MXene-based nano intumescent flame retardant and preparation method thereof

By grafting polymerized phosphorus-nitrogen expansion flame retardant on the surface of MXene nanomaterials, the problems of poor dispersion and poor smoke suppression in polymer materials are solved, and high-efficiency flame retardant, smoke suppression and conductivity are achieved , improves the fire safety and mechanical properties of polymer materials.

CN118930974APending Publication Date: 2024-11-12BEIJING INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410999934.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing flame retardants have poor dispersion and easy stacking in polymer materials, and the traditional flame retardants have limited effects on smoke suppression and toxic gases, affecting the fire safety and mechanical properties of polymer materials.

Method used

By grafting polymerized phosphorus-nitrogen expansion flame retardant on the surface of MXene nanomaterials, the MXene group integrating acid source, gas source and carbon source is designed using the reaction between hydroxyl and hydroxyl groups, and the active functional groups of polymer segments. Nanomodified expansion flame retardant solves the problems of poor dispersion and stacking, and realizes multifunctional properties such as flame retardant, smoke suppression, and conductivity.

Benefits of technology

Achieve excellent flame retardant effect at a lower addition amount, ensure the excellent mechanical properties of polymer materials, significantly reduce heat transfer and smoke generation, improve electromagnetic shielding performance, and expand the application range of polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930974A_ABST
    Figure CN118930974A_ABST
Patent Text Reader

Abstract

The invention relates to an MXene-based nano intumescent flame retardant and a preparation method thereof, and belongs to the technical field of flame retardants. The flame retardant is formed by compounding a polymeric spirocyclic phosphorus-nitrogen intumescent flame retardant and an MXene nano material, and the polymeric spirocyclic phosphorus-nitrogen intumescent flame retardant is grafted or physically bonded on the surface of a single-layer MXene nano material; the nano-based intumescent flame retardant which has a plurality of properties such as flame retardance, excellent mechanical properties, electromagnetic shielding, electric conduction and the like is prepared by utilizing a polymeric phosphorus-nitrogen intumescent flame retardant and a nano MXene material surface grafting manner; the polymer composite material has a more excellent catalytic char forming effect, a more efficient smoke suppression effect, richer performance advantages and a wider application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a MXene-based nano-expansion flame retardant and a preparation method thereof, and belongs to the technical field of flame retardants. Background Art

[0002] With the continuous development of polymer materials, their excellent mechanical properties and applicability in various industries have become an indispensable and important part of people's lives and production. However, due to the elemental composition and carbon chain-based chemical structure of most polymers, most polymers usually exhibit high flammability and smoke emissions, which may lead to serious fire hazards and pose great safety hazards to human production and life safety. Epoxy resin (EP), as a typical polymer widely used in business, will cause violent combustion when a fire occurs, accompanied by a large amount of dense smoke and harmful gases (such as HCN and CO), which will seriously damage life safety and cause environmental pollution. It has been confirmed that halogen-containing or phosphorus-containing flame retardants can provide effective flame retardant properties for epoxy resins, but the addition amount of such flame retardants is usually above 10%, which often seriously affects the mechanical properties of epoxy composites. In addition, these flame retardants have limited inhibition on smoke particles and toxic gases. Therefore, it is still a difficult challenge to develop environmentally friendly and efficient flame retardants to improve the fire safety of EP composites and retain mechanical properties.

[0003] Nowadays, traditional flame retardants no longer meet the needs of practical use of polymer materials. The preparation of multifunctional flame retardants is the key to expanding the application of polymer materials. In order to meet the requirements of green environmental protection, the use of flame retardants is more inclined to phosphorus nitrogen expansion flame retardant system. Its excellent carbonization effect and smoke suppression ability have greatly expanded the flame retardant family and provided beneficial help for improving the flame retardant properties of polymer materials. The emergence of nanofillers, thanks to its rich functional groups (-OH, =O), can prepare more multifunctional flame retardants with flame retardant effects through a variety of bonding methods, giving polymer materials many properties such as conductivity, wave absorption, thermal conductivity, and electromagnetic shielding, which meets the development needs of multifunctional polymer materials. In addition, extensive experimental studies have shown that nano flame retardants can achieve effective catalytic carbonization effects at relatively low addition amounts, and have beneficial heat insulation and oxygen isolation effects during the combustion process, giving nano-composite materials good fire safety. However, there are few reports on nano-modified flame retardants, and the flame retardant efficiency of nano flame retardants and the problems of poor dispersibility and easy agglomeration in the matrix have not been further optimized. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a MXene-based nano-expandable flame retardant and a preparation method thereof. A polymerized phosphorus-nitrogen expandable flame retardant is grafted onto the surface of the nano-material MXene to obtain a MXene-based nano-modified expandable flame retardant integrating an expansion system (acid source, gas source, carbon source). Starting from the mutual reaction between functional groups, the present invention utilizes the reaction between hydroxyl groups and hydroxyl groups, and between hydroxyl groups and active functional groups of polymer segments, and disperses the new polymerized flame retardant into the gap of the MXene material by means of functional group substitution, rubbing, hydrogen bond association, etc.; utilizing the excellent characteristics of good compatibility between the polymerized flame retardant and the matrix, the problems of poor dispersibility and easy stacking of existing nano-materials are solved, and a new type of modified nano-material expandable flame retardant is designed and prepared to open the MXene interlayer into a single layer and realize modification. The addition of such flame retardants gives polymer materials many new properties such as flame retardancy, smoke suppression, and conductivity, achieving excellent flame retardant effects at a relatively low addition amount, ensuring the excellent mechanical properties of polymer materials and making them have both electromagnetic shielding and conductive effects, greatly expanding the application range of polymer materials.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows.

[0006] A MXene-based nano-intumescent flame retardant is composited with a polymeric spirophosphorus nitrogen intumescent flame retardant (DHPPC) and a MXene nano-material, wherein the polymeric spirophosphorus nitrogen intumescent flame retardant is grafted or physically bonded on the surface of a single-layer MXene nano-material;

[0007] Wherein, the structural formula of the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant is as follows:

[0008]

[0009] The repeating unit is C9O8N2H 10 P2, the degree of polymerization n is an integer from 8 to 12;

[0010] The molecular formula of MXene nanomaterials is Ti3C2T x , wherein T is a hydroxyl group or a carbonyl group.

[0011] Preferably, the molecular weight of the polymeric spirophosphorus nitrogen intumescent flame retardant is 3000-4000.

[0012] Preferably, the mass ratio of the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant to the MXene nanomaterial is 1:0.5-2.

[0013] A method for preparing the MXene-based nano-expandable flame retardant of the present invention, the method steps comprising:

[0014] Step 1: In an anhydrous and oxygen-free closed system, pentaerythritol is added to solvent A, stirred until the system is uniformly mixed, the temperature is raised to temperature 1, phosphorus oxychloride is added, nitrogen is introduced and the reaction is kept warm for 2 to 4 hours, and then the temperature is raised to temperature 2 and stirred for 8 to 16 hours, washed and dried to obtain an intermediate spirocyclic phosphate dichloride; wherein the molar ratio of pentaerythritol to phosphorus oxychloride is 1:2 to 7; temperature 1 is 40 to 70°C, and temperature 2 is 80 to 120°C; in an anhydrous and oxygen-free environment, 4,6-dihydroxypyrimidine is added to solvent B and stirred until The solution is clear and transparent, the intermediate spirocyclic phosphate dichloride and the acid binding agent are added, and the reaction is carried out at a temperature of 3 for 1 to 2 hours, and then the temperature is raised to a temperature of 4 and stirred and refluxed for 6 to 16 hours. After the reaction is completed, the solution is washed and dried to obtain a crude flame retardant, which is a yellow-brown powdery solid; wherein the molar ratio of 4,6-dihydroxypyrimidine to spirocyclic phosphate dichloride is 1:1 to 1.5, the temperature 3 is 30 to 55° C., and the temperature 4 is 60 to 100° C. After the crude flame retardant is ground, it is refluxed for purification, and dried to obtain a polymeric spirocyclic phosphorus nitrogen expansion flame retardant;

[0015] Step 2: Prepare an accordion-shaped MXene nanomaterial by adding the MXene nanomaterial into deionized water and ultrasonicating it at 5-10°C for 1-2 hours to obtain a thin layer of MXene nanomaterial;

[0016] Step 3: Add the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant and the thin layer MXene nanomaterial into solvent E, ultrasonically disperse for 0.5 to 2 hours, and then heat to 70 to 90° C. under nitrogen protection for reaction for 4 to 10 hours. After the reaction is completed, ultrasonicate at 5 to 10° C. for 1 to 2 hours, centrifuge, wash, and dry to obtain a MXene-based nano intumescent flame retardant.

[0017] Preferably, in step 1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:3-5.

[0018] Preferably, in step 1, the stirring rate is 220-300 rpm.

[0019] Preferably, in step 1, the flow rate of nitrogen is 5 to 20 mL / min.

[0020] Preferably, in step 1, temperature 1 is 55-65° C. Under this temperature condition, the reaction is more gentle and the yield is higher.

[0021] Preferably, in step 1, temperature 2 is 90-110°C.

[0022] Preferably, in step 1, the solvent A is one or more of anhydrous acetonitrile, acetone, dichloromethane and dioxane.

[0023] Preferably, in step 1, one or more of acetone, chloroform and dichloromethane are used for washing.

[0024] Preferably, in step 1, the solvent B is one or more of acetone, tetrahydrofuran, xylene, anhydrous acetonitrile and N,N-dimethylformamide.

[0025] Preferably, in step 1, the acid binding agent is one or more of triethylamine, cerium chloride, anhydrous potassium carbonate and pyridine.

[0026] Preferably, in step 1, the molar ratio of the 4,6-dihydroxypyrimidine to the acid binding agent is 1:1.5-2.2.

[0027] Preferably, in step 1, temperature 4 is 70-85°C.

[0028] Preferably, in step 1, one or more of deionized water, ether, anhydrous methanol, anhydrous ethanol, dichloromethane and acetonitrile is used for washing.

[0029] Preferably, in step 1, during the reflux purification, the solvent is one or more of acetone, dichloromethane, anhydrous ethanol and tetrahydrofuran.

[0030] Preferably, in step 1, during reflux purification, the temperature is 60 to 90° C., and the cooling reflux is performed for 3 to 12 hours.

[0031] Preferably, in step 1, during drying, vacuum drying is performed at 80-100° C. for 12-24 hours.

[0032] Preferably, in step 2, when preparing the accordion-shaped MXene nanomaterial, LiF and hydrochloric acid solution are mixed and stirred for more than 15 minutes, then the temperature is raised to 40-50°C, TiC2Al3 powder is added in batches, and then etched for 24-48 hours, centrifuged, washed to neutrality, and dried to obtain the accordion-shaped MXene nanomaterial. More preferably, the concentration of the hydrochloric acid solution is 8-12 mol / L, the dosage ratio of LiF to the hydrochloric acid solution is 1-1.5 g: 20-40 mL, and the mass ratio of TiC2Al3 powder to LiF is 1: 1.3-1.5.

[0033] Preferably, in step three, the mass ratio of the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant to the MXene nanomaterial is 1:0.5-2.

[0034] Preferably, in step three, the solvent E is one or more of methanol, ethanol, deionized water, acetone, N,N-dimethylformamide, acetonitrile and tetrahydrofuran.

[0035] Preferably, in step three, during washing, the solvent is one or more of anhydrous methanol, anhydrous ethanol, water, dichloromethane, acetonitrile and tetrahydrofuran.

[0036] Preferably, in step three, during drying, vacuum drying is performed at 40 to 60° C. for 24 to 48 hours.

[0037] Beneficial Effects

[0038] 1. The MXene-based nano-expandable flame retardant provided by the present invention is a high-efficiency nano-polymer flame retardant integrating three sources (acid source, gas source, and carbon source). It can achieve UL-94 V-0 grade flame retardant epoxy resin at an addition amount of only 0.5% to 2%. When the addition amount is 1.5%, the limiting oxygen index can reach 30.8%.

[0039] 2. The MXene-based nano-expandable flame retardant provided by the present invention has good compatibility with the matrix, solves the dispersibility problem of nano-MXene materials, and does not cause uneven stacking and dispersion.

[0040] 3. Compared with traditional flame retardants, the MXene-based nano-expandable flame retardant provided by the present invention has better smoke suppression and carbonization effects thanks to the catalytic carbonization effect of titanium, and significantly reduces the heat transfer between the substrate and the outside world. After adding 1.5% of this flame retardant, the peak heat release rate can be reduced by 36.3%, and the smoke suppression effect is good (carbon dioxide production is reduced by 32.5%, carbon monoxide production is reduced by 42.3%), and it has good heat insulation and oxygen isolation effects.

[0041] 4. The MXene-based nano-expanding flame retardant provided by the present invention not only improves the flame retardant properties of polymer materials, but also gives polymer materials more properties. Compared with the original epoxy resin material, the tensile strength is increased by 20% at an addition amount of 1%. The material exhibits conductive properties that the raw materials do not have, and the electromagnetic shielding performance is improved from the original 2.25dB to 3.02dB. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a scanning electron microscope image of the accordion-shaped MXene nanomaterial synthesized in Example 1 of the present invention.

[0043] Figure 2 This is the X-ray diffraction pattern of the accordion-shaped MXene nanomaterial synthesized in Example 1 of the present invention.

[0044] Figure 3 This is the cone calorimetry carbon residue of the EP / MXene@DPC-2 composite material synthesized in Example 1 of the present invention.

[0045] Figure 4 It is the element content of the EP / MXene@DPC-2 composite material synthesized in Example 1 of the present invention.

[0046] Figure 5Element distribution of the EP / MXene@DPC-2 composite material synthesized in Example 1 of the present invention. DETAILED DESCRIPTION

[0047] The present invention will be further described in detail below in conjunction with specific embodiments.

[0048] A method for preparing a MXene-based nano-expandable flame retardant, the specific steps are as follows:

[0049] Step 1: In a closed system without water or oxygen, add fully ground pentaerythritol to solvent A, first stir at room temperature until the system is evenly mixed, raise the system temperature to temperature 1, add freshly distilled phosphorus oxychloride, introduce nitrogen and react under this temperature condition until the system is stable (this process takes 2 to 4 hours), further slowly heat to temperature 2, stir and react until no gas is generated (this process takes 8 to 16 hours), wash the product with solvent B for multiple times, filter and vacuum dry to obtain the intermediate spirocyclic phosphate dichloride.

[0050] In some embodiments, the molar ratio of pentaerythritol to phosphorus oxychloride in step 1 is preferably 1:(2-7), and more preferably 1:(3-5);

[0051] In some embodiments, the solvent A in step 1 is one of anhydrous acetonitrile, acetone, dichloromethane, dioxane or a mixed solvent, and all solvents need to be dried before use to prevent the introduction of moisture;

[0052] In some embodiments, the flow rate of nitrogen in step 1 is 5 to 20 mL / min;

[0053] In some embodiments, the temperature 1 in step 1 is 40-70° C., and the more preferred temperature is 55-65° C. Under this temperature condition, the reaction is more gentle and the yield is higher;

[0054] In some embodiments, the temperature 2 in step 1 is 80-120° C., and a more preferred temperature is 90-110° C.;

[0055] In some embodiments, the stirring rate in step 1 is 220-300 rpm;

[0056] In some embodiments, the solvent B in step 1 is acetone, chloroform, or dichloromethane, and the order of washing is not important.

[0057] Step 2: In an anhydrous and oxygen-free environment, 4,6-dihydroxypyrimidine is added to solvent C, stirred at room temperature until the solution is clear and transparent, the intermediate spirocyclic phosphate dichloride synthesized in step 1 is added, and an acid binding agent is added to make the nucleophilic substitution reaction more complete, pre-react at temperature 3, further slowly heat up, and stir and reflux at temperature 4. After the reaction is completed, the solvent D is used for alternate washing multiple times, filtered, and vacuum dried to obtain a crude flame retardant as a yellow-brown powdery solid.

[0058] In some embodiments, the solvent C in step 2 is one of acetone, tetrahydrofuran, xylene, anhydrous acetonitrile, and N,N-dimethylformamide. All solvents are analytical grade and are soaked in molecular sieves to remove water for 48 hours before use.

[0059] In some embodiments, the molar ratio of 4,6-dihydroxypyrimidine and spirocyclic phosphate dichloride in step 2 is preferably 1:(1-1.5);

[0060] In some embodiments, the temperature 3 in step 2 is 30-55° C., and the pre-reaction is 1-2 hours;

[0061] In some embodiments, the temperature 4 in step 2 is 60-100° C.; more preferably 70-85° C.;

[0062] In some embodiments, the reflux time in step 2 is preferably 12 to 36 hours;

[0063] In some embodiments, the acid-binding agent in step 2 is triethylamine, cerium chloride, anhydrous potassium carbonate and pyridine. The introduction of the acid-binding agent will increase the product yield, but will produce certain ion salts that affect the product purity; therefore, the molar ratio of 4,6-dihydroxypyrimidine to the acid-binding agent is 1:1.5-2.2;

[0064] In some embodiments, the solvent D in step 2 is one or more of deionized water, ether, anhydrous methanol, anhydrous ethanol, dichloromethane, and acetonitrile, and the washing order is not distinguished.

[0065] Step 3: Grind the obtained polymeric flame retardant crude product thoroughly, transfer it to filter paper for wrapping after weighing, and wrap a circle of rubber rope around the filter paper to prevent the loss of the sample during the purification process. Put the filter paper wrapped with the sample horizontally into a Soxhlet extractor with a condensing device, add solvent E to completely soak the filter paper, raise the reaction temperature to 5, cool and reflux for purification, and vacuum dry it after purification to obtain a polymeric spirocyclic phosphorus nitrogen expansion flame retardant.

[0066] In some embodiments, the solvent E in step 3 is one or more of acetone, dichloromethane, anhydrous ethanol, and tetrahydrofuran;

[0067] In some embodiments, the temperature 5 described in step 3 is 60-90° C., which can be selected according to different types of purification solvents to ensure that the selected temperature range is higher than the boiling point of the solvent;

[0068] In some embodiments, the reflux time in step three is preferably 3 to 12 hours, and the reflux time is adjusted according to the solubility of the solvent.

[0069] In some embodiments, the vacuum drying temperature is 80-100° C., and the drying time is 12-24 hours.

[0070] Step 4: Prepare an accordion-shaped MXene nanomaterial, add the MXene nanomaterial into deionized water, and ultrasonicate at 5-10° C. for 1-2 hours to obtain a thin layer of MXene nanomaterial;

[0071] In some embodiments, LiF and a pre-prepared HCl solution are added to a tetrafluoroethylene reactor, stirred at room temperature for 15 minutes until the solution is light yellow, the reaction temperature is increased to 40-50°C, TiC2Al3 powder is added in batches and etched for 24-48 hours, the supernatant is removed by centrifugation, and then washed with deionized water several times until the pH is neutral, and then dried to obtain an accordion-shaped m-MXene material.

[0072] In some embodiments, the concentration of the hydrochloric acid solution is 8-12 mol / L, the usage ratio of LiF to the hydrochloric acid solution is 1-1.5 g:20-40 mL, and the mass ratio of TiC2Al3 powder to LiF is 1:1.3-1.5.

[0073] Step 5: Add the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant and the thin layer MXene nanomaterial into solvent E, ultrasonically disperse for 0.5 to 2 hours, and then heat to 70 to 90° C. under nitrogen protection for reaction for 4 to 10 hours. After the reaction is completed, ultrasonicate at 5 to 10° C. for 1 to 2 hours, centrifuge, wash, and dry to obtain a MXene-based nano intumescent flame retardant.

[0074] In some embodiments, the mass ratio of the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant to the MXene nanomaterial is 1:0.5-2.

[0075] In some embodiments, the solvent E is one or more of methanol, ethanol, deionized water, acetone, N,N-dimethylformamide, acetonitrile and tetrahydrofuran.

[0076] In some embodiments, during washing, the solvent is one or more of anhydrous methanol, anhydrous ethanol, water, dichloromethane, acetonitrile and tetrahydrofuran.

[0077] In some embodiments, the drying is performed under vacuum at 40-60° C. for 24-48 hours.

[0078] The present invention utilizes a polymeric phosphorus-nitrogen intumescent flame retardant and a nano-MXene material surface grafting method to prepare a nano-based intumescent flame retardant having flame retardancy, excellent mechanical properties, electromagnetic shielding, conductivity and other properties, so that the polymer composite material has a better catalytic carbonization effect, a more efficient smoke suppression effect, richer performance advantages and a wider range of applications.

[0079] Example 1

[0080] A method for preparing a polymeric nano-expandable flame retardant modified by MXene material, the specific steps are as follows:

[0081] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 250mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under nitrogen protection until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 65°C and quickly add 69.3g (0.45mol) of newly distilled phosphorus oxychloride. After the system is stable (the time of this process is 3h), slowly increase the temperature to 100°C gradually, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and dry it at 100°C under vacuum conditions (vacuum degree is -0.1MPa) for 12h to obtain 32.4g of white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 85.8%.

[0082] The molar ratio of spirocyclic phosphate dichloride and 4,6-dihydroxypyrimidine was 1:1. 1.12 g (0.01 mol) of 4,6-dihydroxypyrimidine was weighed and added to a 100 mL three-necked flask. The magnetic stirring, condenser and tail gas treatment device were connected. The mixture was stirred in 50 mL acetonitrile under nitrogen protection until it became clear. 2.97 g (0.01 mol) of spirocyclic phosphate dichloride was added, the temperature was raised to 40°C for reaction for 1 hour, and the temperature was further raised to 65°C. The mixture was stirred and refluxed for 20 hours. The precipitate obtained by the reaction was filtered, and washed alternately with water, ether and acetone three times. The crude flame retardant was obtained, and the yellow powder solid was 2.71 g with a yield of 80.9%.

[0083] The dried crude flame retardant was tightly wrapped with filter paper and transferred to a Soxhlet extractor with a reflux condenser. Acetone was used as a purification solvent. The temperature was raised to 65°C and refluxed for 3 hours. After drying, 2.63 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 97.04%.

[0084] Weigh 1g LiF in 20mL 9mol / L HCl, stir at room temperature for 10min, add 1g TiC2Al3 powder in batches, etch for 24h, remove the supernatant by centrifugation, add deionized water and repeat this step until the pH is 7, and dry to obtain accordion-shaped m-MXene material. Take m-MXene and pass nitrogen in deionized water, then perform ultrasonic stripping in an ice-water bath for 1h, obtain a suspension dispersed in water by centrifugation, filter, and dry at 40℃ in vacuum for 12h to obtain a thin layer of MXene material, gray-black solid powder.

[0085] 1 g of the prepared polymeric flame retardant was dispersed in 20 mL of anhydrous methanol, and 0.5 g of a thin layer of MXene material was added. The mixture was reacted in a tetrafluoroethylene reactor at 70 °C for 4 h. The mixed solution was then transferred to a centrifuge tube, protected by nitrogen, and ultrasonicated in an ice-water bath for 1 h. The supernatant was removed by centrifugation, washed with deionized water, and dried in a vacuum oven at 40 °C for 24 h to obtain a polymeric nano-expandable flame retardant modified based on MXene material.

[0086] The infrared and nuclear magnetic spectra of the polymeric phosphorus nitrogen expansion flame retardant show that the structural formula of the flame retardant is: After GPC gel chromatography testing of the polymeric phosphorus nitrogen intumescent flame retardant, it was found that its molecular weight was maintained at 3000 to 4000. The decomposition temperature of the polymeric phosphorus nitrogen intumescent flame retardant was in the range of 250 to 350°C, and the maximum weight loss temperature was at 275°C, which has a beneficial effect on timely response to flame retardancy.

[0087] The scanning electron microscopy results of the accordion-like m-MXene material are as follows Figure 1 The XRD results are shown in Figure 2 shown.

[0088] The nano flame retardant is used to flame retard epoxy resin, and the addition amount is 0.5% to 2%. The preparation method of epoxy resin sample strip is as follows:

[0089] Put the epoxy resin (EP) in an oven, soften it at 80℃ for 0.5h, then weigh it, transfer it to an oil bath at 80℃ for mechanical stirring for standby use. Weigh the required mass fraction of nano-expansion flame retardant, disperse it in acetone and ultrasonicate it at room temperature for 30min. During this period, increase the oven temperature to 120℃, melt the curing agent while preheating the sample. Increase the temperature of the oil bath to 120℃, add the flame retardant and increase the speed until the acetone is completely evaporated (this operation optimizes the problem of uneven dispersion of traditional flame retardants added directly to the system, and the solvent method greatly improves the dispersion of the flame retardant). Then cool it to 80℃, add the completely melted curing agent, stir for 1 to 2min, quickly pour the system into the preheated sample mold, cure at 120℃ for 1h, and cure at 150 for 3h to obtain EP / MXene@DPC, as shown in Table 1.

[0090] Table 1

[0091]

[0092]

[0093] The flame retardant properties of the prepared specimens were tested. At an addition of 1.5% MXene@DPC flame retardant, its limiting oxygen index can reach 30.8%; the vertical combustion test grade can reach UL-94 V-0 level; the peak heat release rate can be reduced by 36.3%, and the smoke suppression effect is good (carbon dioxide production is reduced by 32.5%, carbon monoxide production is reduced by 42.3%), with good heat insulation and oxygen isolation effects. With the increase in the amount of flame retardant, the tensile strength increased by 20% at an addition of 1%, the material showed conductive properties that the raw materials did not have, and the electromagnetic shielding performance was increased from the original 2.25dB to 3.02dB.

[0094] The cone calorimetry carbon residue results of the EP / MXene@DPC-2 are as follows: Figure 3 The element content and distribution results are shown in Figure 4-5 shown.

[0095] Example 2

[0096] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 250mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under vacuum conditions (-0.1MPa) until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 60°C and quickly add 92.4g (0.6mol) of newly distilled phosphorus oxychloride. After the system is stable (the time for this process is 2h), slowly increase the temperature to 105°C in a gradient manner, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and vacuum dry it at 105°C for 12h to obtain 38.6g of white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 90.8%.

[0097] The molar ratio of spirocyclic phosphate dichloride to 4,6-dihydroxypyrimidine was 1:1.1. Weigh 1.12g (0.011mol) of 4,6-dihydroxypyrimidine and add it to a 100mL three-necked flask. Connect the magnetic stirring, condenser and tail gas treatment device. Stir in 50mL acetone under nitrogen protection until it is clear and transparent. Add 2.97g (0.01mol) of spirocyclic phosphate dichloride, heat to 45℃ for 2h, further heat to 70℃, stir and reflux for 22h, filter the precipitate obtained by the reaction, wash it alternately with dichloromethane, ether and acetone three times, and dry it in a vacuum oven at 80℃ for 16h to obtain a crude flame retardant, 2.88g of yellow powder solid, with a yield of 85.9%.

[0098] The crude flame retardant after drying was tightly wrapped with filter paper and transferred to a Soxhlet extractor with a reflux condenser. Dichloromethane was used as a purification solvent, the temperature was raised to 55°C and refluxed for 6 hours. After drying, 2.76 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 98.83%.

[0099] Weigh 1.5g LiF in 40mL 9mol / L HCl, stir at room temperature for 10min, add 1.5g TiC2Al3 powder in batches, etch for 24h, remove the supernatant by centrifugation, add deionized water and repeat this step until the pH is 7, and dry to obtain accordion-shaped m-MXene material. Take m-MXene and pass nitrogen in deionized water, then perform ultrasonic stripping in an ice-water bath for 1h, obtain a suspension dispersed in water by centrifugation, filter, and dry at 80℃ in vacuum for 12h to obtain a thin layer of MXene material, gray-black solid powder.

[0100] 1 g of the prepared polymeric phosphorus-nitrogen intumescent flame retardant was dispersed in 50 mL of anhydrous ethanol, and 1 g of a thin layer of MXene material was added. The mixture was reacted in a tetrafluoroethylene reactor at 75°C for 6 h. The mixed solution was then transferred to a centrifuge tube, protected by nitrogen, and ultrasonicated in an ice-water bath for 1 h. The supernatant was removed by centrifugation, washed with acetonitrile, and dried in a vacuum oven at 40°C for 24 h to obtain a polymeric nano intumescent flame retardant modified based on MXene material.

[0101] The performance of the flame retardant is similar to that of Example 1.

[0102] Example 3

[0103] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 500mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under vacuum conditions (-0.1MPa) until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 55°C and quickly add 115.5g (0.75mol) of newly distilled phosphorus oxychloride. After the system is stable (this process takes 4h), slowly increase the temperature to 105°C in a gradient manner, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and vacuum dry it at 100°C for 12h to obtain 41.3g of a white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 92.8%.

[0104] The molar ratio of spirocyclic phosphate dichloride to 4,6-dihydroxypyrimidine is 1:1.2. 6.72g (0.06mol) of 4,6-dihydroxypyrimidine is weighed and added to a 250mL three-necked flask. The magnetic stirring, condenser and tail gas treatment device are connected. Stir in 100mL tetrahydrofuran under nitrogen protection until it is clear and transparent. 14.84g (0.05mol) of spirocyclic phosphate dichloride is ultrasonically dispersed in a beaker containing 80ml tetrahydrofuran for 30min, added to the three-necked flask and stirred evenly, 20ml of triethylamine is added and the temperature is raised to 45℃ for pre-reaction for 2h, and the temperature is further raised to 75℃ for reaction for 20h. The precipitate obtained by the reaction is filtered, and washed alternately with water, acetone and ether three times, and dried in a vacuum oven at 80℃ for 24h to obtain 15.15g of yellow-brown powder solid with a yield of 90.2%.

[0105] The crude flame retardant after drying was divided into three parts, tightly wrapped with multiple layers of filter paper, and transferred to a Soxhlet extractor with a reflux condenser. Anhydrous ethanol was used as a purification solvent. The temperature was raised to 80°C and refluxed for 8 hours. After drying, 14.72 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 97.16%.

[0106] Weigh 1.3g LiF in 30mL 9mol / L HCl, stir at room temperature for 10min, add 1.6g TiC2Al3 powder in batches, etch for 24h, remove the supernatant by centrifugation, add deionized water and repeat this step until the pH is 7, and dry to obtain accordion-shaped m-MXene material. Take m-MXene and pass nitrogen in deionized water, then perform ultrasonic exfoliation in an ice-water bath for 1h, obtain a suspension dispersed in water by centrifugation, filter, and dry at 40℃ in vacuum for 12h to obtain a thin layer of MXene material, gray-black solid powder.

[0107] 1 g of the prepared polymeric phosphorus-nitrogen intumescent flame retardant was dispersed in 80 mL of acetone, and 1.5 g of a thin layer of MXene material was added. The mixture was reacted in a tetrafluoroethylene reactor at 80 °C for 8 h. The mixed solution was then transferred to a centrifuge tube, protected by nitrogen, and ultrasonicated in an ice-water bath for 1 h. The supernatant was removed by centrifugation, washed with acetonitrile, and dried in a vacuum oven at 40 °C for 24 h to obtain a polymeric nano intumescent flame retardant modified based on MXene material.

[0108] The performance of the flame retardant is similar to that of Example 1.

[0109] Example 4

[0110] Weigh 20.4g (0.15mol) of fully ground pentaerythritol into a 250mL three-necked flask, connect magnetic stirring, a condenser with tail gas treatment, and a constant pressure dropping funnel. Stir at room temperature under vacuum conditions (-0.1MPa) until the system is evenly mixed. In a nitrogen atmosphere (nitrogen flow rate is 10mL / min), slowly heat to 60°C and quickly add 115.5g (0.75mol) of newly distilled phosphorus oxychloride. After the system is stable (the time of this process is 3h), slowly increase the temperature to 105°C gradually, and react until no HCl gas is produced at the tail gas outlet (reaction is over). Cool to room temperature, filter the obtained precipitate, wash it alternately with dichloromethane and acetone several times, and vacuum dry it at 100°C for 12h to obtain 42.1g of white powdery solid intermediate, which is spirocyclic phosphate dichloride, with a yield of 94.6%.

[0111] The molar ratio of spirocyclic phosphate dichloride to 4,6-dihydroxypyrimidine was 1:1.3, 24.7g (0.065mol) of 4,6-dihydroxypyrimidine was weighed, added to a 500mL three-necked flask, connected with magnetic stirring, condenser, and tail gas treatment device, and stirred in 200mL acetonitrile under nitrogen protection until clear and transparent. 14.84g (0.05mol) of spirocyclic phosphate dichloride was ultrasonically dispersed in a beaker containing 160ml tetrahydrofuran for 50min, added to the three-necked flask and stirred evenly, 28ml of triethylamine was added and heated to 50℃ for pre-reaction for 2h, and further heated to 80℃ for reaction for 24h, and the precipitate obtained by the reaction was filtered, washed alternately with water and ether acetone three times, and dried in a vacuum oven at 80℃ for 24h to obtain a crude flame retardant, 15.97g of yellow-brown powder solid, and a yield of 95.1%.

[0112] The crude flame retardant after drying was divided into three parts, tightly wrapped with multiple layers of filter paper, and transferred to a Soxhlet extractor with a reflux condenser. Tetrahydrofuran was used as a purification solvent, and the temperature was raised to 75°C and refluxed for 12 hours. After drying, 15.33 g of a yellow powdery solid was obtained, which was a purified polymeric phosphorus-nitrogen intumescent flame retardant with a yield of 95.99%.

[0113] Weigh 1.2g LiF in 20mL 9mol / L HCl, stir at room temperature for 10min, add 1.68g TiC2Al3 powder in batches, etch for 48h, remove the supernatant by centrifugation, add deionized water and repeat this step until the pH is 7, and dry to obtain accordion-shaped m-MXene material. Take m-MXene and pass nitrogen in deionized water, then perform ultrasonic exfoliation in an ice-water bath for 1h, obtain a suspension dispersed in water by centrifugation, filter, and dry at 40℃ in vacuum for 12h to obtain a thin layer of MXene material, gray-black solid powder.

[0114] 1 g of the prepared polymeric phosphorus-nitrogen intumescent flame retardant was dispersed in 80 mL of anhydrous methanol, and 2 g of a thin layer of MXene material was added. The mixture was reacted in a tetrafluoroethylene reactor at 80 °C for 10 h. The mixed solution was then transferred to a centrifuge tube, protected by nitrogen, ultrasonicated in an ice-water bath for 1 h, and centrifuged to remove the supernatant. The mixture was washed with anhydrous ethanol and dried in a vacuum oven at 40 °C for 24 h to obtain a polymeric nano-intumescent flame retardant modified based on MXene material.

[0115] The performance of the flame retardant is similar to that of Example 1.

[0116] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.

Claims

1. A MXene-based nano-expandable flame retardant, characterized in that: It is composed of a polymeric spirocyclic phosphorus nitrogen expansion flame retardant and a MXene nanomaterial, wherein the polymeric spirocyclic phosphorus nitrogen expansion flame retardant is grafted or physically bonded on the surface of a single layer of MXene nanomaterial; Wherein, the structural formula of the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant is as follows: The repeating unit is C9O8N2H 10 P2, the degree of polymerization n is an integer from 8 to 12; The molecular formula of MXene nanomaterials is Ti3C2T x , wherein T is a hydroxyl group or a carbonyl group.

2. A MXene-based nano-expandable flame retardant according to claim 1, characterized in that: The molecular weight of the polymeric spirophosphorus nitrogen expansion flame retardant is 3000-4000.

3. A MXene-based nano-expandable flame retardant according to claim 1 or 2, characterized in that: The mass ratio of the polymeric spirocyclic phosphorus nitrogen expansion flame retardant to the MXene nanomaterial is 1:0.5-2.

4. A method for preparing a MXene-based nano-expandable flame retardant according to any one of claims 1 to 3, characterized in that: The method steps include: Step 1: In an anhydrous and oxygen-free closed system, pentaerythritol is added to solvent A, stirred until the system is uniformly mixed, the temperature is raised to temperature 1, phosphorus oxychloride is added, nitrogen is introduced and the reaction is kept warm for 2 to 4 hours, and then the temperature is raised to temperature 2 and stirred for 8 to 16 hours, washed and dried to obtain an intermediate spirocyclic phosphate dichloride; wherein the molar ratio of pentaerythritol to phosphorus oxychloride is 1:2 to 7; temperature 1 is 40 to 70°C, and temperature 2 is 80 to 120°C; in an anhydrous and oxygen-free environment, 4,6-dihydroxypyrimidine is added to solvent B and stirred until The solution is clear and transparent, the intermediate spirocyclic phosphate dichloride and the acid binding agent are added, and the reaction is carried out at a temperature of 3 for 1 to 2 hours, and then the temperature is raised to a temperature of 4 and stirred and refluxed for 6 to 16 hours. After the reaction is completed, the solution is washed and dried to obtain a crude flame retardant, which is a yellow-brown powdery solid; wherein the molar ratio of 4,6-dihydroxypyrimidine to spirocyclic phosphate dichloride is 1:1 to 1.5, the temperature 3 is 30 to 55° C., and the temperature 4 is 60 to 100° C. After the crude flame retardant is ground, it is refluxed for purification, and dried to obtain a polymeric spirocyclic phosphorus nitrogen expansion flame retardant; Step 2: Prepare an accordion-shaped MXene nanomaterial by adding the MXene nanomaterial into deionized water and ultrasonicating it at 5-10°C for 1-2 hours to obtain a thin layer of MXene nanomaterial; Step 3: Add the polymeric spirocyclic phosphorus nitrogen intumescent flame retardant and the thin layer MXene nanomaterial into solvent E, ultrasonically disperse for 0.5 to 2 hours, and then heat to 70 to 90° C. under nitrogen protection for reaction for 4 to 10 hours. After the reaction is completed, ultrasonicate at 5 to 10° C. for 1 to 2 hours, centrifuge, wash, and dry to obtain a MXene-based nano intumescent flame retardant.

5. The method for preparing a MXene-based nano-expandable flame retardant according to claim 4, characterized in that: In step 1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:3-5; the stirring rate is 220-300 rpm; the flow rate when nitrogen is introduced is 5-20 mL / min; temperature 1 is 55-65° C.; temperature 2 is 90-110° C.; the solvent A is one or more of anhydrous acetonitrile, acetone, dichloromethane and dioxane; and one or more of acetone, chloroform and dichloromethane are used for washing.

6. The method for preparing a MXene-based nano-expandable flame retardant according to claim 4, characterized in that: In step 1, the solvent B is one or more of acetone, tetrahydrofuran, xylene, anhydrous acetonitrile and N,N-dimethylformamide; the acid binding agent is one or more of triethylamine, cerium chloride, anhydrous potassium carbonate and pyridine; the molar ratio of 4,6-dihydroxypyrimidine to the acid binding agent is 1:1.5-2.2; the temperature 4 is 70-85° C.; and the washing is carried out using one or more of deionized water, ether, anhydrous methanol, anhydrous ethanol, dichloromethane and acetonitrile.

7. The method for preparing a MXene-based nano-expandable flame retardant according to claim 4, characterized in that: During reflux purification, the solvent is one or more of acetone, dichloromethane, anhydrous ethanol and tetrahydrofuran; the temperature is 60-90°C, and the cooling reflux is carried out for 3-12 hours; during drying, vacuum drying is carried out at 80-100°C for 12-24 hours.

8. The method for preparing a MXene-based nano-expandable flame retardant according to claim 4, characterized in that: In step 2, when preparing the accordion-shaped MXene nanomaterial, LiF and hydrochloric acid solution are mixed and stirred for more than 15 minutes, then the temperature is raised to 40-50°C, TiC2Al3 powder is added in batches and then etched for 24-48 hours, and the accordion-shaped MXene nanomaterial is obtained after centrifugation, washing to neutrality, and drying.

9. The method for preparing a MXene-based nano-expandable flame retardant according to claim 8, characterized in that: The concentration of the hydrochloric acid solution is 8-12 mol / L, the dosage ratio of LiF to the hydrochloric acid solution is 1-1.5 g:20-40 mL, and the mass ratio of TiC2Al3 powder to LiF is 1:1.3-1.

5.

10. The method for preparing a MXene-based nano-expandable flame retardant according to claim 8, characterized in that: In step three, the mass ratio of the polymeric spirophosphorus nitrogen intumescent flame retardant and the MXene nanomaterial is 1:0.5-2; the solvent E is one or more of methanol, ethanol, deionized water, acetone, N,N-dimethylformamide, acetonitrile and tetrahydrofuran; when washing, the solvent is one or more of anhydrous methanol, anhydrous ethanol, water, dichloromethane, acetonitrile and tetrahydrofuran; when drying, vacuum drying is performed at 40-60°C for 24-48h.

Citation Information

Cited By

  • High-flame-retardant epoxy adhesive as well as preparation method and application thereof

    CN119875561A