Salt-tolerant carbomer as well as preparation method and application thereof

By combining acrylic monomers, thickeners and crosslinkers in a specific proportioning system, salt-resistant carbomers with a network structure are solved, and the problem of the viscosity of traditional carbomers decreases when encountering salt is achieved is achieved. Carbomer with viscosity and stability, suitable for pharmaceuticals and daily chemical products.

CN118930698AActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410979876.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Traditional carbomers are susceptible to extrusion when exposed to salt, resulting in a decrease in gel viscosity, limiting its widespread use in pharmaceuticals and daily chemical products.

Method used

By combining acrylic monomers, thickeners, initiators and crosslinking agents with specific contents in a specific proportioning system of cyclohexane and ethyl acetate, a network structure with multi-point crosslinking is formed, and The thickener is interspersed with the mesh polymer to improve the stability and salt resistance of carbomer.

Benefits of technology

The resulting salt-resistant carbomer has high viscosity and stability, with a viscosity retention rate of 56.8%, solving the problem of poor salt resistance of traditional carbomers and enhancing its application potential in pharmaceuticals and daily chemical products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955728700000021
    Figure BDA0004955728700000021
  • Figure BDA0004955728700000081
    Figure BDA0004955728700000081
  • Figure BDA0004955728700000091
    Figure BDA0004955728700000091
Patent Text Reader

Abstract

The invention relates to salt-tolerant carbomer as well as a preparation method and application thereof. The carbomer is prepared from the following raw materials in parts by weight: 8 to 12 parts of acrylic monomer, 30 to 70 parts of cyclohexane, 30 to 70 parts of ethyl acetate, 0.12 to 0.8 part of thickening agent, 0.01 to 0.2 part of initiator and 0.05 to 0.3 part of cross-linking agent. The salt-tolerant carbomer prepared by the invention has certain salt tolerance, can be better applied to solid preparations, semi-solid preparations and liquid preparations in medicines and daily chemical products, is mainly used as an adhesive, a suspending aid, a thickening agent and the like, and has great application value and scientific research significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional polymer materials, and in particular to a salt-resistant carbomer and a preparation method and application thereof. Background Art

[0002] Carbomer, also known as carboxy-polymethleme (CP), is a high molecular polymer cross-linked by acrylic acid and allyl sucrose. When dissolved in water, water molecules gradually diffuse into the interior of the polymer particles, and the carbomer molecules are in a swollen state and evenly dispersed in the water. It takes a long time for water molecules to diffuse into the interior of the particles, but its gel network is still loose, so it has good swelling properties in water, and after a certain period of time, it forms a colloid with high viscosity.

[0003] Carbomer is an important rheology modifier and an excellent gel matrix in the pharmaceutical industry. It is often used in solid, semi-solid and liquid preparations, and is mainly used as an adhesive, suspending agent and thickener. However, traditional carbomer is easily squeezed when it encounters salt in the preparation, causing the gel viscosity to decrease to 2%-10% of the original. This problem limits the wide application of carbomer.

[0004] Therefore, it is of great significance to provide a salt-resistant carbomer with good stability so that it can be widely used in the production of various pharmaceuticals and daily chemical products. Summary of the invention

[0005] In order to solve the above technical problems, the object of the present invention is to provide a salt-resistant carbomer and a preparation method and application thereof. The salt-resistant carbomer provided by the present invention has the characteristics of good salt resistance, high viscosity and good stability, and can be applied to pharmaceutical products and daily chemical products of solid preparations, semi-solid preparations and liquid preparations, meeting the needs of being used as an adhesive, suspending agent and thickener.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a salt-tolerant carbomer, wherein the raw materials for preparing the carbomer include the following components in parts by weight:

[0008]

[0009] The weight percentage of the acrylic monomer may be, for example, 8.2 parts, 8.5 parts, 8.8 parts, 9 parts, 9.5 parts, 10 parts, 10.5 parts, 11 parts or 11.5 parts.

[0010] The weight proportions of the cyclohexane may be, for example, 32 parts, 35 parts, 38 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts or 65 parts.

[0011] The weight proportions of the ethyl acetate may be, for example, 32 parts, 35 parts, 38 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts or 65 parts.

[0012] The weight proportion of the thickener may be, for example, 0.15 parts, 0.18 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, 0.6 parts or 0.7 parts.

[0013] The weight proportion of the initiator may be, for example, 0.02 parts, 0.04 parts, 0.06 parts, 0.08 parts, 0.1 parts, 0.12 parts, 0.14 parts, 0.16 parts or 0.18 parts.

[0014] The weight proportion of the cross-linking agent may be, for example, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts, 0.1 parts, 0.15 parts, 0.2 parts or 0.25 parts.

[0015] In the present invention, acrylic acid monomers, thickeners, initiators and crosslinking agents with specific contents are compounded under a specific ratio system of cyclohexane and ethyl acetate, wherein the crosslinking agent can form multi-point crosslinking between polymer main chains to form a network structure, and the thickener is interlaced with the network polymer after preparing the gel, and in the whole reaction system, the components cooperate with each other to exert a synergistic effect, so that the generated high molecular polymer has a relatively uniform and stable network structure, so that the obtained carbomer has good stability and salt resistance, thereby solving the technical problems in the prior art that the carbomer has poor salt resistance, is easily squeezed when encountering salt, resulting in reduced viscosity, and seriously reduced thickening ability.

[0016] Preferably, the acrylic monomer includes any one of acrylic acid, methyl acrylate, butyl acrylate or methyl methacrylate, or a combination of at least two thereof.

[0017] Preferably, the thickener comprises SAB and / or a food grade thickener, preferably SAB.

[0018] In the present invention, the specifically selected SAB and food-grade thickener not only have good compatibility, are conducive to the uniform dispersion of the raw material components, make the reaction system more stable, and facilitate cross-linking during monomer polymerization, thereby forming a stable network structure, and further improving the salt resistance; but also have an efficient thickening effect. When the added amount is 1%-10% of the acrylic acid monomer, the viscosity required by the hydrogel system can be achieved, and the thickening efficiency is high; at the same time, it also has high safety and can be better applied to medicines and daily chemical products.

[0019] Among them, SAB is an alkali swelling thickener. On the one hand, its structure contains a large number of EO hydrophilic segments. While forming a large number of hydrogen bonds with water to achieve a good thickening effect, it can reduce the compression of the double electric layer of ions in the salt-containing system, thereby achieving the purpose of maintaining good viscosity, and thus making the obtained product have excellent salt resistance. On the other hand, SAB also contains hydrophobic segments and -COOH groups. -COOH can ensure its good compatibility with carbomer molecules, while the hydrophobic segments can provide molecular rigidity, which is conducive to reducing the compression of ions on the carbomer molecular structure, and further improving the salt resistance stability of the product.

[0020] Preferably, the food-grade thickener comprises any one or a combination of at least two of gelatin, sodium caseinate, gum arabic, tamarind polysaccharide gum, sesbania gum, agar, sodium alginate or carrageenan;

[0021] Preferably, the initiator includes any one of dimethyl azobisisobutyrate, azobisisoheptanenitrile or azoisobutylcyanoformamide or a combination of at least two thereof, preferably dimethyl azobisisobutyrate.

[0022] In the present invention, the selected specific azo initiators, azobisisobutyric acid dimethyl ester (AIBME), azobisisoheptanitrile (ABVN) and azoisobutylcyanamide (CABN), not only have good initiation activity, but are also more conducive to long-term stable safe production compared to commonly used initiators. Commonly used initiators such as azobisisobutyronitrile (AIBN) decompose to generate solid tetramethylsuccinonitrile, which is not only harmful to the human body, but also easy to block equipment and pipelines in long-term production; and the decomposition process of dilauroyl peroxide (LPO) will produce oxygen, which not only inhibits polymerization and affects the reaction, but is also not conducive to production safety.

[0023] Among them, the decomposition temperature of dimethyl azobisisobutyrate (AIBME) is 65°C-85°C, which is suitable for the preparation reaction of the salt-resistant carbomer of the present invention, and its decomposition rate is less affected by solvent changes, which is beneficial to improving the stability of the entire reaction system; at the same time, the initiation activity of dimethyl azobisisobutyrate is moderate, so that the polymerization reaction is easy to control, there is no residue in the polymerization process, the product conversion rate is high, and the decomposition product is harmless.

[0024] Preferably, the crosslinking agent comprises any one of di-tert-butyl peroxy isopropylbenzene, diisopropylbenzene peroxide, divinylbenzene, diisocyanate or N,N-methylenebisacrylamide or a combination of at least two thereof, preferably di-tert-butyl peroxy isopropylbenzene and / or diisopropylbenzene peroxide.

[0025] In the present invention, unlike common cross-linking agents that need to connect linear polymers through cross-linking agent molecules, the cross-linking agents di-tert-butyl peroxyisopropylbenzene (BIPB) and diisopropylbenzene peroxide (DCP) used in the present invention can generate chemical bonds between linear molecules, so that the linear molecules are connected to each other through the carbon atoms of the main chain through CC bonds to form a network structure, thereby improving the strength and elasticity of the obtained carbomer, reducing the possibility of its chain breaking, and further producing a good salt resistance effect.

[0026] Under the specific solvent ratio system of the present invention, the half-lives of the initiator dimethyl azobisisobutyrate and the cross-linking agent di-tert-butylperoxyisopropylbenzene (BIPB) are basically the same at 55° C.-75° C., which can meet the requirements of uniform and controllable monomer polymerization rate and main chain cross-linking rate during the reaction process. The generated polymer structure is relatively uniform, which is beneficial to improving the stability and salt resistance of the product.

[0027] Preferably, the mass ratio of cyclohexane to ethyl acetate is (3:7)-(7:3), for example, it can be 3:7, 4:6, 4.5:5.5, 5:5, 5.5:4.5, 6:4 or 7:3, etc.

[0028] In the present invention, cyclohexane and ethyl acetate in a specific mass ratio are used as a mixed solvent. Ethyl acetate has excellent dissolving ability, is quick-drying and has low toxicity, which provides convenience for post-processing. Cyclohexane and ethyl acetate are highly miscible. Using the two as a common solvent can facilitate the adjustment of the polarity of the entire solvent, so that the low molecular weight primary polymer has good stability and will not precipitate from the solvent too early or too late. If the volume ratio of the two solvents is reduced or increased, the chain length of the polymerization intermediate will be too short or too long, and the predetermined molecular weight cannot be reached, thereby reducing the viscosity and salt resistance of the final product.

[0029] Preferably, the mass ratio of the thickener to the acrylic acid monomer is (0.025-0.067):1, for example, it can be 0.028:1, 0.03:1, 0.035:1, 0.04:1, 0.045:1, 0.05:1, 0.055:1, 0.06:1 or 0.065:1, etc.

[0030] In the present invention, the mass ratio of the thickener to the acrylic acid monomer is within a specific range, and the obtained carbomer has good viscosity and salt resistance. When the mass ratio is lower than 0.025:1, due to the low content of the thickener, the thickening effect is not obvious, so that the compatibility and stability of the system cannot be well improved, and the salt resistance of the obtained carbomer cannot be significantly improved; when the mass ratio is higher than 0.067:1, as the content of the thickener increases, the obtained carbomer does not swell in water, which is not conducive to the stability and uniformity of its viscosity.

[0031] Preferably, the mass ratio of the crosslinking agent to the acrylic acid monomer content is (0.015-0.022):1, for example, it can be 0.0155:1, 0.016:1, 0.0165:1, 0.017:1, 0.0175:1, 0.018:1 or 0.02:1, etc.

[0032] In the present invention, the mass ratio of the cross-linking agent to the acrylic acid monomer is within a specific range, and the obtained carbomer has good viscosity and salt resistance. When the mass ratio is lower than 0.015:1, due to the low content of the cross-linking agent, the degree of cross-linking between polymer molecules is low. Although the initial viscosity of the prepared hydrogel system is large, the molecular structure is easily compressed after adding salt due to the lack of rigidity of the polymer molecules, thereby reducing the salt resistance; when the mass ratio is higher than 0.022:1, due to the high content of the cross-linking agent, the cross-linking density increases, but the excessively high cross-linking density will reduce the maximum water absorption rate of the polymer, and the extension of the molecular chain of the polymer in the solution will be severely restricted, that is, the water solubility is reduced, so that the carbomer cannot be completely swelled in water, and a precipitate is formed, thereby significantly reducing its initial viscosity and failing to meet the use requirements.

[0033] In a second aspect, the present invention provides a method for preparing the salt-tolerant carbomer as described in the first aspect, the preparation method comprising the following steps:

[0034] Acrylic acid monomer, thickener, initiator and crosslinking agent are added into the mixed solvent to react and obtain the salt-resistant carbomer.

[0035] Preferably, the reaction is carried out under stirring.

[0036] Preferably, the reaction temperature is 55°C-75°C, for example, 57°C, 60°C, 62°C, 65°C, 68°C, 70°C or 72°C.

[0037] In the present invention, when the reaction temperature is lower than 55°C, the decomposition rate of the initiator is low, and sufficient free radicals cannot be formed for monomer polymerization, the polymerization reaction efficiency is low, the free radicals are easily inactivated by external influences, and only small molecular oligomers can be generated, the reaction cannot proceed normally, and the resulting product has low viscosity; when the reaction temperature is higher than 75°C, the system generates a large number of free radicals, the monomer reaction speed is too fast and uncontrolled, and implosion is likely to occur, the generated polymer has a wide molecular weight distribution and an uneven structure, thereby reducing the viscosity of the carbomer and further causing poor salt resistance.

[0038] Preferably, the reaction time is 7-9 h, for example, 7 h, 7.5 h, 8 h, 8.5 h or 9 h.

[0039] Preferably, the reaction is carried out under a protective gas atmosphere.

[0040] Preferably, the protective gas includes any one of nitrogen, argon or helium, or a combination of at least two of them.

[0041] Preferably, after the reaction is completed, a post-treatment step is further included.

[0042] Preferably, the post-processing steps include: cooling, washing, filtering, drying, and crushing and screening;

[0043] Preferably, the drying is vacuum drying.

[0044] Preferably, the vacuum drying temperature is 80°C-90°C, for example, it can be 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C.

[0045] Preferably, the vacuum drying time is 9-11 h, for example, it can be 9 h, 9.2 h, 9.5 h, 9.7 h, 10 h, 10.2 h, 10.5 h, 10.7 h or 11 h.

[0046] Preferably, the mesh size of the crushed and sieved sieve is 40 meshes.

[0047] Preferably, the preparation method of the salt-tolerant carbomer specifically comprises the following steps:

[0048] (1) mixing cyclohexane and ethyl acetate to obtain a mixed solvent;

[0049] (2) under a protective gas atmosphere, adding acrylic acid monomer, thickener, initiator and crosslinking agent to the mixed solvent of step (1), stirring and reacting at 55° C.-75° C. for 7-9 hours;

[0050] (3) The reaction solution of step (2) is cooled to 25° C., washed and filtered, vacuum dried at 80° C.-90° C. for 9-11 hours, and pulverized with a pulverizer to pass through a 40-mesh sieve to obtain the salt-tolerant carbomer.

[0051] In the present invention, a blending preparation method is adopted, which has simple process, convenient operation, low requirements on preparation conditions and is suitable for large-scale industrial production.

[0052] In a third aspect, the present invention provides a use of the salt-resistant carbomer as described in the first aspect in a medicament or daily chemical product.

[0053] Compared with the prior art, the present invention has at least the following beneficial effects:

[0054] (1) In the present invention, in a specific ratio system of cyclohexane and ethyl acetate, by compounding acrylic acid monomer, thickener, initiator and crosslinking agent with specific contents, the generated high molecular polymer has a relatively uniform network structure, so that the obtained carbomer has good stability and salt resistance, thereby solving the technical problems in the prior art that carbomer has poor salt resistance, is easily squeezed when encountering salt, resulting in reduced viscosity, and seriously reduced thickening ability;

[0055] (2) The present invention optimizes the raw materials for preparing carbomer, so that the obtained carbomer has high viscosity and stability as well as good salt resistance, and the viscosity retention rate measured at 25° C. can reach 56.8%;

[0056] (3) The present invention uses less thickener, initiator and cross-linking agent, which not only reduces the production cost but also helps to improve the safety of the obtained salt-resistant carbomer. DETAILED DESCRIPTION

[0057] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0058] The information of some raw materials involved in the specific implementation method is as follows:

[0059] SAB was purchased from Wanhua Chemical Group Co., Ltd. with the brand name Vesmody A401;

[0060] Dimethyl azobisisobutyrate was purchased from Liaoning Shuangqi Fine Chemical Co., Ltd.;

[0061] Di-tert-butylperoxyisopropylbenzene (BIPB) was purchased from Tianmen Hengchang Chemical Co., Ltd.;

[0062] Gelatin was purchased from MacLean Reagent Co., Ltd., brand name Gelatin G6317;

[0063] Gum Arabic was purchased from MacLean Reagent Co., Ltd. with the brand name Acacia A800707.

[0064] Example 1

[0065] This embodiment provides a salt-tolerant carbomer, the raw materials for preparing the carbomer include the following components in parts by weight:

[0066]

[0067] The preparation method of the salt-tolerant carbomer is as follows:

[0068] (1) mixing cyclohexane and ethyl acetate according to a formula to obtain a mixed solvent;

[0069] (2) Under a nitrogen atmosphere, the mixed solvent in step (1) was added to an oblique four-necked flask, and then acrylic acid, SAB, dimethyl azobisisobutyrate and di-tert-butyl peroxyisopropylbenzene were added in sequence according to the formula, and the mixture was stirred at 65° C. for 8 h;

[0070] (3) The reaction solution of step (2) is cooled to 25° C., washed and filtered, vacuum dried at 85° C. for 10 h, and pulverized with a grinder to pass through a 40-mesh sieve to obtain a white, fine, light powder of salt-tolerant carbomer.

[0071] Example 2

[0072] This embodiment provides a salt-tolerant carbomer, the raw materials for preparing the carbomer include the following components in parts by weight:

[0073]

[0074] The preparation method of the salt-tolerant carbomer is the same as that in Example 1.

[0075] Example 3

[0076] This embodiment provides a salt-tolerant carbomer, the raw materials for preparing the carbomer include the following components in parts by weight:

[0077]

[0078] The preparation method of the salt-tolerant carbomer is the same as that in Example 1.

[0079] Example 4

[0080] This embodiment provides a salt-tolerant carbomer, the raw materials for preparing the carbomer include the following components in parts by weight:

[0081]

[0082] The preparation method of the salt-tolerant carbomer is the same as that in Example 1.

[0083] Example 5

[0084] This embodiment provides a salt-tolerant carbomer, the raw materials for preparing the carbomer include the following components in parts by weight:

[0085]

[0086] The preparation method of the salt-tolerant carbomer is as follows:

[0087] (1) mixing cyclohexane and ethyl acetate according to a formula to obtain a mixed solvent;

[0088] (2) Under a nitrogen atmosphere, the mixed solvent in step (1) was added to an oblique four-necked flask, and then methyl methacrylate, gelatin, azoisobutylcyanamide and diisopropylbenzene peroxide were added in sequence according to the formula, and the mixture was stirred at 55° C. for 7 h;

[0089] (3) The reaction solution of step (2) is cooled to 25° C., washed and filtered, vacuum dried at 80° C. for 9 h, and pulverized with a grinder to pass through a 40-mesh sieve to obtain a white, fine, light powder of salt-tolerant carbomer.

[0090] Example 6

[0091] This embodiment provides a salt-tolerant carbomer, the raw materials for preparing the carbomer include the following components in parts by weight:

[0092]

[0093] The preparation method of the salt-tolerant carbomer is as follows:

[0094] (1) mixing cyclohexane and ethyl acetate according to a formula to obtain a mixed solvent;

[0095] (2) Under a nitrogen atmosphere, the mixed solvent in step (1) was added to an oblique four-necked flask, and then butyl acrylate, gum arabic, azobisisoheptanenitrile and diisopropylbenzene peroxide were added in sequence according to the formula, and the mixture was stirred at 75° C. for 9 h;

[0096] (3) The reaction solution of step (2) is cooled to 25° C., washed and filtered, vacuum dried at 90° C. for 11 h, and pulverized with a grinder to pass through a 40-mesh sieve to obtain a white, fine, light powder of salt-tolerant carbomer.

[0097] Example 7

[0098] The difference between this embodiment and embodiment 1 is that the weight portion of SAB is adjusted to 0.2 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0099] Example 8

[0100] The difference between this embodiment and embodiment 1 is that the weight portion of SAB is adjusted to 0.25 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0101] Example 9

[0102] The difference between this embodiment and embodiment 1 is that the weight portion of SAB is adjusted to 0.67 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0103] Example 10

[0104] The difference between this embodiment and embodiment 1 is that the weight portion of SAB is adjusted to 0.7 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0105] Embodiment 11

[0106] The difference between this embodiment and embodiment 1 is that the weight portion of di-tert-butyl peroxyisopropylbenzene is adjusted to 0.12 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0107] Example 12

[0108] The difference between this embodiment and embodiment 1 is that the weight portion of di-tert-butyl peroxyisopropylbenzene is adjusted to 0.15 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0109] Example 13

[0110] The difference between this embodiment and embodiment 1 is that the weight portion of di-tert-butyl peroxyisopropylbenzene is adjusted to 0.22 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0111] Embodiment 14

[0112] The difference between this embodiment and embodiment 1 is that the weight portion of di-tert-butyl peroxyisopropylbenzene is adjusted to 0.25 parts, and the other components, contents and preparation methods are the same as those in embodiment 1.

[0113] Comparative Example 1

[0114] The difference between this comparative example and Example 1 is that the weight parts of cyclohexane are adjusted to 20 parts, the weight parts of ethyl acetate are adjusted to 80 parts, and the other components, contents and preparation methods are the same as those in Example 1.

[0115] Comparative Example 2

[0116] The difference between this comparative example and Example 1 is that SAB is not added, the weight portion of acrylic acid is adjusted to 10.48 parts, and the other components, amounts and preparation methods are the same as those in Example 1.

[0117] Comparative Example 3

[0118] The difference between this comparative example and Example 1 is that the weight portion of SAB is adjusted to 0.1 part, and the other components, contents and preparation methods are the same as those in Example 1.

[0119] Comparative Example 4

[0120] The difference between this comparative example and Example 1 is that the weight portion of SAB is adjusted to 0.9 parts, and the other components, contents and preparation methods are the same as those in Example 1.

[0121] Comparative Example 5

[0122] The difference between this comparative example and Example 1 is that the weight portion of di-tert-butyl peroxyisopropylbenzene is adjusted to 0.04 parts, and the other components, contents and preparation methods are the same as those in Example 1.

[0123] Comparative Example 6

[0124] The difference between this comparative example and Example 1 is that the weight portion of di-tert-butylperoxyisopropylbenzene is adjusted to 0.32 parts, and the other components, contents and preparation methods are the same as those in Example 1.

[0125] Comparative Example 7

[0126] The difference between Comparative Example 1 and Example 1 is that in the preparation method of this comparative example, the reaction temperature of step (2) is 50°C.

[0127] Comparative Example 8

[0128] The difference between Comparative Example 1 and Example 1 is that in the preparation method of this comparative example, the reaction temperature of step (2) is 80°C.

[0129] The carbomer provided in Examples 1-14 and Comparative Examples 1-8 was subjected to a salt tolerance test, and the test method was as follows:

[0130] At 25°C, 0.5% carbomer hydrogel was prepared, and the pH value was adjusted to 7.35-7.45 with 18% sodium hydroxide solution; the viscosity value η was measured with a Brookfield DV2 viscometer. 水 Then, sodium chloride was added at a ratio of 1%, and the viscosity value η after adding NaCl was measured by Brookfield DV2 viscometer 盐 , the viscosity retention rate μ of carbomer is calculated using formula (1):

[0131] μ=(η 盐 ÷η 水 )×100% (1)

[0132] Among them, the larger the μ, the better the salt resistance.

[0133] The test results are shown in Table 1:

[0134] Table 1

[0135]

[0136] The test results show that:

[0137] (1) It can be seen from Examples 1-14 that the present invention optimizes the components and contents of the raw materials of carbomer so that the salt-tolerant carbomer obtained has good viscosity and salt resistance, and its viscosity retention rate can reach 56.8% at 25°C.

[0138] (2) By comparing Example 1 with Examples 7-10, it can be seen that when the weight portion of SAB is 0.48 parts, the mass ratio of SAB to acrylic acid is 0.048:1, and the obtained carbomer has the best salt resistance; when the mass ratio of SAB to acrylic acid is 0.02:1, due to the low content of SAB, the thickening effect is not obvious, so that the compatibility and stability of the system cannot be well improved, and thus the salt resistance of the obtained carbomer cannot be significantly improved; when the mass ratio of SAB to acrylic acid is 0.07:1, due to the high content of SAB, the carbomer does not swell in water, which is not conducive to the stability and uniformity of its viscosity. Therefore, when the mass ratio of SAB to acrylic acid exceeds the preferred mass ratio of the present invention (0.025-0.067):1, the viscosity and viscosity retention rate of the obtained salt-resistant carbomer are reduced, that is, the salt resistance is poor.

[0139] (3) By comparing Example 1 with Examples 11-14, it can be seen that when the weight portion of di-tert-butyl peroxy isopropylbenzene is 0.16 parts, the mass ratio of di-tert-butyl peroxy isopropylbenzene to acrylic acid is 0.016:1, and the obtained carbomer has the best salt resistance; when the mass ratio of the two is 0.012:1, due to the low content of di-tert-butyl peroxy isopropylbenzene, the degree of crosslinking between polymer molecules is low. Although the initial viscosity of the prepared hydrogel system is large, the lack of rigidity of the polymer molecules causes the molecular structure to be easily compressed after adding salt, thereby reducing the salt resistance; when the mass ratio of the two is 0.025:1, due to the high content of di-tert-butyl peroxy isopropylbenzene, the crosslinking density increases, but the excessively high crosslinking density will reduce the maximum water absorption rate of the polymer, and the extension of the molecular chain of the polymer in the solution will be severely restricted, that is, the water solubility is reduced, so that the carbomer cannot be completely swelled in water, forming a precipitate, thereby significantly reducing its initial viscosity and failing to meet the use requirements. Therefore, when the mass ratio of the two exceeds the preferred mass ratio of the present invention (0.015-0.022):1, the viscosity and viscosity retention rate of the obtained salt-resistant carbomer are reduced, that is, the salt resistance is poor.

[0140] (4) By comparing Example 1 with Comparative Example 1, it can be seen that the contents of cyclohexane and ethyl acetate exceed the specific range of the present invention, and the mass ratio of the two is less than 3:7, and the salt resistance of the salt-resistant carbomer obtained is poor. In the present invention, the polarity of the entire solvent system is adjusted by adjusting the mass ratio between cyclohexane and ethyl acetate, so that the low molecular weight primary polymer has good stability and does not precipitate from the solvent too early or too late. If the mass ratio of the two solvents is reduced or increased, the chain length of the polymerization intermediate will be too short or too long, and the predetermined molecular weight cannot be reached, thereby reducing the viscosity and salt resistance of the final product.

[0141] (5) By comparing Example 1 with Comparative Examples 3 and 4, it can be seen that when the content of the thickener is less than 0.12 parts, the salt resistance of the obtained carbomer is poor; when the content is higher than 0.8 parts, the resistance performance obtained is higher, but the viscosity of the product is significantly poor, which is not conducive to the practical application of the product.

[0142] (6) By comparing Example 1 with Comparative Examples 5 and 6, it can be seen that when the content of the cross-linking agent is less than 0.05 parts, although the initial viscosity of the prepared hydrogel system is large, due to the lack of rigidity of the polymer molecules, the molecular structure is easily compressed after the addition of salt, thereby reducing the salt resistance; when the content of the cross-linking agent is higher than 0.3 parts, although it obtains high salt resistance, it has a poor viscosity value and cannot meet the actual use requirements.

[0143] (7) By comparing Example 1 with Comparative Examples 7 and 8, it can be seen that when the reaction temperature of the system is lower than 55°C, it has a poor viscosity value. Although the salt resistance is increased, it cannot meet the actual use needs; when the temperature of the system is higher than 75°C, the salt resistance of the product is poor.

[0144] In summary, the present invention is compounded under a specific ratio system of cyclohexane and ethyl acetate by specific contents of acrylic acid monomer, thickener, initiator and cross-linking agent, and the generated high molecular polymer has a relatively uniform network structure, so that the obtained carbomer has good stability and salt resistance, thereby solving the technical problems in the prior art that carbomer has poor salt resistance, is easily squeezed when encountering salt, resulting in reduced viscosity, and seriously reduced thickening ability.

[0145] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A salt-tolerant carbomer, characterized in that: The raw materials for preparing the carbomer include the following components in parts by weight:

2. The salt-tolerant carbomer according to claim 1, characterized in that The acrylic monomer includes any one or a combination of at least two of acrylic acid, methyl acrylate, butyl acrylate or methyl methacrylate; Preferably, the thickener comprises SAB and / or a food grade thickener; Preferably, the food-grade thickener comprises any one or a combination of at least two of gelatin, sodium caseinate, gum arabic, tamarind polysaccharide gum, sesbania gum, agar, sodium alginate or carrageenan; Preferably, the initiator comprises any one of dimethyl azobisisobutyrate, azobisisoheptanenitrile or azoisobutylcyanoformamide or a combination of at least two thereof; Preferably, the crosslinking agent includes any one of di-tert-butyl peroxyisopropylbenzene, diisopropylbenzene peroxide, divinylbenzene, diisocyanate or N,N-methylenebisacrylamide, or a combination of at least two thereof.

3. The salt-tolerant carbomer according to claim 1 or 2, characterized in that The mass ratio of cyclohexane to ethyl acetate is (3:7)-(7:3).

4. The salt-tolerant carbomer according to any one of claims 1 to 3, characterized in that The mass ratio of the thickener to the acrylic acid monomer is (0.025-0.067):1; Preferably, the mass ratio of the cross-linking agent to the acrylic acid monomer content is (0.015-0.022):

1.

5. A method for preparing the salt-tolerant carbomer according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Acrylic acid monomer, thickener, initiator and crosslinking agent are added into the mixed solvent to react and obtain the salt-resistant carbomer.

6. The preparation method according to claim 5, characterized in that: The reaction is carried out under stirring; Preferably, the reaction temperature is 55°C-75°C; Preferably, the reaction time is 7-9 hours.

7. The preparation method according to claim 5 or 6, characterized in that: The reaction is carried out under a protective gas atmosphere; Preferably, the protective gas includes any one of nitrogen, argon or helium, or a combination of at least two of them.

8. The preparation method according to any one of claims 5 to 7, characterized in that: After the reaction is completed, a post-processing step is also included; Preferably, the post-processing steps include: cooling, washing, filtering, drying, and crushing and screening; Preferably, the drying is vacuum drying; Preferably, the vacuum drying temperature is 80°C-90°C; Preferably, the vacuum drying time is 9-11 hours; Preferably, the mesh size of the crushed and sieved sieve is 40 meshes.

9. The preparation method according to any one of claims 5 to 8, characterized in that: The preparation method specifically comprises the following steps: (1) mixing cyclohexane and ethyl acetate to obtain a mixed solvent; (2) under a protective gas atmosphere, adding acrylic acid monomer, thickener, initiator and crosslinking agent to the mixed solvent of step (1), stirring and reacting at 55° C.-75° C. for 7-9 hours; (3) The reaction solution of step (2) is cooled to 25° C., washed and filtered, vacuum dried at 80° C.-90° C. for 9-11 hours, and pulverized with a pulverizer to pass through a 40-mesh sieve to obtain the salt-tolerant carbomer.

10. Use of the salt-tolerant carbomer according to any one of claims 1 to 4 in medicines or daily chemical products.

Citation Information

Patent Citations

  • Alkyl acrylate copolymer dispersants and uses thereof

    CN101130710A

  • Carbomer and preparation method thereof

    CN103483491A

  • Method for preparing medicinal auxiliary material Carbomer

    CN106632801A

  • Carbomer thickening agent capable of being quickly wetted and dispersed and preparation method thereof

    CN114195943A

  • Carbomer resin and preparation method therefor

    WO2017036001A1