol, and n-propanol.

[0011] Furthermore, the copper oxide particle dispersion is composed of the following raw materials in percentage by mass: 5-10% nano copper oxide particles, 20-30% stearic acid, 10-20% polyvinyl alcohol, 5-10% dimethylformamide, and 30-50% ethylene glycol.

[0012] Furthermore, the specific process of the spraying method in step (2) is as follows: the coating liquid is atomized at 0.2-0.8 MPa, and the pressure nozzle is a 360° omnidirectional rotating nozzle.

[0013] Furthermore, the conditions for laser curing in step (3) are: laser wavelength 1060nm, laser power 2W~8W.

[0014] The present invention has the following advantages: the present invention improves the absorption efficiency of laser energy by introducing a copper oxide film layer into the composite structure film layer, and compared with conventional high-temperature heating forms, laser curing has the advantages of high efficiency, high energy utilization efficiency, and the ability to directly heat the film layer through glass, thereby reducing the temperature difference of the glass bottle before and after curing, preventing the glass bottle from bursting, and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a graph showing the gold impurity precipitation test results for Examples 1-4. DETAILED DESCRIPTION

[0016] A method for coating the inner surface of a glass bottle, the specific implementation steps are as follows: The alkaline cleaning agent used in the following embodiments is composed of the following raw materials in weight percentage: 2% potassium hydroxide, 5% ethylenediaminetetraacetic acid, 3% gluconic acid, 4% isopropyl alcohol, 82% deionized water, and 4% sodium α-olefin sulfonate; the acidic cleaning agent is composed of the following raw materials in weight percentage: 6% citric acid, 16% acetic acid, 76% deionized water, and 2% alkyl glycoside. Example

[0017] (1) After ultrasonic treatment for 20 min in pure water, alkaline detergent, acidic detergent, and pure water, the glass bottle was placed in an oven at 80°C for drying; (2) Spray the inner surface of the dried glass bottle with 0.2Mpa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 8% silica sol, 12% deionized water, and 80% ethanol), and then place the bottle mouth downward in an 80°C oven for drying; (3) Spray the inner surface of the dried glass bottle with a 0.2 MPa atomized copper oxide particle dispersion (composed of the following raw materials in percentage by mass: 8% nano copper oxide particles, 22% stearic acid, 15% polyvinyl alcohol, 8% dimethylformamide, and 47% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (4) Spray the inner surface of the dried glass bottle with 0.2Mpa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 8% silica sol, 12% deionized water, and 80% ethanol), and then place the bottle mouth downward in an 80°C oven for drying; (5) Move the glass bottle into the infrared laser curing equipment, adjust the laser power to 2W and the laser wavelength to 1060nm to complete the curing of the composite film structure. Example

[0018] (1) After ultrasonic treatment for 40 min in pure water, alkaline detergent, acidic detergent, and pure water, the glass bottle was placed in an oven at 80°C for drying; (2) Spray the inner surface of the dried glass bottle with 0.5 MPa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 3% silica sol, 17% deionized water, and 80% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (3) Spray the inner surface of the dried glass bottle with a 0.5 MPa atomized copper oxide particle dispersion (composed of the following raw materials in percentage by mass: 6% nano copper oxide particles, 24% stearic acid, 12% polyvinyl alcohol, 8% dimethylformamide, and 50% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (4) Spray the inner surface of the dried glass bottle with 0.5 MPa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 3% silica sol, 17% deionized water, and 80% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (5) Move the glass bottle into the infrared laser curing equipment, adjust the laser power to 5W and the laser wavelength to 1060nm to complete the curing of the composite film structure. Example

[0019] (1) After ultrasonic treatment for 60 min in pure water, alkaline detergent, acidic detergent, and pure water, the glass bottle was placed in an oven at 80°C for drying; (2) Spray the inner surface of the dried glass bottle with 0.8Mpa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 5% silica sol, 18% deionized water, and 77% ethanol), and then place the bottle mouth downward in an 80°C oven for drying; (3) Spray the inner surface of the dried glass bottle with a 0.8 MPa atomized copper oxide particle dispersion (composed of the following raw materials in percentage by mass: 10% nano copper oxide particles, 28% stearic acid, 18% polyvinyl alcohol, 9% dimethylformamide, and 35% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (4) Spray the inner surface of the dried glass bottle with 0.8 MPa atomized acidic silica coating solution (composed of the following raw materials in percentage by mass: 5% silica sol, 18% deionized water, and 77% n-propanol), and then place the bottle mouth downward in an 80°C oven for drying; (5) Move the glass bottle into the infrared laser curing equipment, adjust the laser power to 8W and the laser wavelength to 1060nm to complete the curing of the composite film structure. Example

[0020] (1) After ultrasonic treatment for 30 min in pure water, alkaline detergent, acidic detergent, and pure water, the glass bottle was placed in an oven at 80°C for drying; (2) Spray the inner surface of the dried glass bottle with 0.6 MPa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 7% silica sol, 17% deionized water, 36% ethanol, and 40% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (3) Spray the inner surface of the dried glass bottle with a 0.6 MPa atomized copper oxide particle dispersion (composed of the following raw materials in percentage by mass: 7% nano copper oxide particles, 21% stearic acid, 17% polyvinyl alcohol, 7% dimethylformamide, and 48% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (4) Spray the inner surface of the dried glass bottle with 0.6 MPa atomized acidic silica coating liquid (composed of the following raw materials in percentage by mass: 7% silica sol, 17% deionized water, 36% ethanol, and 40% ethylene glycol), and then place the bottle mouth downward in an 80°C oven for drying; (5) Move the glass bottle into the infrared laser curing equipment, adjust the laser power to 4W and the laser wavelength to 1060nm to complete the curing of the composite film structure.

[0021] According to the method of Examples 1-4, a glass bottle with a composite film layer on the inner surface was obtained, and its performance was tested. The results of the gold impurity precipitation test are shown in Figure 1 : From the gold impurity precipitation test of Examples 1-4, it can be seen that the precipitation of B, Na, K, Ca, and Mg elements is less than 0.1ppb, which meets the relevant requirements of storage bottles for microelectronics industry reagents (metal ion precipitation is less than 0.1ppb), among which the most critical alkali metal element Na precipitates very little, close to 0, and is suitable for storage bottles for microelectronics industry reagents. Therefore, it can be known that the spray coating method can obtain better film quality and reduce the effect of gold impurity precipitation when the atomization is 0.2~0.8Mpa and the curing conditions are 1060nm laser wavelength and 2W~8W laser power.

[0022] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form; any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the above disclosed methods and technical contents without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. A method for coating the inner surface of a glass bottle, characterized in that The steps include: (1) Clean and dry the glass bottles; (2) coating the inner surface of the glass bottle with a silicon dioxide film by spraying, drying the glass bottle at low temperature after taking it out, coating the copper oxide film on the silicon dioxide film by spraying, drying the glass bottle at low temperature after taking it out, and coating the silicon dioxide film on the copper oxide film by spraying again, drying the glass bottle at low temperature after taking it out; (3) The glass bottle with the multi-layer film structure coated on the inner surface is subjected to laser curing by a laser curing device, and after the curing is completed, the glass bottle with the film coated on the inner surface is obtained by cleaning.

2. The method for coating the inner surface of a glass bottle according to claim 1, characterized in that: The cleaning and drying process in step (1) is as follows: the glass bottle is ultrasonically treated in pure water, alkaline cleaning agent, acidic cleaning agent and pure water for 20 to 60 minutes respectively, and then placed in a 75 to 85°C oven for drying.

3. The method for coating the inner surface of a glass bottle according to claim 1, characterized in that: The alkaline cleaning agent is 1-3% potassium hydroxide, 1-10% ethylenediaminetetraacetic acid, 1-5% gluconic acid, 2-5% isopropyl alcohol, 75-90% deionized water, and 2-10% surfactant, wherein the surfactant is one of sodium α-olefin sulfonate, sodium dodecylbenzene sulfonate, stearic acid, and the like.

4. The method for coating the inner surface of a glass bottle according to claim 1, characterized in that: The acidic cleaning agent is 5-15% citric acid, 10-25% acetic acid, 75-85% deionized water, and 2-10% non-ionic surfactant, wherein the non-ionic surfactant is one of alkyl glycoside, fatty acid glyceride, polyethylene glycol octylphenyl ether, etc.

5. The method for coating the inner surface of a glass bottle according to claim 1, characterized in that: The process of coating the inner surface of the glass bottle with a thin film by spraying in step (2) is as follows: placing the glass bottle mouth downward, atomizing the silicon dioxide coating liquid and the copper oxide particle dispersion liquid to obtain an atomized liquid, and then spraying the atomized liquid onto the inner surface of the glass bottle by using a pressure nozzle device, so that the inner surface is evenly coated with a thin film.

6. A method for coating the inner surface of a glass bottle according to claim 5, characterized in that: The silicon dioxide coating solution is composed of the following raw materials in mass percentage: 2-10% silicon dioxide sol, 10-20% deionized water, and 75-85% alcohol, wherein the alcohol is one of ethanol, ethylene glycol, n-propanol, etc., or a mixture of two or more thereof.

7. The method for coating the inner surface of a glass bottle according to claim 5, characterized in that: The copper oxide particle dispersion is composed of the following raw materials in percentage by mass: 5-10% nano copper oxide particles, 20-30% stearic acid, 10-20% polyvinyl alcohol, 5-10% dimethylformamide, and 30-50% ethylene glycol.

8. The method for coating the inner surface of a glass bottle according to claim 1, characterized in that: The specific process of the spraying method in step (2) is as follows: the coating liquid is atomized at 0.2-0.8 MPa, and the pressure nozzle is a 360° omnidirectional rotating nozzle.

9. A method for coating the inner surface of a glass bottle according to any one of claims 1 to 8, characterized in that: The conditions for laser curing in step (3) are: laser wavelength 1060nm, laser power 2W~8W.

Citation Information

Patent Citations

  • Cleaning agent for cleaning anti-reflection films of glass and cleaning process for anti-reflection films of glass

    CN109517676A

  • Microstructure-nano copper oxide synergistic antibacterial surface of stainless steel surface and laser-chemical composite preparation method and application of microstructure-nano copper oxide synergistic antibacterial surface

    CN111254433A

  • Preparation method of nano film-coating liquid

    CN113462275A

  • Preparation method of composite protective film layer with transition layer for glass bottle

    CN117623641A

  • Process for coating film on glass

    CN1907898A

Cited By

  • Preparation method of brown glass bottle for glue storage

    CN119954412A

  • A method for preparing a brown glass bottle for storing adhesives

    CN119954412B

  • Method for coating inner surface of glass container

    CN120040092A