Steel slag pressurized carbonization synergistic stabilization treatment method
By using pressure steaming and low-pressure carbonization in steel slag, the volume expansion problem caused by the hydration reaction of free oxides in steel slag is solved, its application in building materials is improved, and solidification is achieved by capturing CO2 exhaust gas Carbon reduces carbon emissions and environmental pollution.
Patent Information
- Application Number
- CN202410990053.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The hydration reaction of free calcium oxide and magnesium oxide in steel slag leads to volume expansion, causing product cracking, limiting its application in the field of building materials. The existing treatment methods cannot guarantee sufficient hydrolysis, and there are high energy consumption and environmental pollution problems.
The low-pressure carbonization coordinated stabilization treatment is carried out by step-by-step carbonization. First, the hydration of f-CaO and f-MgO is accelerated in a saturated water vapor environment by press-evaporation, and then the carbonization reaction is carried out in CO2 and humid and heat environment to generate CaCO3. and MgCO3 to enhance the stability of steel slag and cure carbon dioxide.
Effectively eliminate the potential for volume expansion of steel slag, improve stability, realize the comprehensive utilization of steel slag, and achieve carbon sequestration by capturing CO2 exhaust gas, reduce carbon emissions, and reduce environmental pollution.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for coordinating and stabilizing steel slag under pressure carbonization. Background Art
[0002] Steel slag is a kind of industrial solid waste, which is the slag discharged from steelmaking. It is formed at a temperature of 1500-1700℃, is liquid at high temperature, and becomes blocky after cooling. The main mineral phases are tricalcium silicate, dicalcium silicate, calcium magnesium olivine, calcium magnesium rhodonite, calcium ferroaluminate, and solid solution formed by oxides of silicon, magnesium, iron, manganese, and phosphorus. It also contains a small amount of free calcium oxide and metallic iron, fluoroapatite, etc. In some areas, because the ore contains titanium and vanadium, these components are also slightly contained in the steel slag. The content of various components in steel slag varies greatly due to the different steelmaking furnace types, steel types, and the smelting stages of each furnace.
[0003] Steel slag contains a certain amount of free calcium oxide (f-CaO) and magnesium oxide (f-MgO), which can react with water or moisture to convert into hydroxides, causing the slag to expand and break:
[0004] f-CaO+H2O==Ca(OH)2
[0005] f-MgO+H2O==Mg(OH)2
[0006] When the above two reactions are carried out, the system will expand violently. Since the free calcium and magnesium oxides in the overburned state in the steel slag are particularly dense in volume and react very slowly with water, the steel slag will cause cracking of the product due to volume expansion during long-term use, resulting in poor volume stability, which has a negative impact on the resource utilization of steel slag, especially in the field of building materials with a broad market, where its application is greatly restricted. Therefore, in order to solve the problem of poor stability of steel slag, it is necessary to cause the free calcium oxide (f-CaO) and magnesium oxide (f-MgO) in the steel slag to fully react with water in advance, and then use them in building materials to eliminate the hidden danger of volume expansion.
[0007] Existing slag stabilization treatment methods include hot pouring method, hot stewing method, drum method, etc., as follows:
[0008] (1) Hot pouring method: After the hot molten slag is poured into the slag pot, it is transported to the slag hot pouring workshop by vehicle, and the liquid slag in the slag pot is poured onto the slag bed (or slag pit) in layers by a crane. An appropriate amount of water is sprayed to quench and break the high-temperature slag and accelerate the cooling. The slag is then transported to the slag dump. The slag that needs to be processed is transported to the slag processing room for crushing, screening, magnetic separation and other process treatments.
[0009] (2) Hot-steaming method: hot molten slag is placed in a hot-steaming pool and sprinkled with water. The slag will be heated to a very high temperature, which accelerates the hydration of free calcium oxide and free magnesium oxide in the slag. Based on the traditional pool-steaming process, new bottom-sprinkling pool-steaming and pressurized closed container hot-steaming methods have emerged to further improve the processing efficiency. Specifically: ① Bottom-sprinkling pool-steaming method: the traditional top-sprinkling water is changed to bottom-sprinkling water. Since water sprays upward in the hot slag and quickly turns into steam, the slag-steaming process is actually achieved by the combined action of water and steam. The advantages are: first, it saves water, and the water consumption is about 1 / 3 to 1 / 2 of the traditional process; second, the water circulation treatment system is eliminated, reducing investment and operating costs; ② Pressurized closed container hot-steaming method: the hot slag is poured into an open hopper, first rolled and crushed by roller teeth, and then loaded into a closed material tank for water-sprinkling hot-steaming. The advantages are: first, it greatly improves the environment and the labor intensity of workers; second, it significantly shortens the slag processing time; third, it realizes the partial recovery of the sensible heat of the slag.
[0010] (3) Drum method: The steel slag is poured into a rotating drum with steel balls and water is poured into the drum. The steel slag is crushed and cooled by the impact of the steel balls in the rotating drum.
[0011] However, the above-mentioned slag stabilization treatment methods cannot ensure that f-CaO and f-MgO in the slag are fully hydrolyzed, which can easily cause serious cracking of slag products, which has a serious impact on the large-scale application of slag. At the same time, the slag is dense and hard, and it is difficult to crush and grind. There are also problems such as high water consumption, high energy consumption, factory smoke, extremely poor environment in the treatment area, and serious corrosion of equipment and factory buildings by corrosive smoke. The drum method with better stabilization treatment effect has a large investment and equipment maintenance, and the heat has not yet been recycled. Summary of the invention
[0012] In view of the following problems of poor stability of steel slag, the purpose of the present invention is to provide a method for coordinating and stabilizing steel slag with pressurized carbonization, which uses a step-by-step carbonization method to achieve low-pressure carbonization and coordinating stabilization of steel slag. The first step is pressure steam stabilization. Since steel slag contains f-CaO and f-MgO, and its structure is dense, hydration reaction is difficult to carry out. The full reaction of f-CaO and f-MgO in the steel slag with water is accelerated by a pressurized wet heat medium, thereby eliminating the harm caused by volume expansion of the steel slag during long-term use due to the hydration reaction of f-CaO and f-MgO. The second step is pressurized carbonization coordinating treatment, which captures CO2 emitted by the steel plant and coordinating the steel slag, so that the Ca(OH)2 and Mg(OH)2 generated by the hydration of f-CaO and f-MgO in the steel slag undergo carbonization reaction with CO2 in a wet and hot environment to generate CaCO3 and MgCO3, effectively solidifying carbon dioxide while improving the stability of the steel slag.
[0013] To achieve the above object, the present invention adopts the following technical solution:
[0014] The present invention provides a steel slag pressure carbonization coordinated stabilization treatment method, comprising the following steps:
[0015] (1) Stabilization treatment by autoclave: The slag is stabilized in a saturated steam environment;
[0016] (2) Low-pressure carbonization coordinated treatment: The steel slag treated in step (1) is placed in a mixture of CO2 and air at a certain pressure, humidity and concentration for low-pressure carbonization and stabilization simultaneous treatment.
[0017] Preferably, in step (1), the steel slag includes steel slag discharged from various smelting processes, which is crushed and magnetically separated and then wetted with water, the steel slag particle size is ≤10mm, and the water content of the steel slag is 5% to 20%.
[0018] Preferably, in step (1), the saturated water vapor pressure is less than 2.0 MPa.
[0019] Preferably, in step (1), saturated water vapor pressure is first injected into the sealed container until the total pressure reaches 1.1-2.0 MPa and then the constant pressure is maintained for 2-12 hours.
[0020] Preferably, the sealed container is an autoclave.
[0021] Preferably, in step (2), the steel slag after stabilization treatment by the autoclave method is placed in a carbonization device for low-pressure carbonization, and the carbonization duration is 0.5 to 6 hours.
[0022] Preferably, in step (2), the pressure of the mixed gas of CO2 and air is 0.1-0.5 MPa, the concentration of CO2 in the mixed gas is 10%-30%, and the relative humidity is 65%-75%.
[0023] Preferably, in step (2), the pressure-time product is used as the pressure carbonization synergistic stabilization treatment effect of the steel slag, and the pressure-time product refers to the steam pressure and the constant pressure duration, the unit is MPa.h, and the pressure-time product is 6 to 12 MPa.h.
[0024] In the above-mentioned steel slag pressure carbonization coordinated stabilization treatment method of the present invention, the reaction equations involved in each step are as follows:
[0025] (1) Pressure steam stabilization treatment process: After the steel slag is treated for 2 to 12 hours in a closed environment with a total pressure of CO2 and water vapor of 1.1 to 2.0 MPa, the f-CaO and f-MgO in the steel slag are partially converted into Ca(OH)2 and Mg(OH)2. The reaction equation for this step is as follows:
[0026] f-CaO+H2O==Ca(OH)2
[0027] f-MgO+H2O==Mg(OH)2
[0028] (2) Low-pressure carbonization synergistic treatment process: Using a certain partial pressure of carbon dioxide, under a certain humidity and time, the unhydrated f-CaO and f-MgO in the slag are converted into Ca(OH)2 and Mg(OH)2, while continuing to react with carbon dioxide and water to form calcium carbonate and magnesium carbonate. The reaction equation for this step is as follows:
[0029] Ca(OH)2+CO2+H2O==CaCO3+2H2O
[0030] Mg(OH)2+CO2+H2O==MgCO3+2H2O
[0031] The present invention also provides the application of the steel slag pressurized carbonization synergistic stabilization treatment method in preparing fine aggregate of premixed mortar, road base material and asphalt pavement material, concrete porous bricks and pavement bricks, fine aggregate of cement concrete and steel slag powder.
[0032] Compared with the prior art, the present invention adopts pressurized carbonization for the first time to treat steel slag in a coordinated manner, including pressure steam stabilization treatment and pressurized carbonization coordinated treatment. While achieving rapid digestion of f-CaO and f-MgO and eliminating poor stability of steel slag, it simultaneously absorbs CO2 to generate CaCO3 and MgCO3, achieves carbon fixation, and effectively reduces carbon emissions. The specific beneficial effects are:
[0033] (1) Effectively improve the stability of steel slag, achieve full hydration of f-CaO and f-MgO during the autoclave process, and lay the foundation for the comprehensive utilization of steel slag.
[0034] (2) Effectively utilize carbon dioxide exhaust gas emitted by steel mills to achieve sufficient carbon fixation and reduce carbon emissions.
[0035] (3) The processed steel slag can be utilized in a cascade manner, generating certain economic benefits. Particles larger than 5 mm can be used as coarse aggregate for asphalt concrete or roadbed materials, particles smaller than 5 mm can be used as fine aggregate, and steel slag powder can be used as an admixture for concrete and its products.
[0036] (4) After being processed, steel slag can be comprehensively utilized to eliminate environmental pollution caused by the storage of steel slag and reduce the land occupied by slag yards. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention will be described in detail below in conjunction with the embodiments of the present invention. However, the following embodiments are only used to understand the present invention and cannot limit the present invention.
[0038] The following embodiment provides a method for synergistic stabilization treatment of steel slag by pressure carbonization, the steps comprising: pressure steaming the steel slag in a closed environment of saturated water vapor, and then carbonizing it in a mixed gas of CO2 and air, wherein: the saturated water vapor pressure is <2.0MPa, the pressure of the mixed gas of CO2 and air is 0.1-0.5MPa, the concentration of CO2 in the mixed gas is 10%-30%, the relative humidity is 70%±5%, and the carbonization duration is 0.5-6h.
[0039] In one implementation, saturated water vapor is injected into a closed container, and when the saturated water vapor pressure reaches a design pressure value, the constant pressure time is 2 to 12 hours, and the design pressure value of the saturated water vapor pressure is 1.1 to 2.0 MPa.
[0040] In one embodiment, a CO2 mixed gas is first injected into a closed container, the pressure of the mixed gas of CO2 and air is 0.1-0.5 MPa, the concentration of CO2 in the mixed gas is 10%-30%, and the relative humidity is 70%±5%. Further, when the CO2 mixed gas reaches the design pressure, the constant pressure time is 0.5-6.0 hours.
[0041] In one embodiment, the steel slag includes steel slag discharged from various smelting processes.
[0042] In one embodiment, the steel slag is crushed to a particle size of less than 5 mm before entering the carbonization and stabilization treatment to achieve sufficient contact between f-CaO and f-MgO and water vapor and CO2 gas to ensure the effect of the carbonization and stabilization treatment.
[0043] In one embodiment, the steel slag is subjected to magnetic separation after being crushed to improve the utilization rate of iron.
[0044] Example 1
[0045] In this embodiment, the steel slag is subjected to pressure carbonization and coordinated stabilization treatment, and the steps are as follows:
[0046] (1) Crushing the steel slag to a particle size of less than 10 mm and performing magnetic separation.
[0047] (2) The steel slag treated in step 1 is placed in a closed environment of saturated water vapor for autoclave treatment, and then carbonized in a mixed gas of CO2 and air, wherein: the saturated water vapor pressure is reduced to <1.5 MPa, the constant pressure is maintained for 5 hours, the mixed gas pressure of CO2 and air is 0.20 MPa, the concentration of CO2 in the mixed gas is 20%, the relative humidity is 70%, and the carbonization duration is 2 hours.
[0048] Results Evaluation
[0049] (1) Environmental protection: no exhaust gas or wastewater discharge, dust atmospheric emission ≤30mh / Nm 3 .
[0050] (2) Properties of treated steel slag: pressure steam pulverization rate is 1.0%, water expansion rate is 0.03%, pressure steam expansion rate is 0.06%, and carbon fixation rate is 9.9%. Among them: the pressure steam pulverization rate is tested according to the national standard YB / T4329-2012 Technical Specifications for the Application of Steel Slag Sand for Cement Concrete Pavement, the water expansion rate is tested according to the national standard GB / T25824-2010 Steel Slag for Roads, and the pressure steam expansion rate is tested according to the national standard GB / T32546-2016 Technical Requirements for the Application of Steel Slag.
[0051] It can be seen from the performance test data that the properties of the steel slag treated in this embodiment are as follows: the pressure steam pulverization rate is ≤1.9% (the national standard YB / T4329-2012 Technical Specification for the Application of Steel Slag Sand for Cement Concrete Pavement requires ≤5.9%), the water expansion rate is ≤0.2% (the national standard GB / T25824-2010 Steel Slag for Roads requires: ≤2.0%), the pressure steam expansion rate is ≤0.07% (the national standard GB / T32546-2016 Technical Requirements for the Application of Steel Slag requires: ≤0.8%). The test method and the pilot method have been tested and verified many times. The performance of the treated steel slag is far better than the index requirements in the relevant standards. The treated steel slag can be widely used in: (1) fine aggregate for premixed mortar; (2) road base materials and asphalt pavement materials; (3) concrete porous bricks and pavement bricks; (4) fine aggregate for cement concrete; (5) steel slag powder, etc.
[0052] In summary, the steel slag pressure carbonization coordinated stabilization treatment method of the present invention can make the f-CaO and f-MgO in the steel slag fully digested in a saturated water vapor environment first, and then carry out low-pressure carbonization coordinated treatment, so as to achieve the dual effects of steel slag stabilization and effective carbon fixation. In particular, while effectively improving the stability of steel slag and realizing the comprehensive resource utilization of steel slag in civil engineering, it fully utilizes the CO2 tail gas captured by the steel plant, effectively realizes carbon fixation, reduces carbon emissions, accurately controls the carbonization effect, and eliminates the negative effects caused by excessive carbonization.
[0053] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for slag pressure carbonization and stabilization treatment, characterized in that: The following steps are involved: (1) Stabilization treatment by autoclave: The slag is stabilized in a saturated steam environment; (2) Low-pressure carbonization coordinated treatment: The steel slag treated in step (1) is placed in a mixture of CO2 and air at a certain pressure, humidity and concentration for low-pressure carbonization and stabilization simultaneous treatment.
2. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 1, characterized in that: In step (1), the steel slag includes steel slag discharged from a smelting process, which is crushed and magnetically separated and then wetted with water. The steel slag particle size is ≤10 mm and the water content of the steel slag is 5% to 20%.
3. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 1, characterized in that: In step (1), the saturated water vapor pressure is less than 2.0 MPa.
4. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 1, characterized in that: In step (1), saturated water vapor is injected into the sealed container until the total pressure reaches 1.1 to 2.0 MPa and then the constant pressure is maintained for 2 to 12 hours.
5. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 4, characterized in that: The closed container is an autoclave.
6. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 1, characterized in that: In step (2), the steel slag after the autoclave stabilization treatment is placed in a carbonization device for low-pressure carbonization, and the carbonization duration is 0.5 to 6 hours.
7. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 1, characterized in that: In step (2), the pressure of the mixed gas of CO2 and air is 0.1-0.5 MPa, the concentration of CO2 in the mixed gas is 10%-30%, and the relative humidity is 65%-75%.
8. The steel slag pressure carbonization coordinated stabilization treatment method according to claim 1, characterized in that: In step (2), the pressure-time product is used as the slag pressure carbonization synergistic stabilization treatment effect, and the pressure-time product refers to the steam pressure and the constant pressure duration, the unit is MPa.h, and the pressure-time product is 6 to 12 MPa.h.
9. Application of the steel slag pressurized carbonization synergistic stabilization treatment method according to any one of claims 1 to 8 in the preparation of fine aggregate for premixed mortar, road base materials and asphalt pavement materials, concrete porous bricks and pavement bricks, fine aggregate for cement concrete and steel slag powder.
Citation Information
Cited By
Gradient carbonization-silane coupling synergistically modified steel slag and ultrathin wearing layer preparation method
CN120271259A
A preparation method of gradient carbonization-silane coupling synergistically modified steel slag and ultra-thin wearing layer
CN120271259B