Hardening film, preparation method thereof and flexible display device

By forming a silicon-containing hardened coating on the flexible plastic substrate and enhancing the wear-resistant layer, combined with the anti-fouling layer, the deficiencies in the hardened film in bending, wear resistance and cold and cold impact resistance are solved, and the hardened film and The stability and stain resistance of flexible display devices are improved.

CN118930930APending Publication Date: 2024-11-12CHINA LUCKY GROUP CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410862117.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for existing hardened films to achieve the effects of bending resistance, high wear resistance and cold and cold impact resistance at the same time, especially on flexible plastic substrates, stress accumulation and separation problems caused by material performance differences.

Method used

The silicon-containing raw materials are used to form a hardened coating by hydrolysis and condensation, and the chemical vapor deposition is enhanced on its surface to form a wear-resistant layer, forming a composite film layer to improve wear resistance and cold and cold impact resistance, while on flexible substrates Add anti-fouling layer to improve overall performance.

Benefits of technology

It achieves good bending, wear and cold impact resistance of the hardened film, ensures the firm combination of the film layer and the substrate, and improves the stability and anti-fouling effect of the flexible display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930930A_ABST
    Figure CN118930930A_ABST
Patent Text Reader

Abstract

The invention discloses a hardened film, a preparation method thereof and a flexible display device. The method for preparing the hardened film comprises the following steps: providing a flexible substrate; at least one hardened wear-resistant composite layer is formed on at least one side of the flexible base material, the hardened wear-resistant composite layer comprises a hardened coating and a wear-resistant layer, and the wear-resistant layer is located on the surface, away from the flexible base material, of the hardened coating; the step of forming the hardened wear-resistant composite layer comprises the following steps that a first raw material forms a hardened coating on one side of the flexible base material through hydrolytic condensation, the first raw material comprises a first compound shown in the formula (1) or a mixture of the first compound and a second compound shown in the formula (2), the formula (1) is X-Y-SiR'n (OR) 3-n, the formula (2) is Si (OR '') 4, and n is equal to 0, 1 or 2; and a silicon source compound is used as a second raw material, and a plasma enhanced chemical vapor deposition method is adopted to form a wear-resistant layer on the surface, away from the flexible base material, of the hardened coating. Therefore, the hardened wear-resistant composite layer has good wear resistance and cold and hot impact resistance, and the hardened wear-resistant composite layer is firmly combined with the flexible base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of hardened films, and in particular to a hardened film and a preparation method thereof, and a flexible display device. Background Art

[0002] In recent years, display technology and flexible materials have developed rapidly, the process of flexible display equipment has become more and more mature, and the related flexible display terminal market has continued to expand. Among them, folding display products have developed the fastest and most mature. Folding display products usually require a folding radius of 1mm to 2mm. Therefore, not only the outer protective material needs to have excellent bending resistance, but also excellent wear resistance and / or anti-fouling performance. Although traditional glass materials have excellent hardness and wear resistance, they have poor flexibility, poor impact resistance, and no anti-fouling performance. Hardened films based on flexible plastic substrates are an important alternative to glass materials, but it is still a challenge to simultaneously achieve anti-bending, high wear resistance, and resistance to cold and hot shocks on flexible plastic substrates.

[0003] Therefore, the current hardened film and preparation method thereof and flexible display device still need to be improved. Summary of the invention

[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems:

[0005] The current hardening film is difficult to achieve the effects of anti-bending, high wear resistance, and resistance to cold and hot shocks at the same time, and needs to be improved.

[0006] Many inorganic thin film materials have natural advantages over organic materials in terms of hardness and scratch resistance, such as silicon oxide, silicon nitride, aluminum oxide, diamond-like carbon, etc. These materials have been used as wear-resistant coatings for a long time. However, the substrate of this type of inorganic wear-resistant coating is usually a hard material such as metal. If a flexible plastic substrate is used, there are usually the following problems: on the one hand, the heat resistance of the plastic substrate is limited, and the deposition process of the inorganic wear-resistant layer is limited; on the other hand, the thermomechanical properties between the plastic substrate and the inorganic wear-resistant material are quite different, and more stress will be accumulated during the film formation process, resulting in subsequent separation from the plastic substrate after bending, scratching, and cold and hot shocks. The inventor found that some silicon-containing raw materials can be used to form a hardened coating on a flexible plastic substrate through hydrolysis and condensation, and then plasma-enhanced chemical vapor deposition is used to form a wear-resistant layer on the surface of the hardened coating. The obtained composite film layer can have good wear resistance and cold and hot shock resistance at the same time. The composite film layer is combined with a flexible plastic substrate, and the obtained hardened film has good bending resistance, wear resistance, and cold and hot shock resistance.

[0007] The present invention aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.

[0008] In one aspect of the present invention, the present invention proposes a method for preparing a hardened film. In some embodiments of the present invention, the method for preparing a hardened film includes: providing a flexible substrate; forming at least one hardened wear-resistant composite layer on at least one side of the flexible substrate, wherein the hardened wear-resistant composite layer includes a hardened coating and a wear-resistant layer, and the wear-resistant layer is located on the surface of the hardened coating away from the flexible substrate; forming the hardened wear-resistant composite layer includes the following steps: a first raw material is hydrolyzed and condensed to form the hardened coating on one side of the flexible substrate, the first raw material includes a first compound represented by formula (1) or a mixture of the first compound and the second compound represented by formula (2), XY-SiR' n (OR) 3-n Formula (1), Si(OR")4 Formula (2), n = 0, 1 or 2; X is selected from epoxy, epoxycyclohexane, acrylate or methacrylate; Y is selected from C 1~6 Alkylene, C 6~20 or a C having an ether bond, an acyl group, a urea group or a carbamate group in the chain or at the end. 1~6 Alkylene or C 6~20 Each R and each R' in formula (1) are independently selected from C 1~6 Alkyl, C 2~6 The alkenyl group, C 3~6 Alkynyl, C 6~20 Each R" in formula (2) is independently selected from C 1~6 Alkyl, C 2~6 The alkenyl group, C 3~6 Alkynyl, C 6~20 The first raw material comprises a mixture of a first compound and a second compound, and the mass ratio of the second compound to the first compound is ≤10:1; the silicon source compound is used as the second raw material, and the wear-resistant layer is formed on the surface of the hardened coating away from the flexible substrate by a plasma enhanced chemical vapor deposition method. Thus, the prepared hardened wear-resistant composite layer has good wear resistance and resistance to cold and hot shocks, and the hardened wear-resistant composite layer is firmly bonded to the flexible substrate, so that the hardened film can maintain good stability while achieving good flexibility.

[0009] In some embodiments of the present invention, one hardened wear-resistant composite layer is formed on both sides of the flexible substrate respectively; or, a plurality of hardened wear-resistant composite layers are formed on at least one side of the flexible substrate, and the plurality of hardened wear-resistant composite layers are stacked.

[0010] In some embodiments of the present invention, the first raw material further includes at least one of silicon oxide, aluminum oxide, titanium oxide nanoparticles and colloids; and / or the first raw material further includes at least one of an initiator and a cross-linking agent. This is conducive to further improving the overall performance of the hardened film.

[0011] In some embodiments of the present invention, the method for preparing a hardened film satisfies at least one of the following conditions: the wear-resistant layer is prepared under the condition of the presence of a first gas, the first gas includes oxygen, and the flow ratio of the silicon source compound to the first gas is 1:20-1:6; the silicon source compound includes hexamethyldisiloxane; when forming the wear-resistant layer, the plasma discharge power density is 0.5 kW / m 2 -10kw / m 2 The gas pressure of the reaction zone where the wear-resistant layer is formed is 0.1-10 Pa. When the wear-resistant layer is formed, the magnetic field strength at the flexible substrate is 5GS-100GS. Thus, the wear-resistant layer prepared has good wear resistance and is not prone to scratches after multiple frictions.

[0012] In some embodiments of the present invention, the first gas is oxygen; or, the first gas includes oxygen and an inert gas, and a flow ratio of the inert gas to the first gas is ≤1:5.

[0013] In some embodiments of the present invention, the method for preparing a hardened film satisfies at least one of the following conditions: the material of the flexible substrate includes at least one of transparent polyimide, cycloolefin polymer, polyethylene naphthalate and polyethylene terephthalate; the thickness of the flexible substrate is 5μm-188μm; the thickness of the hardened coating is 1μm-30μm; the thickness of the wear-resistant layer is 50nm-500nm.

[0014] In some embodiments of the present invention, the method for preparing a hardened film further includes: a third raw material is hydrolyzed and condensed to form an antifouling layer on the side of the outermost hardened wear-resistant composite layer away from the flexible substrate, and the third raw material forming the antifouling layer includes a first siloxane, and the first siloxane contains fluorine. As a result, the antifouling layer has a good waterproof and oil-proof effect, and the bonding force between the antifouling layer and the hardened wear-resistant composite layer is strong, which is conducive to improving the overall performance of the hardened film.

[0015] In some embodiments of the present invention, the method for preparing a hardened film satisfies at least one of the following conditions: the first siloxane includes at least one of heptadecafluorodecyltrimethoxysilane, perfluorooctylethyltriethoxysilane, perfluorohexylethyltriethoxysilane, trifluoropropyltriethoxysilane, trifluoropropyltrimethoxysilane, and perfluorohexylethyltriethoxysilane; the third raw material also includes a second siloxane, the second siloxane does not contain fluorine, and the second siloxane includes at least one of KH550 silane coupling agent and A187 silane coupling agent; the third raw material also includes a second siloxane, the second siloxane does not contain fluorine, and the mass ratio of the first siloxane to the second siloxane is ≥1:2; the thickness of the anti-fouling layer is 10nm-300nm.

[0016] In another aspect of the present invention, the present invention provides a hardened film. In some embodiments of the present invention, the hardened film is prepared by the method described above. Thus, the hardened film has good anti-bending and wear-resistant properties and can be used in flexible display devices.

[0017] In another aspect of the present invention, the present invention provides a flexible display device. In some embodiments of the present invention, the flexible display device includes a display screen and the aforementioned hardened film, and the hardened film is located on the light-emitting surface of the display screen. Therefore, the flexible display device has all the characteristics and advantages of the aforementioned hardened film, which will not be repeated here. In general, the flexible display device has good anti-bending performance and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0019] Figure 1 A schematic diagram showing the structure of a hardening film according to an embodiment of the present invention is shown;

[0020] Figure 2 A schematic structural diagram of a hardening film according to another embodiment of the present invention is shown;

[0021] Figure 3 A schematic structural diagram of a hardening film according to another embodiment of the present invention is shown;

[0022] Figure 4 A schematic structural diagram of a hardening film according to another embodiment of the present invention is shown;

[0023] Figure 5 A schematic structural diagram of a hardening film according to another embodiment of the present invention is shown;

[0024] Figure 6A schematic structural diagram of a hardening film according to another embodiment of the present invention is shown;

[0025] Figure 7 A schematic structural diagram of a hardening film according to another embodiment of the present invention is shown;

[0026] Figure 8 A schematic structural diagram of a flexible display device according to an embodiment of the present invention is shown.

[0027] Description of reference numerals:

[0028] 100: hardened film; 200: display screen; 10: flexible substrate; 20: hardened wear-resistant composite layer; 21: hardened coating; 22: wear-resistant layer; 30: antifouling layer; 40: base coating. DETAILED DESCRIPTION

[0029] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0030] In one aspect of the present invention, the present invention provides a method for preparing a hardened film. In some embodiments of the present invention, the method for preparing a hardened film may include: providing a flexible substrate, and forming at least one hardened wear-resistant composite layer on at least one side of the flexible substrate. Figures 1 to 8 The hardened wear-resistant composite layer 20 may include a hardened coating layer 21 and a wear-resistant layer 22 , wherein the wear-resistant layer 22 is located on a surface of the hardened coating layer 21 away from the flexible substrate 10 .

[0031] In some embodiments of the present invention, forming a hardened wear-resistant composite layer 20 may include the following steps: a first raw material is hydrolyzed and condensed to form a hardened coating 21 on one side of the flexible substrate 10, the first raw material comprising a first compound represented by formula (1) or a mixture of the first compound and a second compound represented by formula (2); a silicon source compound is used as the second raw material, and a plasma enhanced chemical vapor deposition method is used to form a wear-resistant layer 22 on the surface of the hardened coating 21 away from the flexible substrate 10.

[0032] XY-SiR' n (OR) 3-n Formula (1), Si(OR”)4 formula (2).

[0033] In formula (1), n ​​can be 0, 1 or 2.

[0034] X can be selected from epoxy, epoxycyclohexane, acrylate or methacrylate; Y can be selected from C 1~6Alkylene, C 6~20 or a C having an ether bond, an acyl group, a urea group or a carbamate group in the chain or at the end. 1~6 Alkylene or C 6~20 Each R and each R' in formula (1) are independently selected from C 1~6 Alkyl, C 2~6 The alkenyl group, C 3~6 Alkynyl, C 6~20 Each R" in formula (2) is independently selected from C 1~6 Alkyl, C 2~6 The alkenyl group, C 3~6 Alkynyl, C 6~20 The aromatic group.

[0035] In some embodiments, the first compound may include at least one of the compounds shown in the following structural formulas:

[0036]

[0037]

[0038] In some embodiments, the second compound may include at least one of the compounds shown in the following structural formulas:

[0039]

[0040] The first compound or the mixture of the first compound and the second compound can form a hardened coating on the flexible substrate through a hydrolysis condensation reaction. The hardened coating includes a silicon-containing resin material, has certain flexibility and hardness, and the film layer has a high bonding strength with the flexible substrate and has certain wear resistance. The wear-resistant layer is formed by a silicon source compound through plasma enhanced chemical vapor deposition. SiO in the wear-resistant layer x It can form chemical bonds with the hardened coating, greatly improving the wear resistance of the coating, and it is not easy to be scratched by multiple frictions; the flexible substrate, hardened coating and wear-resistant layer gradually transition in chemical composition, and chemical bonds can be formed between the layers. Therefore, it has excellent resistance to cold and hot shocks and is not prone to cracking or falling off during cold and hot shocks.

[0041] In some embodiments of the present invention, the hardened coating can be obtained by hydrolysis and condensation of the first compound. The hardened coating has good flexibility and a certain hardness and good comprehensive performance.

[0042] In other embodiments of the present invention, the first raw material includes a mixture of a first compound and a second compound, and the mass ratio of the second compound to the first compound is ≤10:1, whereby the obtained hardened coating includes a silicon-containing organic-inorganic hybrid resin, has good anti-bending performance, and has good comprehensive performance. The inventors have found that when the content of the second compound is too high, the content of the inorganic silicon compound in the obtained hardened coating is high, which may cause the flexibility of the hardened coating to decrease, and the anti-bending performance is poor, which is not conducive to improving the flexibility of the hardened film.

[0043] In some embodiments of the present invention, the first raw material may further include at least one of silicon oxide, aluminum oxide, titanium oxide nanoparticles and colloids. Functional groups such as hydroxyl groups on the surface of the nanoparticles and colloids can participate in the hydrolysis process of the first and second compounds and form chemical bonds therewith, which can not only further improve the wear resistance of the coating, but also dissipate the internal stress generated when the coating is cured into a film, further improving the adhesion of the coating. The specific content of the nanoparticles or colloids is not particularly limited in the present invention, and those skilled in the art can add a certain amount of nanoparticles and / or colloids to the raw materials according to actual needs.

[0044] In some embodiments of the present invention, the first raw material may further include at least one of an initiator and a cross-linking agent. The initiator can promote the reaction, and the cross-linking agent can promote the cross-linking and curing of materials such as resins.

[0045] In some embodiments of the present invention, the initiator may include at least one of a free radical initiator and a cationic initiator, which can improve the curing efficiency and save energy and protect the environment. In some specific embodiments of the present invention, the free radical initiator may include a commonly used photoinitiator 184, and the cationic initiator may include an iodonium salt or a sulfonium salt photoinitiator. The amount of the initiator added is not particularly limited in the present invention, and those skilled in the art may add it according to actual needs.

[0046] In some embodiments of the present invention, the crosslinking agent may be a thermal crosslinking agent or a thermal crosslinking resin. The amount of the crosslinking agent added is not particularly limited in the present invention, and those skilled in the art may add the crosslinking agent according to actual needs.

[0047] In some embodiments of the present invention, the first raw material may further include a solvent, for example, the solvent may be ethanol, tetrahydrofuran, or the like.

[0048] In some embodiments of the present invention, the first raw material may further include a catalyst, such as an acidic catalyst (hydrochloric acid, etc.) or a basic catalyst (potassium carbonate, etc.).

[0049] The amount of solvent or catalyst added is not particularly limited in the present invention, and those skilled in the art can add it according to actual needs.

[0050] In some embodiments of the present invention, the wear-resistant layer 22 can be prepared under the condition of the presence of a first gas, the first gas can include oxygen, and the flow ratio of the silicon source compound to the first gas can be 1:20-1:6. For example, the flow ratio of the silicon source compound to the first gas can be 1:20, 1:15, 1:12, 1:10, 1:6, etc. As a result, the wear-resistant layer has excellent wear resistance, good flexibility and good transparency. The inventors found that if the flow ratio of the silicon source compound to the first gas is less than 1:20, the wear-resistant layer deposition efficiency may be too low, and the flexibility of the wear-resistant layer may also decrease; if the flow ratio of the silicon source compound to the first gas is greater than 1:6, the transparency and wear resistance of the prepared wear-resistant layer may be poor.

[0051] In some embodiments of the present invention, the silicon source compound may include hexamethyldisiloxane. The wear-resistant layer formed by plasma enhanced chemical vapor deposition of the above material in an oxygen atmosphere has good wear resistance and flexibility.

[0052] In some specific embodiments of the present invention, the first gas may be oxygen.

[0053] In other specific embodiments of the present invention, the first gas may include oxygen and an inert gas, and the flow ratio of the inert gas to the first gas is ≤1:5. In some embodiments of the present invention, the first gas may be a mixture of oxygen and an inert gas (argon, helium, etc.), and the content of the inert gas is ≤20%, thereby improving the bonding strength between the wear-resistant layer and the hardened coating, thereby facilitating further improving the overall performance of the hardened film.

[0054] In some embodiments of the present invention, when forming the wear-resistant layer, the plasma discharge power density may be 0.5 kW / m 2 -10kw / m 2 For example, the plasma discharge power density can be 0.5 kW / m 2 , 0.8kW / m 2 , 1kW / m 2 , 3kW / m 2 , 5kW / m 2 、10kw / m 2 Etc. This is conducive to forming a wear-resistant layer with good flexibility and wear resistance. The inventors found that the power density is less than 0.5kW / m 2 When the wear-resistant layer is deposited at a low efficiency and has poor bonding strength with the deposition interface; power density>10kW / m 2 When the deposition interface is damaged, the performance will be affected.

[0055] In some embodiments of the present invention, when forming the wear-resistant layer, the air pressure in the reaction zone may be 0.1-10Pa, for example, the air pressure in the reaction zone may be 0.1Pa, 0.5Pa, 1Pa, 3Pa, 5Pa, 10Pa, etc., which is beneficial to improve the deposition efficiency of the wear-resistant layer and improve the compactness and wear resistance of the wear-resistant layer. The inventors found that if the air pressure in the reaction zone is less than 0.1Pa, it may result in a low deposition efficiency; if the air pressure in the reaction zone is greater than 10Pa, it may result in poor compactness of the wear-resistant layer and reduced wear resistance.

[0056] In some embodiments of the present invention, when forming the wear-resistant layer, the magnetic field strength of the flexible substrate can be 5GS-100GS, for example, the magnetic field strength of the flexible substrate can be 5GS, 10GS, 30GS, 50GS, 80GS, 100GS, etc. The magnetic field strength within the above range is conducive to improving the bonding strength between the wear-resistant layer and the hardened coating. If the magnetic field strength is less than 5GS, the bonding force between the wear-resistant layer and the deposition interface may be small; if the magnetic field strength is greater than 100GS, the cost of the equipment may be significantly increased, which is not conducive to large-scale production.

[0057] In some embodiments of the present invention, the material of the flexible substrate may include at least one of transparent polyimide (CPI), cycloolefin polymer, polyethylene naphthalate (PEN) and polyethylene terephthalate (PET).

[0058] In some embodiments of the present invention, the thickness of the flexible substrate 10 may be 5 μm-188 μm, for example, the thickness of the flexible substrate 10 may be 5 μm, 10 μm, 50 μm, 100 μm, 150 μm, 188 μm, etc., so that the flexible substrate can provide good support and has good anti-bending performance. When the thickness of the flexible substrate is less than 12 μm, there may be a problem of low yield in the subsequent preparation of the hardened wear-resistant composite layer; when the thickness of the flexible substrate is greater than 188 μm, the flexible substrate may have a problem of poor anti-bending performance, which is not conducive to improving the flexibility of the hardened film.

[0059] In some embodiments of the present invention, reference Figure 1 and Figure 2 , a hardened wear-resistant composite layer 20 may be formed only on one side of the flexible substrate 10 .

[0060] In some other embodiments of the present invention, a plurality of hardened wear-resistant composite layers 20 may be formed on at least one side of the flexible substrate 10, and the plurality of hardened wear-resistant composite layers 20 may be stacked. Increasing the number of hardened wear-resistant composite layers may further increase the hardness of the hardened film and improve the protective effect. Figure 3 and Figure 4, two hardened wear-resistant composite layers 20 may be formed on one side of the flexible substrate 10, and the two hardened wear-resistant composite layers 20 are stacked. When multiple hardened wear-resistant composite layers are formed on both sides of the flexible substrate, the number of hardened wear-resistant composite layers on both sides of the flexible substrate may be the same or different. For example, the number of hardened wear-resistant composite layers on both sides of the flexible substrate may be 2, 3, 4, 5 or more, respectively, independently.

[0061] In some other embodiments of the present invention, reference Figure 5 and Figure 6 , a hardened wear-resistant composite layer 20 can be formed on both sides of the flexible substrate 10 respectively.

[0062] In some embodiments of the present invention, the thickness of the hardened coating 21 may be 1 μm-30 μm, for example, the thickness of the hardened coating 21 may be 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, etc., which is conducive to further improving the wear resistance and bending resistance of the hardened film. If the thickness of the hardened coating is less than 1 μm, the wear resistance of the hardened film may be poor; if the thickness of the hardened coating is greater than 30 μm, the hardened film may be easily cracked during the bending process.

[0063] In some embodiments of the present invention, the thickness of the wear-resistant layer 22 may be 50nm-500nm, for example, the thickness of the wear-resistant layer 22 may be 50nm, 80nm, 100nm, 300nm, 500nm, etc. If the thickness of the wear-resistant layer is less than 50nm, the wear resistance of the hardened film may be poor; if the thickness of the wear-resistant layer is greater than 500nm, the wear-resistant layer may have a risk of cracking.

[0064] In some embodiments of the present invention, the method for preparing a hardened film may further include: a third raw material is hydrolyzed and condensed to form an antifouling layer on the side of the outermost hardened wear-resistant composite layer away from the flexible substrate, and the third raw material forming the antifouling layer may include a first siloxane, and the first siloxane contains fluorine. When the hardened film is used for a flexible display screen, in addition to wear resistance and bending resistance, the antifouling performance of the hardened film is also required to be high. The antifouling layer is formed on the side of the hardened wear-resistant composite layer away from the flexible substrate by the above method, which has good waterproof and oil-proof effects, and the antifouling effect of the hardened film can be prevented from being significantly attenuated during the life cycle of the device (such as a flexible display device).

[0065] In some embodiments of the present invention, the first siloxane may include at least one of heptadecafluorodecyltrimethoxysilane, perfluorooctylethyltriethoxysilane, perfluorohexylethyltriethoxysilane, trifluoropropyltriethoxysilane, trifluoropropyltrimethoxysilane, and perfluorohexylethyltriethoxysilane. The fluorine-containing silicone material (fluorosilicone resin) obtained by hydrolysis and condensation of the above fluorine-containing silicone has a good waterproof and oil-proof effect, which is beneficial to improve the antifouling performance of the hardened film.

[0066] In some embodiments of the present invention, the third raw material may further include a second siloxane, the second siloxane does not contain fluorine, and the second siloxane may include at least one of a KH550 silane coupling agent and an A187 silane coupling agent. Adding the second siloxane is beneficial to improving the solubility of the fluorosilicone resin, which is beneficial to the subsequent coating of the antifouling liquid.

[0067] In some embodiments of the present invention, the third raw material includes a first siloxane and a second siloxane, and the mass ratio of the first siloxane to the second siloxane is ≥1:2, which is beneficial to improving the waterproof and oil-proof effect of the antifouling layer.

[0068] In some embodiments of the present invention, after selecting the first siloxane or the first siloxane and the second siloxane, water with a molar amount of 0.1-0.8 times the molar amount of water to the siloxane group can be introduced in the presence of an acidic catalyst (such as hydrochloric acid) or a basic catalyst to perform hydrolysis and condensation reaction to obtain a fluorosilicone resin. The above-mentioned fluorosilicone resin is dissolved or dispersed with a suitable solvent, such as an alcohol solvent, and then formed into a film on the wear-resistant layer by a common wet coating method. The fluorosilicone resin can be dissolved or dispersed with solvents such as methanol, ethanol, propanol, isopropanol, etc. The specific amount of the solvent is not particularly limited in the present invention, and those skilled in the art can set or adjust it according to actual needs.

[0069] In some embodiments of the present invention, reference Figure 2 , Figure 4 , Figure 6 and Figure 7 The thickness of the antifouling layer 30 can be 10nm-300nm, for example, the thickness of the antifouling layer 30 can be 10nm, 30nm, 50nm, 100nm, 200nm, 300nm, etc. Therefore, the antifouling layer has a good waterproof and oil-proof effect, and the preparation cost is low. If the thickness of the antifouling layer is less than 10nm, it may lead to poor waterproof and oleophobic effect; if the thickness of the antifouling layer is greater than 300nm, on the one hand, it will significantly increase the preparation cost of the hardened film, on the other hand, it is difficult for an overly thick antifouling layer to further improve the waterproof and oleophobic effect.

[0070] In some embodiments of the present invention, before forming the antifouling layer, the wear-resistant layer may be subjected to a plasma treatment, thereby improving the bonding strength between the wear-resistant layer and the antifouling layer.

[0071] In some embodiments of the present invention, in order to improve the bonding strength between the flexible substrate and the hardened wear-resistant composite layer, reference Figure 7 , a primer layer 40 may be formed on the surface of the flexible substrate 10. In some embodiments of the present invention, the material of the primer layer 40 may include polymers such as acrylic, polyurethane, epoxy, or a blend of the above resins, thereby improving the bonding effect between the flexible substrate and the hardened wear-resistant composite layer, improving the bonding strength between the flexible substrate and the hardened wear-resistant composite layer, and thus improving the overall performance of the hardened film.

[0072] In general, the hardened coating in the hardened film has good adhesion to the flexible substrate and has certain wear resistance. The wear-resistant layer is introduced by plasma enhanced chemical vapor deposition. The SiO x It can form chemical bonds with the hardened coating, and the wear resistance of the coating is greatly improved, and it can withstand more than 2000 times of friction with 750g of 0000# steel wool; the flexible substrate gradually transitions to the hardened coating and then to the wear-resistant layer in chemical composition, and at the same time, chemical bonds can be formed between the layers, so the performance of resistance to cold and hot shocks is excellent. The present invention can achieve the required wear resistance under the condition of thinner functional layer thickness through the coordinated use of tough hardened coating and wear-resistant layer. The thinning of the functional layer and the improvement of the close contact between the layers can make the hardened film folded more than 100,000 times with a radius of ≤2mm. Furthermore, the hardened film of the present invention can introduce an anti-fouling layer with excellent wear resistance, because the outer side of the hardened wear-resistant composite layer is SiO obtained by plasma enhanced chemical vapor deposition method. x The surface of the wear-resistant layer naturally has or is easily accessible to abundant Si-OH bonds. The fluorosilicone antifouling layer is deposited on the surface of the wear-resistant layer to form Si-O-Si bonds. Therefore, the wear-resistant performance of the antifouling layer is very excellent.

[0073] In another aspect of the present invention, the present invention provides a hardening film. The structure of the hardening film 100 can refer to Figures 1 to 8 The hardened film is prepared by the method described above. Therefore, the hardened film has good anti-bending performance and wear resistance. When an anti-fouling layer is provided, the hardened film also has good waterproof and oil-proof effects.

[0074] In another aspect of the present invention, the present invention provides a flexible display device. In some embodiments of the present invention, reference Figure 8 The flexible display device may include a display screen 200 and the aforementioned hardening film 100, and the hardening film 100 is located on the light emitting surface side of the display screen 200. Thus, the hardening film can play a role in protecting the display screen.

[0075] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.

[0076] Preparation of hardening liquid 1

[0077] 40 g of tetraethoxysilane and 4 g of epoxysiloxane A187 were mixed, and then 20 g of ethanol (solvent) and 30 g of dilute hydrochloric acid solution with a pH of 1 (catalyst) were added, and stirred at 80°C for 4 h. After standing at room temperature for 24 h, 1 g of aluminum sec-butoxide and 1 g of ethyl acetoacetate were added (aluminum sec-butoxide and ethyl acetoacetate can promote the ring-opening crosslinking of epoxy functional groups and promote the partial crosslinking of silanols or siloxanes) to obtain a hardening solution 1.

[0078] Preparation of hardening liquid 2

[0079] 40g of epoxysilane A187 was dissolved in 80g of tetrahydrofuran (solvent), and then 0.5g of potassium carbonate (alkaline catalyst) and 9g of water were added, and the mixture was stirred at room temperature for 10 days and the solid was filtered out. Low boiling points were removed by vacuum distillation, and the remaining resin was dissolved in butanone, and a 5wt% cationic initiator (bis(4-tert-butylphenyl)iodonium hexafluorophosphate PI-256) was added to the solution to obtain hardening solution 2.

[0080] Preparation of hardening liquid 3

[0081] 40g of methacrylate silane A174 was dissolved in 80g of tetrahydrofuran, and then 0.5g of potassium carbonate (alkaline catalyst) and 9g of water were added. The mixture was stirred at room temperature for 10 days and the solid was filtered off. Low boiling substances were removed by vacuum distillation, and the remaining resin was dissolved in butanone and a free radical initiator (photoinitiator 184) was added at a ratio of 5wt% to obtain hardening solution 3.

[0082] Antifouling liquid preparation

[0083] 10 g of perfluorooctylethyltriethoxysilane and 10 g of aminosiloxane KH550 are mixed, 10 g of water is added, 1 g of a dilute hydrochloric acid solution with a pH of 1 is dropped, and the mixture is stirred at room temperature for 24 h. An appropriate alcohol solvent (such as isopropanol) is added to dilute the mixture and the mixture is set aside.

[0084] Example 1

[0085] The hardening solution 1 was coated on the PET with a thickness of 50 μm and cured at 120°C for 3 min to obtain a hardened coating with a thickness of 3 μm. The above sample was transferred to the PECVD coating equipment, and the silicon source compound hexamethyldisiloxane and oxygen were introduced under vacuum conditions with a flow ratio of 1:20. The gas pressure was controlled at 0.8 Pa, and the power density in the discharge area was 0.8 kW / m 2 , the magnetic field strength above the flexible substrate is 10 GS, and a wear-resistant layer is obtained, and the thickness of the wear-resistant layer is 50 nm. The prepared product is recorded as hardened film 1.

[0086] Example 2

[0087] Apply hardening solution 2 on PET with a thickness of 50 μm, cure at 85°C for 3 minutes, and then use 800 mJ / cm 2 UV irradiation was performed to obtain a hardened coating having a thickness of 6 μm. The coating conditions of the wear-resistant layer in Example 2 were the same as those in Example 1. The product obtained was recorded as hardened film 2.

[0088] Example 3

[0089] The curing liquid 3 was applied on PET with a thickness of 50 μm, and after curing at 85°C for 3 min, the film was heated with 800 mJ / cm 2 UV irradiation was performed to obtain a hardened coating having a thickness of 6 μm. The coating conditions of the wear-resistant layer in Example 2 were the same as those in Example 1. The prepared product was recorded as hardened film 3.

[0090] Example 4

[0091] The hardening solution 1 was coated on the PET with a thickness of 50 μm and cured at 120°C for 3 min to obtain a hardened coating with a thickness of 3 μm. The above sample was transferred to the PECVD coating equipment, and the silicon source compound hexamethyldisiloxane and oxygen were introduced under vacuum conditions with a flow ratio of 1:6. The gas pressure was controlled at 0.8 Pa, and the power density of the discharge area was 3 kW / m 2 , the magnetic field strength above the flexible substrate is 10 GS, and a wear-resistant layer is obtained, and the thickness of the wear-resistant layer is 50 nm. The prepared product is recorded as hardened film 4.

[0092] Example 5

[0093] The hardening solution 1 was coated on the PET with a thickness of 50 μm and cured at 120°C for 3 min to obtain a hardened coating with a thickness of 3 μm. The above sample was transferred to the PECVD coating equipment, and the silicon source compound hexamethyldisiloxane and oxygen were introduced under vacuum conditions with a flow ratio of 1:6. The gas pressure was controlled at 0.8 Pa, and the power density of the discharge area was 3 kW / m 2, the magnetic field strength above the flexible substrate is 10 GS, and a wear-resistant layer is obtained, and the thickness of the wear-resistant layer is 500 nm. The prepared product is recorded as hardened film 5.

[0094] Example 6

[0095] After preparing the hardened coating and the wear-resistant layer according to the steps and parameters in Example 1, pure oxygen was introduced to treat the wear-resistant layer with oxygen plasma, and then an antifouling liquid was coated on the wear-resistant layer to obtain an antifouling layer with a thickness of 100 nm. The prepared product was recorded as hardened film 6.

[0096] Example 7

[0097] With hardened film 1 as the substrate, a hardened coating and a wear-resistant layer were sequentially prepared on the wear-resistant layer according to the conditions in Example 1 to obtain hardened film 7. Compared with the product in Example 1, the product in Example 7 formed two hardened wear-resistant composite layers on one side of the flexible substrate.

[0098] Example 8

[0099] With the hardened film 1 as the substrate, a hardened coating layer and a wear-resistant layer are prepared on the side away from the hardened coating layer and the wear-resistant layer according to the process in Example 1 to obtain a hardened film 8. Compared with the product in Example 1, Example 8 forms a hardened wear-resistant composite layer on both sides of the flexible substrate.

[0100] Comparative Example 1

[0101] The hardening solution 1 was coated on a PET film with a thickness of 50 μm and cured at 120° C. for 3 min to obtain a hardened coating with a thickness of 3 μm. The product prepared in Comparative Example 1 was recorded as Hardened Film 9.

[0102] Comparative Example 2

[0103] The same wear-resistant layer was directly deposited on PET with a thickness of 50 μm according to the coating process in Example 1 to obtain a hardened film 10 .

[0104] Comparative Example 3

[0105] The same wear-resistant layer was directly deposited on PET with a thickness of 50 μm according to the coating process in Example 5 to obtain a hardened film 11 .

[0106] Comparative Example 4

[0107] A commercially available acrylic hardened film with a thickness of 50 μm (CH1081 hardened film produced by Hefei Lucky) was used as the substrate, and the same wear-resistant layer was prepared according to the coating process in Example 1 to obtain a hardened film 12 .

[0108] Comparative Example 5

[0109] According to the process of Example 6, a PET substrate with a thickness of 50 μm was directly subjected to plasma treatment and coated with antifouling liquid to obtain a hardened film 13. Compared with the product of Example 6, the product in Comparative Example 5 has no hardened coating layer and wear-resistant layer.

[0110] Comparative Example 6

[0111] After forming a hardened coating on a PET substrate with a thickness of 50 μm according to the process of Example 6, plasma treatment was directly performed and antifouling liquid was applied to obtain a hardened film 14. Compared with the product of Example 6, the product in Comparative Example 6 has no wear-resistant layer.

[0112] The hardened films prepared in the embodiments and comparative examples were subjected to performance tests, including a wear resistance test, a bending resistance test, a thermal shock resistance test, and an antifouling test.

[0113] Wear resistance test: 0000# steel wool, load 750g, contact area 1cm 2 , rub the coating surface, stop and observe the scratches on the coating surface after every 20 frictions, stop the test when there are more than 5 scratches, and record the number of frictions; if there is no scratch after 2000 frictions, its wear resistance is considered to be >2000 times.

[0114] Bending resistance test: With a bending radius of 1mm, the hardened film is folded outward and inward 100,000 times, and then the coating cracking is observed. If there is no visible crack, it is recorded as OK, otherwise it is recorded as No.

[0115] Thermal shock resistance test: from -40℃ for 30min to 95℃ for 30min, temperature switching time ≤1min. Observe the coating status after 1000 cycles.

[0116] The test results of wear resistance, bending resistance, and thermal shock resistance of each embodiment and comparative example are recorded in Table 1.

[0117] Table 1

[0118] Sample No. Wear results (wear times) Bending resistance results Thermal shock resistance results Example 1 (hardened film 1) >2000 OK normal Example 2 (hardened film 2) >2000 OK normal Example 3 (hardened film 3) >2000 OK normal Example 4 (hardened film 4) >2000 OK normal Example 5 (hardened film 5) >2000 OK normal Example 7 (hardened film 7) >2000 OK normal Example 8 (hardened film 8) >2000 OK normal Comparative Example 1 (hardened film 9) 200 OK normal Comparative Example 2 (hardened film 10) 20 OK Coating peeling off Comparative Example 3 (hardened film 11) 40 No Coating peeling Comparative Example 4 (hardened film 12) 200 No Coating peeling off

[0119] Antifouling effect evaluation: First, record the water contact angle of the antifouling layer of the hardened film before the test, then perform the above-mentioned cold and hot shock resistance cycle 1000 times and the wear resistance test 2000 times on the hardened film, and record the water contact angle of the antifouling layer after the test. The test results are recorded in Table 2.

[0120] Table 2

[0121]

[0122] The test results show that in Comparative Example 5, since no hardened wear-resistant composite layer was introduced, the adhesion of the antifouling layer decreased significantly after the thermal shock. After the wear test, part of the antifouling layer fell off, and the substrate was exposed, resulting in a significant decrease in the water contact angle. After the thermal shock and wear test, many scratches appeared on the surface of the sample of Comparative Example 6, part of the antifouling layer fell off, the hardened coating was exposed, and the water contact angle also decreased significantly. However, after the test of Example 6, there were no scratches on the surface, and the antifouling layer was intact as a whole, and the water contact angle was basically unchanged.

[0123] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", "some embodiments", "other embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0124] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a hardened film, characterized in that: include: providing a flexible substrate; forming at least one hardened wear-resistant composite layer on at least one side of the flexible substrate, wherein the hardened wear-resistant composite layer comprises a hardened coating layer and a wear-resistant layer, and the wear-resistant layer is located on a surface of the hardened coating layer away from the flexible substrate; Forming the hardened wear-resistant composite layer comprises the following steps: The first raw material is hydrolyzed and condensed to form the hardened coating on one side of the flexible substrate, wherein the first raw material comprises a first compound represented by formula (1) or a mixture of the first compound and a second compound represented by formula (2), X-Y-SiR’ n (OR) 3-n Formula (1), Si(OR”)4 Formula (2), n=0, 1 or 2; X is selected from epoxy, epoxycyclohexane, acrylate or methacrylate; Y is selected from C 1~6 Alkylene, C 6~20 or a C having an ether bond, an acyl group, a urea group or a carbamate group in the chain or at the end. 1~6 Alkylene or C 6~20 Each R and each R' in formula (1) are independently selected from C 1~6 Alkyl, C 2~6 The alkenyl group, C 3~6 Alkynyl, C 6~20 Each R" in formula (2) is independently selected from C 1~6 Alkyl, C 2~6 The alkenyl group, C 3~6 Alkynyl, C 6~20 The aromatic group; When the first raw material includes a mixture of a first compound and a second compound, the mass ratio of the second compound to the first compound is ≤10:1; The silicon source compound is used as the second raw material, and the wear-resistant layer is formed on the surface of the hardened coating away from the flexible substrate by a plasma enhanced chemical vapor deposition method.

2. The method according to claim 1, characterized in that forming a hardened wear-resistant composite layer on both sides of the flexible substrate; Alternatively, a plurality of the hardened wear-resistant composite layers are formed on at least one side of the flexible substrate, and the plurality of the hardened wear-resistant composite layers are stacked.

3. The method according to claim 1, characterized in that The first raw material further includes at least one of silicon oxide, aluminum oxide, titanium oxide nanoparticles and colloids; And / or, the first raw material further includes at least one of an initiator and a cross-linking agent.

4. The method according to claim 1, characterized in that: At least one of the following conditions is met: The wear-resistant layer is prepared in the presence of a first gas, the first gas includes oxygen, and the flow ratio of the silicon source compound to the first gas is 1:20-1:6; The silicon source compound includes hexamethyldisiloxane; When forming the wear-resistant layer, the plasma discharge power density is 0.5 kW / m 2 -10kw / m 2 ; The gas pressure in the reaction zone where the wear-resistant layer is formed is 0.1-10 Pa; When the wear-resistant layer is formed, the magnetic field intensity at the flexible substrate is 5GS-100GS.

5. The method according to claim 4, characterized in that The first gas is oxygen; Alternatively, the first gas includes oxygen and an inert gas, and a flow ratio of the inert gas to the first gas is ≤1:

5.

6. The method according to claim 1, characterized in that At least one of the following conditions is met: The material of the flexible substrate includes at least one of transparent polyimide, cycloolefin polymer, polyethylene naphthalate and polyethylene terephthalate; The thickness of the flexible substrate is 5 μm-188 μm; The thickness of the hardened coating is 1 μm-30 μm; The thickness of the wear-resistant layer is 50nm-500nm.

7. The method according to any one of claims 1 to 6, characterized in that Also includes: The third raw material is hydrolyzed and condensed to form an antifouling layer on the side of the outermost hardened wear-resistant composite layer away from the flexible substrate. The third raw material forming the antifouling layer includes a first siloxane containing fluorine.

8. The method according to claim 7, characterized in that At least one of the following conditions is met: The first siloxane comprises at least one of heptadecafluorodecyltrimethoxysilane, perfluorooctylethyltriethoxysilane, perfluorohexylethyltriethoxysilane, trifluoropropyltriethoxysilane, trifluoropropyltrimethoxysilane, and perfluorohexylethyltriethoxysilane; The third raw material further includes a second siloxane, the second siloxane does not contain fluorine, and the second siloxane includes at least one of a KH550 silane coupling agent and an A187 silane coupling agent; The third raw material further includes a second siloxane, the second siloxane does not contain fluorine, and the mass ratio of the first siloxane to the second siloxane is ≥1:2; The thickness of the antifouling layer is 10nm-300nm.

9. A hardened film, characterized in that: It is prepared by the method described in any one of claims 1 to 8.

10. A flexible display device, characterized in that: It comprises a display screen and the hardened film according to claim 9, wherein the hardened film is located on the light emitting surface side of the display screen.