Anti-icing asphalt pavement and maintenance method thereof

Through the combination technology of heat storage phase change microcapsules and modified salt storage fibers, the anti-icing performance and stability of asphalt pavement are improved, and the problem of asphalt pavement is solved is solved, thus achieving more efficient and environmentally friendly Anti-ice-coagulation effect.

CN118930131AInactive Publication Date: 2024-11-12JIANGSU ZENGGUANG COMPOSITE MATERIAL TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410984031.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Asphalt pavement is prone to freezing under low temperature conditions, resulting in hindering highway operations. The existing method of spreading salt and melting ice consumes manpower and is harmful to the environment. It is necessary to develop asphalt pavement with better anti-icing performance.

Method used

Using the combination technology of heat storage phase change microcapsules and modified salt storage fibers, the heat storage phase change microcapsules are coated into the microcapsule structure through phase change material to improve heat storage and release capacity, and the modified salt storage fibers are slowed down through fiber materials. Release salt, reduce the impact of salt on asphalt pavement, and form long-term anti-coagulation ice performance.

Benefits of technology

It significantly improves the anti-coagulation ice performance and stability of asphalt pavement, reduces the impact of salt on the environment, extends the durability of anti-coagulation ice performance, and reduces the risk of road icing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956879310000101
    Figure BDA0004956879310000101
  • Figure BDA0004956879310000111
    Figure BDA0004956879310000111
Patent Text Reader

Abstract

The invention relates to an anti-freezing asphalt pavement and a maintenance method thereof, and relates to the technical field of asphalt, and the anti-freezing asphalt pavement comprises the following components in parts by mass: 80-160 parts of matrix asphalt, 100-200 parts of mineral powder, 800-1000 parts of coarse aggregate, 200-400 parts of fine aggregate, 10-20 parts of heat storage phase change microcapsules, and 15-20 parts of modified salt storage fibers. The maintenance method of the anti-freezing asphalt pavement comprises the following steps: cleaning the anti-freezing asphalt pavement, spraying the super-hydrophobic maintenance liquid to the anti-freezing concrete pavement, completing maintenance after spraying for 2-4 times, and performing maintenance operation once every 3-5 months. The anti-freezing asphalt pavement has the effect of improving the stability, the anti-freezing performance and the anti-skid performance of the anti-freezing asphalt pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of asphalt, and in particular to an anti-icing asphalt pavement and a maintenance method thereof. Background Art

[0002] Compared with cement concrete pavement, asphalt pavement has the advantages of smooth surface, low driving noise, small vibration and simple maintenance. It is an important structural form of my country's highways. Asphalt pavement is easy to freeze in winter. Highways in most provinces in my country have experienced serious icing in winter, which has caused difficulties in the normal operation of highways. The main hazards caused by road icing to highway transportation include traffic interruption, slow driving, frequent traffic accidents and even car crashes and deaths.

[0003] At present, the main solution adopted by the highway system for road icing is salting, that is, a large amount of ice-melting salts such as sodium chloride, potassium chloride and calcium chloride are artificially spread on the frozen road surface and area to melt the ice. Although this method has a significant ice-melting effect, it requires a lot of manpower and material resources, and a large amount of industrial salt left over will also pose a threat to the environment. Therefore, it is necessary to develop an asphalt pavement with anti-icing properties to prevent freezing rain from freezing on the road surface under low temperature conditions. Summary of the invention

[0004] In order to improve the anti-icing performance of asphalt, the present application provides an anti-icing asphalt pavement and a maintenance method thereof.

[0005] The anti-ice asphalt pavement provided in this application adopts the following technical solution: In the first aspect, the present application provides an anti-ice asphalt pavement, which adopts the following technical solution: An anti-icing asphalt pavement comprises the following components in parts by weight: 80-160 parts of base asphalt Mineral powder 100-200 parts Coarse aggregate 800-1000 parts Fine aggregate 200-400 parts 10-20 parts of heat storage phase change microcapsules 15-20 parts of modified salt-storing fiber.

[0006] The heat storage phase change microcapsule encapsulates the phase change material in the microcapsule structure. The microcapsule structure prevents the direct contact between the phase change material and the asphalt material, thereby improving the stability of the asphalt material and enabling the heat storage phase change microcapsule to better store and release heat through the phase change process, thereby improving the anti-icing performance of the asphalt pavement. The modified salt storage fiber stores the anti-icing agent in the fiber material, thereby reducing the impact of salt on the asphalt pavement and improving the stability of the asphalt pavement. The fiber material stores salt, which can play a slow-release role, allowing the anti-icing asphalt pavement to maintain good anti-icing performance for a long time.

[0007] Preferably, the raw materials for preparing the heat storage phase change microcapsules include modified phase change materials, polyaniline modified acrylate and nano titanium dioxide.

[0008] The heat storage phase change microcapsules prepared by modified phase change materials, polyaniline modified acrylate and nano-titanium dioxide have good anti-icing performance. The modified phase change materials are encapsulated by polyaniline modified acrylate and nano-titanium dioxide, so that the modified phase change materials can better exert their phase change performance; nano-titanium dioxide can reinforce the wall material structure of the microcapsules and increase the continuity of the heat storage phase change microcapsules. Nano-titanium dioxide can also absorb the energy of photons and convert them into thermal energy, thereby improving the heat storage capacity of the microcapsules and thus improving the anti-icing performance of the heat storage phase change microcapsules; the heat storage phase change microcapsules can reinforce the defects in asphalt materials, improve the self-healing ability of asphalt materials, and thereby improve the stability of asphalt materials.

[0009] Preferably, the raw materials for preparing the modified phase change material include diol and hexadecanoic acid.

[0010] The modified phase change material prepared by diol and hexadecanoic acid has a low melting point and high thermal stability. The modified phase change material has a diester structure, has a faster crystallization rate, can better perform phase transition under low temperature conditions, and has good anti-icing performance.

[0011] Preferably, the raw materials for preparing the polyaniline-modified acrylate include aniline, 2-hydroxyethyl methacrylate and ammonium persulfate.

[0012] Polyaniline is obtained by aniline doping polymerization. Polyaniline has good heat absorption and energy storage properties. It absorbs and releases heat through the transition of redox states, and synergizes with nano-titanium dioxide to improve the phase change properties of heat storage phase change microcapsules, thereby improving their anti-icing properties. 2-Hydroxyethyl methacrylate has abundant active groups and good reaction properties. It can react with asphalt to improve the system compatibility of heat storage phase change microcapsules, and can also play a role in reinforcing asphalt materials and improving the stability of asphalt materials.

[0013] Preferably, the mass ratio of the modified phase change material, polyaniline-modified acrylate and nano-titanium dioxide is 1:1:(0.02-0.05).

[0014] The heat storage phase change microcapsules prepared according to the above mass ratio have good phase change properties and can improve the anti-icing performance and stability of asphalt pavement.

[0015] Preferably, the modified salt-storing fiber comprises composite fiber, composite organic salt and branched polyethyleneimine.

[0016] The modified salt-storage fiber prepared by composite fiber, composite organic salt and branched polyethyleneimine has good anti-icing performance. The composite fiber absorbs a large amount of composite organic salt and is further wrapped by branched polyethyleneimine, which can effectively store salt, improve the sustained release performance of the modified salt-storage fiber, reduce salt precipitation, and improve anti-skid performance, anti-icing performance and durability. Branched polyethyleneimine has good reactivity and can react with asphalt materials to improve the system compatibility of asphalt pavement, thereby improving the stability of asphalt pavement.

[0017] Preferably, the composite fiber includes sepiolite fiber, lignin fiber and polyvinyl alcohol fiber.

[0018] The combination of sepiolite fiber, lignin fiber and polyvinyl alcohol fiber can synergistically toughen and reinforce asphalt materials, achieve an effective adsorption and desorption balance between the fibers, and effectively store salt, thereby improving the stability, anti-icing and anti-skid properties of asphalt pavement.

[0019] Preferably, the composite organic salt includes sodium silicate, sodium acetate and sodium carbonate.

[0020] The composite organic salt obtained by compounding sodium silicate, sodium acetate and sodium carbonate has good anti-icing performance. The organic salt is environmentally friendly. The synergistic effect of the three composite organic salts can effectively lower the freezing point and reduce the occurrence of icing through melting heat, and synergize with heat storage phase change microcapsules to improve the anti-icing performance of asphalt pavement.

[0021] In a second aspect, the present application provides a maintenance method for anti-icing asphalt pavement, which adopts the following technical scheme: A maintenance method for anti-icing asphalt pavement, comprising the following steps: Clean the anti-icing asphalt pavement, spray the super-hydrophobic curing liquid onto the anti-icing asphalt pavement, complete the curing after spraying 2-4 times, and perform the curing operation every 3-5 months.

[0022] By regularly spraying superhydrophobic curing liquid, a rough and hydrophobic micro-nano surface is constructed on the surface of the anti-icing asphalt pavement, which improves the hydrophobicity of the pavement, causes the droplets to roll off automatically, and delays the freezing time of the moisture on the pavement; the micro-nano rough surface can improve the swing value of the pavement and improve the anti-skid performance. The construction of the superhydrophobic layer can also reduce the wear on the asphalt pavement and improve the stability and durability of the anti-icing asphalt pavement.

[0023] Preferably, the super hydrophobic curing solution is prepared by the following steps: Nano-silicon dioxide is added to a mixed solvent of isopropanol and water to obtain a silicon dioxide dispersion, concentrated hydrochloric acid, heptadecafluorodecyltrimethoxysilane and dimethylphenylsilane are added to the silicon dioxide dispersion, methanol and acetone are added after stirring, and finally a silane coupling agent is added to obtain a mixed hydrophobic solution after stirring, the mixed hydrophobic solution is heated and stirred for reaction, and a super hydrophobic curing solution is obtained after cooling.

[0024] The super-hydrophobic curing liquid prepared according to the above steps has good hydrophobic properties. Nano-silicon dioxide is cross-linked with heptadecafluorodecyltrimethoxysilane and dimethylphenylsilane to form a nano-gel, and then mixed and cross-linked with a silane coupling agent to form a spatial network structure. It can construct a super-hydrophobic coating with a micro-nano structure on the anti-icing asphalt pavement. The fluorine atoms and phenyl groups of heptadecafluorodecyltrimethoxysilane and dimethylphenylsilane can further reduce the surface energy of the super-hydrophobic coating, improve the hydrophobic properties of the super-hydrophobic coating, and thereby improve the anti-icing performance of the anti-icing pavement.

[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. The heat storage phase change microcapsule encapsulates the phase change material in the microcapsule structure. The microcapsule structure prevents the direct contact between the phase change material and the asphalt material, improves the stability of the asphalt material, and enables the heat storage phase change microcapsule to better store and release heat through the phase change process, thereby improving the anti-icing performance of the asphalt pavement; the modified salt storage fiber stores the anti-icing agent in the fiber material, reduces the impact of salt on the asphalt pavement, and improves the stability of the asphalt pavement. The fiber material stores salt, which can play a slow-release role, so that the anti-icing asphalt pavement can maintain good anti-icing performance for a long time.

[0026] 2. The modified phase change material has a diester structure, has a faster crystallization rate, can better undergo phase transition under low temperature conditions, and has good anti-icing properties; polyaniline is obtained by aniline doping polymerization, and polyaniline has good heat absorption and energy storage properties. It absorbs and releases heat through the transition of redox states, and synergizes with nano-titanium dioxide to improve the phase change properties of the heat storage phase change microcapsules, thereby improving its anti-icing properties; the heat storage phase change microcapsules can reinforce the defects in asphalt materials, enhance the self-healing ability of asphalt materials, and thereby improve the stability of asphalt materials.

[0027] 3. The modified salt-storage fiber prepared by composite fiber, composite organic salt and branched polyethyleneimine has good anti-icing performance. The composite fiber adsorbs a large amount of composite organic salt and is further wrapped by branched polyethyleneimine, which can effectively store salt, improve the sustained release performance of the modified salt-storage fiber, reduce salt precipitation, and improve anti-skid performance, anti-icing performance and durability; branched polyethyleneimine has good reactivity and can react with asphalt materials to improve the system compatibility of asphalt pavement, thereby improving the stability of asphalt pavement. DETAILED DESCRIPTION

[0028] The present application discloses an anti-ice asphalt pavement and a maintenance method thereof. The raw materials used in the present application can be obtained from commercially available raw materials unless otherwise specified. The present application is further described in detail below in conjunction with the embodiments: Raw materials description: diol is 1,5-pentanediol (CAS No.: 111-29-5), hexadecanoic acid (CAS No.: 57-10-3), aniline (CAS No.: 62-53-3), 2-hydroxyethyl methacrylate (CAS No.: 868-77-9), ammonium persulfate (CAS No.: 7727-54-0), azobisisobutyronitrile (CAS No.: 78-67-1), Tween-80 (CAS No.: 9005-65-6), nano titanium dioxide purchased from Ningbo Jiwei Nano New Material Technology Co., Ltd., sodium silicate (CAS No.: 1344-09-8), sodium acetate (CAS No.: 127-09-3), sodium carbonate (CAS No.: 497-19-8), sepiolite fiber purchased from Lingshou County Keyue Mine Product processing plant, lignin fiber was purchased from Anfeng New Materials, polyvinyl alcohol fiber was purchased from Shandong Huahe New Materials Co., Ltd., branched polyethyleneimine was purchased from Hubei Keward Chemical Co., Ltd., matrix asphalt was purchased from German-Japanese Coal Chemical, mineral powder model was S95, coarse aggregate was gravel with an average particle size of 5 mm, fine aggregate was medium sand with an average particle size of 0.3 mm, nano silicon dioxide was purchased from Huifu Nano Materials, heptadecafluorodecyltrimethoxysilane (CAS No.: 83048-65-1), dimethylphenylsilane (CAS No.: 766-77-8), silane coupling agent was KH-550 (CAS No.: 919-30-2), acrylate (CAS No.: 1214-39-7), methyltriethoxysilane (CAS No.: 2031-67-6).

[0029] Example 1 Preparation of heat storage phase change microcapsules 3.43 kg of diol and 16.57 kg of hexadecanoic acid were mixed to obtain a mixture, and the mixture was melted in an oil bath at 100° C., 0.2 kg of ferric chloride hexahydrate was added to the melted mixture, and the mixture was reacted in an oil bath at 100° C. and a gauge pressure of 0.1 MPa for 8 hours. After the reaction mixture was cooled to below 30° C., it was washed three times with deionized water and ethanol respectively to obtain a modified phase change material.

[0030] The polyaniline-modified acrylate is obtained by in-situ polymerization of aniline, 2-hydroxyethyl methacrylate and ammonium persulfate, and the mass ratio of aniline, 2-hydroxyethyl methacrylate and ammonium persulfate is 1:5:0.5, so that the mass of the polyaniline-modified acrylate is 14.85 kg. 2-Hydroxyethyl methacrylate and 14.85kg of modified phase change material are mixed and dispersed in 200L of deionized water to obtain a mixed solution, 0.56kg of azobisisobutyronitrile and 3kg of Tween-80 are added to the mixed solution under 50°C water bath conditions, and a dispersed emulsion is obtained after homogenization for 30 minutes; aniline is dispersed in 20L of 1mol / L hydrochloric acid solution to obtain an aniline solution, ammonium persulfate accounting for 5% of the total mass of ammonium persulfate is added to the aniline solution, and a semi-oxidized polyaniline is obtained after reaction for 5 minutes, the semi-oxidized polyaniline and 0.3kg of nano-titanium dioxide are added to the dispersed emulsion and homogenized for 10 minutes, and the remaining ammonium persulfate is added to the homogenized emulsion, and after the emulsion turns black, the emulsion is stirred and reacted at 75°C at a speed of 400rpm for 6 hours, and the emulsion after the reaction is filtered, washed and dried to obtain a heat storage phase change microcapsule.

[0031] Preparation of modified salt-storing fiber 5kg of sodium silicate, 10kg of sodium acetate and 10kg of sodium carbonate were dispersed in 10L of deionized water, and stirred at 200rpm in a water bath at 80℃ to obtain a composite organic salt blend; 1kg of sepiolite fiber, 2kg of lignin fiber and 2kg of polyvinyl alcohol fiber were added to the composite organic salt blend, and stirred at 200rpm for 2h in a water bath at 100℃ to obtain a salt-storage fiber blend; the salt-storage fiber blend was dried at 150℃, crushed and sieved through a 900-mesh sieve to obtain salt-storage fiber; 21kg of the salt-storage fiber was added to 9kg of branched polyethyleneimine, stirred for 1h, and then dried at 160℃ to obtain modified salt-storage fiber.

[0032] Preparation of ice-resistant asphalt pavement 80 kg of base asphalt was heated and melted, 10 kg of heat storage phase change microcapsules and 15 kg of modified salt storage fibers were added to the melted base asphalt, and the mixture was kept at 180°C for 1 hour to obtain modified asphalt; 100 kg of mineral powder, 800 kg of coarse aggregate and 200 kg of fine aggregate were mixed and stirred to obtain a mixture, the mixture was heated to 180°C, mixed with modified asphalt, and kept at 180°C for 30 minutes to obtain an anti-ice asphalt mixture, which was paved on the road surface and compacted to obtain an anti-ice asphalt pavement.

[0033] Maintenance method of anti-ice asphalt pavement 1.2 kg of nano-silica was added to 100 L of a mixed solvent of isopropanol and water in a volume ratio of 3:1 to obtain a silica dispersion, 0.8 L of concentrated hydrochloric acid with a mass fraction of 98%, 3.5 kg of heptadecafluorodecyltrimethoxysilane and 2.7 kg of dimethylphenylsilane were added to the silica dispersion, 2 L of methanol and 1 L of acetone were added after stirring, and finally 2 kg of silane coupling agent was added, and the mixed hydrophobic solution was obtained after stirring at a speed of 200 rpm, the mixed hydrophobic solution was placed in a magnetic stirrer at 60 ° C and stirred at a speed of 50 rpm for 1 hour, and the super hydrophobic curing solution was obtained after cooling to 30 ° C.

[0034] Use a sweeper to clean the anti-icing asphalt pavement to remove the garbage and dust on the anti-icing asphalt pavement. Spray the super-hydrophobic curing liquid on the anti-icing concrete pavement. After spraying twice, the curing is completed and the curing operation is performed every 3 months.

[0035] Example 2 Preparation of heat storage phase change microcapsules 3.43 kg of diol and 16.57 kg of hexadecanoic acid were mixed to obtain a mixture, and the mixture was melted in an oil bath at 100° C., 0.2 kg of ferric chloride hexahydrate was added to the melted mixture, and the mixture was reacted in an oil bath at 100° C. and a gauge pressure of 0.1 MPa for 8 hours. After the reaction mixture was cooled to below 30° C., it was washed three times with deionized water and ethanol respectively to obtain a modified phase change material.

[0036] The polyaniline-modified acrylate is obtained by in-situ polymerization of aniline, 2-hydroxyethyl methacrylate and ammonium persulfate, and the mass ratio of aniline, 2-hydroxyethyl methacrylate and ammonium persulfate is 1:5:0.5, so that the mass of the polyaniline-modified acrylate is 14.63 kg. 2-Hydroxyethyl methacrylate and 14.63kg of modified phase change material are mixed and dispersed in 200L of deionized water to obtain a mixed solution, 0.56kg of azobisisobutyronitrile and 3kg of Tween-80 are added to the mixed solution under 50°C water bath conditions, and a dispersed emulsion is obtained after homogenization for 30 minutes; aniline is dispersed in 20L of 1mol / L hydrochloric acid solution to obtain an aniline solution, ammonium persulfate accounting for 5% of the total mass of ammonium persulfate is added to the aniline solution, and a semi-oxidized polyaniline is obtained after reaction for 5 minutes, the semi-oxidized polyaniline and 0.74kg of nano titanium dioxide are added to the dispersed emulsion and homogenized for 10 minutes, and the remaining ammonium persulfate is added to the homogenized emulsion, and after the emulsion turns black, the emulsion is stirred and reacted at 75°C at a speed of 400rpm for 6 hours, and the emulsion after the reaction is filtered, washed and dried to obtain a heat storage phase change microcapsule.

[0037] Preparation of modified salt-storing fiber 5kg of sodium silicate, 10kg of sodium acetate and 10kg of sodium carbonate were dispersed in 10L of deionized water, and stirred at 200rpm in a water bath at 80℃ to obtain a composite organic salt blend; 1kg of sepiolite fiber, 2kg of lignin fiber and 2kg of polyvinyl alcohol fiber were added to the composite organic salt blend, and stirred at 200rpm for 2h in a water bath at 100℃ to obtain a salt-storage fiber blend; the salt-storage fiber blend was dried at 150℃, crushed and sieved through a 900-mesh sieve to obtain salt-storage fiber; 21kg of the salt-storage fiber was added to 9kg of branched polyethyleneimine, stirred for 1h, and then dried at 160℃ to obtain modified salt-storage fiber.

[0038] Preparation of ice-resistant asphalt pavement 160 kg of base asphalt was heated and melted, 20 kg of heat storage phase change microcapsules and 20 kg of modified salt storage fibers were added to the melted base asphalt, and the mixture was kept at 180°C for 1 hour to obtain modified asphalt; 200 kg of mineral powder, 1000 kg of coarse aggregate and 400 kg of fine aggregate were mixed and stirred to obtain a mixture, the mixture was heated to 180°C, mixed with modified asphalt, and kept at 180°C for 30 minutes to obtain an anti-ice asphalt mixture, which was paved on the road surface and compacted to obtain an anti-ice asphalt pavement.

[0039] Maintenance method of anti-ice asphalt pavement 1.2 kg of nano-silica was added to 100 L of a mixed solvent of isopropanol and water in a volume ratio of 3:1 to obtain a silica dispersion, 0.8 L of concentrated hydrochloric acid with a mass fraction of 98%, 3.5 kg of heptadecafluorodecyltrimethoxysilane and 2.7 kg of dimethylphenylsilane were added to the silica dispersion, 2 L of methanol and 1 L of acetone were added after stirring, and finally 2 kg of silane coupling agent was added, and the mixed hydrophobic solution was obtained after stirring at a speed of 200 rpm, the mixed hydrophobic solution was placed in a magnetic stirrer at 60 ° C and stirred at a speed of 50 rpm for 1 hour, and the super hydrophobic curing solution was obtained after cooling to 30 ° C.

[0040] Use a sweeper to clean the anti-icing asphalt pavement to remove the garbage and dust on the anti-icing asphalt pavement. Spray the super-hydrophobic curing liquid on the anti-icing concrete pavement. After spraying 4 times, the curing is completed. The curing operation is carried out every 5 months.

[0041] Example 3 Preparation of heat storage phase change microcapsules 3.43 kg of diol and 16.57 kg of hexadecanoic acid were mixed to obtain a mixture, and the mixture was melted in an oil bath at 100° C., 0.2 kg of ferric chloride hexahydrate was added to the melted mixture, and the mixture was reacted in an oil bath at 100° C. and a gauge pressure of 0.1 MPa for 8 hours. After the reaction mixture was cooled to below 30° C., it was washed three times with deionized water and ethanol respectively to obtain a modified phase change material.

[0042] The polyaniline-modified acrylate is obtained by in-situ polymerization of aniline, 2-hydroxyethyl methacrylate and ammonium persulfate, and the mass ratio of aniline, 2-hydroxyethyl methacrylate and ammonium persulfate is 1:5:0.5, so that the mass of the polyaniline-modified acrylate is 14.74 kg. 2-Hydroxyethyl methacrylate and 14.74 kg of modified phase change material are mixed and dispersed in 200 L of deionized water to obtain a mixed solution, 0.56 kg of azobisisobutyronitrile and 3 kg of Tween-80 are added to the mixed solution under 50° C. water bath conditions, and a dispersed emulsion is obtained after homogenization for 30 minutes; aniline is dispersed in 20 L of 1 mol / L hydrochloric acid solution to obtain an aniline solution, ammonium persulfate accounting for 5% of the total mass of ammonium persulfate is added to the aniline solution, and a semi-oxidized polyaniline is obtained after reaction for 5 minutes, and the semi-oxidized polyaniline and 0.52 kg of nano titanium dioxide are added to the dispersed emulsion and homogenized for 10 minutes, and the remaining ammonium persulfate is added to the homogenized emulsion. After the emulsion turns black, the emulsion is stirred and reacted at 75° C. at a speed of 400 rpm for 6 hours, and the emulsion after the reaction is filtered, washed, and dried to obtain a heat storage phase change microcapsule.

[0043] Preparation of modified salt-storing fiber 5kg of sodium silicate, 10kg of sodium acetate and 10kg of sodium carbonate were dispersed in 10L of deionized water, and stirred at 200rpm in a water bath at 80℃ to obtain a composite organic salt blend; 1kg of sepiolite fiber, 2kg of lignin fiber and 2kg of polyvinyl alcohol fiber were added to the composite organic salt blend, and stirred at 200rpm for 2h in a water bath at 100℃ to obtain a salt-storage fiber blend; the salt-storage fiber blend was dried at 150℃, crushed and sieved through a 900-mesh sieve to obtain salt-storage fiber; 21kg of the salt-storage fiber was added to 9kg of branched polyethyleneimine, stirred for 1h, and then dried at 160℃ to obtain modified salt-storage fiber.

[0044] Preparation of ice-resistant asphalt pavement 120 kg of base asphalt was heated and melted, 15 kg of heat storage phase change microcapsules and 17.5 kg of modified salt storage fiber were added to the melted base asphalt, and the mixture was kept warm at 180°C for 1 hour to obtain modified asphalt; 150 kg of mineral powder, 900 kg of coarse aggregate and 300 kg of fine aggregate were mixed and stirred to obtain a mixture, the mixture was heated to 180°C, mixed with modified asphalt, and kept warm at 180°C for 30 minutes to obtain an anti-ice asphalt mixture, which was paved on the road surface and compacted to obtain an anti-ice asphalt pavement.

[0045] Maintenance method of anti-ice asphalt pavement 1.2 kg of nano-silica was added to 100 L of a mixed solvent of isopropanol and water in a volume ratio of 3:1 to obtain a silica dispersion, 0.8 L of concentrated hydrochloric acid with a mass fraction of 98%, 3.5 kg of heptadecafluorodecyltrimethoxysilane and 2.7 kg of dimethylphenylsilane were added to the silica dispersion, 2 L of methanol and 1 L of acetone were added after stirring, and finally 2 kg of silane coupling agent was added, and the mixed hydrophobic solution was obtained after stirring at a speed of 200 rpm, the mixed hydrophobic solution was placed in a magnetic stirrer at 60 ° C and stirred at a speed of 50 rpm for 1 hour, and the super hydrophobic curing solution was obtained after cooling to 30 ° C.

[0046] Use a sweeper to clean the anti-icing asphalt pavement to remove the garbage and dust on the anti-icing asphalt pavement. Spray the super-hydrophobic curing liquid on the anti-icing concrete pavement. After spraying 3 times, the curing is completed and the curing operation is carried out every 4 months.

[0047] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, the amount of modified phase change material is 14.92 kg, the amount of polyaniline modified acrylic acid obtained by in-situ polymerization is 14.92 kg, and the amount of nano titanium dioxide is 0.16 kg.

[0048] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the amount of modified phase change material used is 14.49 kg, the amount of polyaniline modified acrylic acid obtained by in-situ polymerization is 14.49 kg, and the amount of nano titanium dioxide used is 1.02 kg.

[0049] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, the modified phase change material used in preparing the heat storage phase change microcapsules is replaced with hexadecanoic acid.

[0050] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that aniline is not added when preparing the heat storage phase change microcapsules in Example 7.

[0051] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, 2-hydroxyethyl methacrylate used in preparing heat storage phase change microcapsules is replaced by acrylate.

[0052] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that nano titanium dioxide is not added when preparing the heat storage phase change microcapsules in Example 9.

[0053] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, the composite fiber is replaced by sepiolite fiber and polyvinyl alcohol fiber when preparing the modified salt-storage fiber.

[0054] Embodiment 11 Example 11 is based on Example 3. The only difference between Example 11 and Example 3 is that in Example 11, the composite fiber is replaced by lignin fiber when preparing the modified salt-storing fiber.

[0055] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that in Example 12, the composite organic salt is replaced by sodium silicate and sodium carbonate when preparing the modified salt-storing fiber.

[0056] Example 13 Example 13 is based on Example 3. The only difference between Example 13 and Example 3 is that in Example 13, the composite organic salt is replaced by sodium acetate when preparing the modified salt-storing fiber.

[0057] Embodiment 14 Example 14 is based on Example 3. The only difference between Example 14 and Example 3 is that no branched polyethyleneimine is added when preparing the modified salt-storing fiber in Example 14.

[0058] Embodiment 15 Example 15 is based on Example 3. The only difference between Example 15 and Example 3 is that in Example 15, dimethylphenylsilane used in preparing the super-hydrophobic curing liquid is replaced with methyltriethoxysilane.

[0059] Example 16 Example 16 is based on Example 3. The only difference between Example 16 and Example 3 is that in Example 16, heptadecafluorodecyltrimethoxysilane used in preparing the superhydrophobic curing liquid is replaced with methyltriethoxysilane.

[0060] Comparative Example 1 Comparative Example 1 is based on Example 3, and the only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, the heat storage phase change microcapsules are replaced by modified phase change materials.

[0061] Comparative Example 2 Comparative Example 2 is based on Example 3, and the only difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the modified salt-storing fiber is replaced by a composite organic salt.

[0062] Performance testing (1) The "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure" was selected as the standard. The anti-ice asphalt mixture was cast into a plate-shaped specimen and cured. Then the dynamic stability test was carried out. The dynamic stability was expressed by the number of times the wheel rolled when the rutting depth dropped by 1 mm. The more times, the better the dynamic stability of the specimen. Three specimens were prepared for each sample, and the average value was taken after measurement. The results are recorded in Table 1.

[0063] (2) Static anti-icing performance test: A sponge pull-out test was used. The specimens were prepared into Marshall specimens and cured. A sponge saturated with water was placed on the specimens. The specimens were then frozen at -10°C and 15°C for 4 h. The tensile force when the sponge was completely separated from the specimen was tested. Each specimen was tested three times, and the average value was taken after measurement. The results are recorded in Table 1.

[0064] (3) Dynamic anti-icing performance test: The anti-icing asphalt mixture was cast into block specimens. After curing, the dynamic stability rutting test was performed 2000 times. The rolled specimens were then flushed with running water for 48 hours at a flow rate of 100m / s. 3 / h, pressure of 3bar, after the surface moisture of the specimen is drained, dry it at 60℃ for 24h, and carry out the above-mentioned sponge pull test on the dried specimen to obtain the tensile force when the specimen and the sponge are completely separated; each specimen is tested three times, and the average value is taken after measurement, and the results are recorded in Table 1.

[0065] (4) Select "JTG / D50-2017 Highway Asphalt Pavement Design Specification" as the standard, and use a pendulum tribometer to test the anti-skid performance of anti-icing asphalt pavement. Prepare the sample and perform maintenance, test the surface pendulum value, the larger the pendulum value, the better the anti-skid performance of the pavement; each sample is tested three times, and the average value is taken after measurement, and the results are recorded in Table 1.

[0066] Table 1 Test results of stability, anti-icing performance and anti-skid performance of anti-icing asphalt pavement It can be seen from Table 1 that the dynamic stability of Examples 1-3 is greater than 5671 times / mm, the static anti-icing performance at -15°C is less than 6.25N, the dynamic anti-icing performance at -15°C is less than 7.87N, and the swing value is greater than 78BPN. It can be seen that the anti-icing asphalt pavement prepared in the present application has good stability, anti-icing performance and anti-skid performance.

[0067] As can be seen from Table 1, the only difference between Examples 4 and 5 and Example 3 is that in Example 4, the mass ratio of the modified phase change material, polyaniline modified acrylate and nano-titanium dioxide is 1:1:0.01, and in Example 5, the mass ratio of the modified phase change material, polyaniline modified acrylate and nano-titanium dioxide is 1:1:0.07. Compared with Example 3, the stability and anti-icing performance of Examples 4 and 5 are reduced. This is because the mass ratio of the modified phase change material, polyaniline modified acrylate and nano-titanium dioxide is not within the specified range. Too much or too little nano-titanium dioxide will affect the morphology and stability of the heat storage phase change microcapsules, and the heat storage phase change microcapsules will further affect the stability and anti-icing performance of the asphalt material, thereby reducing the stability and anti-icing performance.

[0068] As shown in Table 1, the only difference between Examples 6, 7, 8, and 9 and Example 3 is that in Example 6, the modified phase change material in the preparation of the heat storage phase change microcapsules is replaced with hexadecanoic acid, in Example 7, aniline is not added when the heat storage phase change microcapsules are prepared, in Example 8, 2-hydroxyethyl methacrylate is replaced with acrylate when the heat storage phase change microcapsules are prepared, and in Example 9, nano titanium dioxide is not added when the heat storage phase change microcapsules are prepared. Compared with Example 3, the stability, anti-icing performance, and anti-skid performance of Examples 6, 7, 8, and 9 are all reduced. This is because the synthetic components of the heat storage phase change microcapsules are replaced. Hexadecanoic acid has only a single ester group, and compared with the diester, its melting point is higher, its thermal stability is lower, its crystallization rate is lower, and its phase change performance is worse, thus affecting its anti-icing performance; there is a synergistic effect between aniline and nano-titanium dioxide, which helps in photothermal conversion and improves the heat storage performance of the microcapsules. The lack of one of them will affect the synergistic effect; replacing 2-hydroxyethyl methacrylate with acrylate will reduce the number of active groups of acrylate and reduce the system compatibility of the heat storage phase change microcapsules. These component changes will affect the performance of the heat storage phase change microcapsules, thereby reducing the stability, anti-icing performance and anti-slip performance.

[0069] As can be seen from Table 1, the only difference between Examples 10, 11, 12, 13, and 14 and Example 3 is that in Example 10, the composite fiber is replaced with sepiolite fiber and polyvinyl alcohol fiber when preparing the modified salt-storage fiber, in Example 11, the composite fiber is replaced with lignin fiber when preparing the modified salt-storage fiber, in Example 12, the composite organic salt is replaced with sodium silicate and sodium carbonate when preparing the modified salt-storage fiber, in Example 13, the composite organic salt is replaced with sodium acetate when preparing the modified salt-storage fiber, and in Example 14, branched polyethylene glycol is not added when preparing the modified salt-storage fiber. Amine, compared with Example 3, Examples 10, 11, 12, 13, and 14 have reduced stability, anti-icing performance, and anti-skid performance. This is because reducing the components in the composite fiber and the composite organic salt will destroy the synergistic effect, the salt storage performance of the composite salt-storage fiber will decrease, the salt will be more easily precipitated, and the anti-icing performance of the organic salt will decrease; when no branched polyethyleneimine is added, there is no resin to seal the salt-storage fiber, there is a lack of sustained-release effect, the salt is more easily precipitated and affects the asphalt material, thereby reducing the stability, anti-icing performance, and anti-skid performance.

[0070] As can be seen from Table 1, the only difference between Examples 15 and 16 and Example 3 is that in Example 15, the dimethylphenylsilane used in preparing the super-hydrophobic curing solution is replaced with methyltriethoxysilane, and in Example 16, the heptadecafluorodecyltrimethoxysilane used in preparing the super-hydrophobic curing solution is replaced with methyltriethoxysilane. Compared with Example 3, the anti-icing performance of Examples 15 and 16 is reduced. This is because dimethylphenylsilane or heptadecafluorodecyltrimethoxysilane is replaced with methyltriethoxysilane, lacking the introduction of phenyl and fluorine atoms, and the hydrophobic performance of the hydrophobic coating formed by the super-hydrophobic curing solution is reduced, the surface energy is increased, and thus the anti-icing performance is reduced.

[0071] It can be seen from Table 1 that the only difference between Comparative Example 1 and Example 3 is that Comparative Example 1 replaces the heat storage phase change microcapsules with modified phase change materials. Compared with Example 3, the stability, anti-icing performance and anti-skid performance of Comparative Example 1 are significantly reduced. This is because the modified phase change material lacks the encapsulation of microcapsules, and directly adding it to the asphalt material will affect the stability of the asphalt material, and the durability of the asphalt material will decrease. At the same time, due to the lack of auxiliary heat storage of microcapsules, the phase change performance of the modified phase change material is also reduced, so that the stability, anti-icing performance and anti-skid performance are significantly reduced.

[0072] It can be seen from Table 1 that the only difference between Comparative Example 2 and Example 3 is that Comparative Example 2 replaces the modified salt-storage fiber with a composite organic salt. Compared with Example 3, Comparative Example 2 lacks the encapsulation of the composite fiber and branched polyethyleneimine. Direct addition will affect the stability of the asphalt material, and the durability of the asphalt material will decrease, thereby significantly reducing the stability, anti-icing performance and anti-skid performance.

[0073] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. An anti-ice asphalt pavement, characterized by: The composition includes the following components in parts by weight: 80-160 parts of base asphalt Mineral powder 100-200 parts Coarse aggregate 800-1000 parts Fine aggregate 200-400 parts 10-20 parts of heat storage phase change microcapsules 15-20 parts of modified salt-storing fiber.

2. The anti-icing asphalt pavement according to claim 1, characterized in that: The raw materials for preparing the heat storage phase change microcapsule include modified phase change material, polyaniline modified acrylate and nano titanium dioxide.

3. The anti-icing asphalt pavement according to claim 2, characterized in that: The raw materials for preparing the modified phase change material include diol and hexadecanoic acid.

4. The anti-icing asphalt pavement according to claim 3, characterized in that: The raw materials for preparing the polyaniline-modified acrylate include aniline, 2-hydroxyethyl methacrylate and ammonium persulfate.

5. The anti-icing asphalt pavement according to claim 4, characterized in that: The mass ratio of the modified phase change material, polyaniline modified acrylate and nano titanium dioxide is 1:1:(0.02-0.05).

6. The anti-icing asphalt pavement according to claim 1, characterized in that: The modified salt-storing fiber comprises composite fiber, composite organic salt and branched polyethyleneimine.

7. The anti-icing asphalt pavement according to claim 6, characterized in that: The composite fiber comprises sepiolite fiber, lignin fiber and polyvinyl alcohol fiber.

8. The anti-icing asphalt pavement according to claim 7, characterized in that: The composite organic salt includes sodium silicate, sodium acetate and sodium carbonate.

9. A maintenance method for the anti-icing asphalt pavement as claimed in claim 1, characterized in that: The steps include: Clean the anti-icing asphalt pavement, spray the super-hydrophobic curing liquid onto the anti-icing asphalt pavement, complete the curing after spraying 2-4 times, and perform the curing operation every 3-5 months.

10. The curing method according to claim 9, characterized in that: The super hydrophobic curing solution is prepared by the following steps: Nano-silicon dioxide is added to a mixed solvent of isopropanol and water to obtain a silicon dioxide dispersion, concentrated hydrochloric acid, heptadecafluorodecyltrimethoxysilane and dimethylphenylsilane are added to the silicon dioxide dispersion, methanol and acetone are added after stirring, and finally a silane coupling agent is added to obtain a mixed hydrophobic solution after stirring, the mixed hydrophobic solution is heated and stirred to react, and a super hydrophobic curing solution is obtained after cooling.

Citation Information

Patent Citations

  • Micro-surfacing mixture with snow-melting function and preparation method of micro-surfacing mixture

    CN106396561A

  • Anti-freezing asphalt pavement structure and method for preparing pavement material

    CN112160212A

  • Anti-cracking asphalt concrete and preparation method thereof

    CN117383875A

  • Super-hydrophobic coating as well as preparation method and application thereof

    CN117887313A