High-light-color-fastness thermoplastic elastomer material for automotive trim and preparation method of high-light-color-fastness thermoplastic elastomer material

Through the combination of high hydrogenation SEBS and high crystallinity polypropylene, combined with the use of specific additives, the problem of aging of thermoplastic elastomer materials under high light conditions is solved, and the material has high aging resistance and ultraviolet resistance are achieved. In the field of automotive interior.

CN118931093APending Publication Date: 2024-11-12ANHUI ZHONGHAN POLYMER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192070.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The mechanical properties of existing thermoplastic elastomer materials are reduced under high light conditions, and aging leads to color changes, reducing the service life of the material and unable to meet the high demand in the automotive interior field.

Method used

Using a combination of high hydrogenation SEBS, high crystallinity polypropylene and specific additives, a thermoplastic elastomer material with high color fastness is prepared through a twin-screw extrusion process. The additive contains hindered amines and benzotriazole structures that can Capture free radicals degraded by photooxidation and enhance the material's anti-UV aging properties.

Benefits of technology

It significantly improves the material's aging resistance, UV resistance and light stability, extends the service life of the material, ensures high color fastness under high light conditions, and is suitable for automotive interior materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015380950000031
    Figure BDA0005015380950000031
  • Figure BDA0005015380950000041
    Figure BDA0005015380950000041
  • Figure BDA0005015380950000042
    Figure BDA0005015380950000042
Patent Text Reader

Abstract

The invention discloses a high-light-color-fastness thermoplastic elastomer material for automotive interiors and a preparation method of the high-light-color-fastness thermoplastic elastomer material, and belongs to the technical field of thermoplastic elastomers. Comprising the following raw materials in parts by weight: 15-30 parts of SEBS, 10-60 parts of paraffin oil, 10-20 parts of homo-polypropylene, 0.1-0.3 part of an initiator, 4-12 parts of an auxiliary agent, 2-4 parts of a lubricant and 15-30 parts of a filler. Wherein SEBS is high in hydrogenation degree, so that the material is endowed with good stability and aging resistance; the polypropylene with high crystallinity is good in heat-resistant stability, and the paraffin oil is good in yellowing resistance, so that the heat-resistant stability and aging resistance of the material are enhanced; wherein the auxiliary agent can greatly enhance the ultraviolet aging resistance and light stability of the matrix, and the performance is long-lasting and stable; therefore, the prepared material has stable and efficient aging resistance, ultraviolet resistance and light stability, so that the color fastness is high under high illumination, and the material has important application value in the field of automotive interior materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoplastic elastomers, and in particular relates to a thermoplastic elastomer material for automobile interior decoration with high light color fastness and a preparation method thereof. Background Art

[0002] With the development of the automobile industry, people's requirements for the beauty of automobile interiors have gradually increased in addition to the increasing requirements for automobile driving. As a result, more and more automobile interior color matching has come about, which requires that the color stability of automobile interior materials after color matching should be high.

[0003] Thermoplastic elastomer (TPE) is a material that combines the elastic properties of rubber and the processing convenience of plastic. It has the characteristics of environmental protection and non-toxicity, a wide range of hardness, excellent colorability, soft touch, weather resistance, fatigue resistance and temperature resistance. TPE has excellent processing performance, does not require vulcanization, can be recycled, reduces costs, and can be coated, bonded or molded separately with a variety of plastic materials such as PP, PE, PC, PS, ABS, etc., for example, it is used to manufacture seals, shock absorption systems, interior and exterior parts, wiring harnesses and cables, hoses and pipeline systems, etc., and because it has a good touch, high processing efficiency, and relatively cheap price, TPE materials have begun to become the darling of the automotive interior material field in recent years, but the quality of the material can be said to be mixed, and sunlight will shine on part of the automotive interior materials through the windshield of the car. Long-term exposure will cause the mechanical properties of the automotive interior materials to decrease, and age, causing the materials to turn yellow and discolor, reducing the service life of the materials. Therefore, there is an urgent need to invent a thermoplastic elastomer material with high light color fastness to meet its higher demands in the field of automotive interiors. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a thermoplastic elastomer material for automobile interior decoration with high light color fastness and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a thermoplastic elastomer material for automobile interior decoration with high light color fastness comprises the following steps:

[0007] Styrene-ethylene-butylene-styrene block copolymer (SEBS) and paraffin oil are placed in a high-mixing device and fully mixed. After the paraffin oil is completely absorbed by the SEBS, homopolymer polypropylene, initiator, additive, lubricant and filler are added and stirred for 30 minutes, and then added to a twin-screw extruder, melt-blended and extruded to obtain a thermoplastic elastomer material for automotive interior with high light color fastness.

[0008] Furthermore, the raw materials are calculated in parts by weight as follows: 15-30 parts of SEBS, 10-60 parts of paraffin oil, 10-20 parts of homopolypropylene, 0.1-0.3 parts of initiator, 4-12 parts of auxiliary agent, 2-4 parts of lubricant, and 15-30 parts of filler.

[0009] Furthermore, the SEBS is a high-hydrogenation degree SEBS, and its hydrogenation degree is required to be ≥99.98%.

[0010] Furthermore, the CP value of the paraffin oil is ≥65%, and the CN value is ≤35%.

[0011] Furthermore, the homopolypropylene is a high-crystallinity homopolypropylene, and the crystallinity is ≥65%.

[0012] Furthermore, the initiator is one of cyclohexanone peroxide and dibenzoyl peroxide.

[0013] Furthermore, the filler is one or more of calcium carbonate, barium sulfate, mica powder, calcined clay, and talc powder.

[0014] Furthermore, the lubricant is one or more of silicone powder, stearic acid, calcium stearate, and zinc stearate.

[0015] Furthermore, the temperature range of the twin-screw extruder is 160-210° C., the rotation speed is 300-400 rpm, and the screw length-to-diameter ratio is 55-64.

[0016] Using SEBS with a high degree of hydrogenation means fewer double bonds. Double bonds are less stable and are more likely to break under aging conditions such as light or high temperatures, causing the material to yellow. Therefore, using SEBS with a high degree of hydrogenation as a matrix can give the material good stability and aging resistance. In addition, polypropylene with high crystallinity has good heat stability, high CP value, and low CN value. The yellowing resistance of paraffin oil will be more prominent, enhancing the material's heat stability and aging resistance.

[0017] Furthermore, the auxiliary agent is prepared by the following steps:

[0018] S1. Add 3-butene-1-amine, trimesic acid, dicyclohexylcarbodiimide (DCC, dehydrating agent) and toluene to a three-necked flask equipped with a stirring device, stir and mix well, place in a 55° C. water bath, heat in a water bath for 4 h, and after the reaction is completed, remove the solvent by vacuum distillation, wash with ethanol 2-3 times, and vacuum dry to obtain intermediate 1; the ratio of 3-butene-1-amine, trimesic acid, dicyclohexylcarbodiimide and toluene is 7.1 g:22.1 g:20.6 g:100 mL;

[0019] Under the action of a dehydrating agent, 3-butene-1-amine and trimesic acid undergo an amidation reaction. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of trimesic acid, only one carboxyl group on the trimesic acid participates in the reaction to obtain intermediate 1. The specific reaction process is shown below:

[0020]

[0021] S2. Add 1-aminobenzotriazole, intermediate 1, dicyclohexylcarbodiimide (DCC, dehydrating agent) and toluene to a three-necked flask equipped with a stirring device, stir and mix well, place in a water bath at 55°C, heat in a water bath for 8 hours, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 3:2), remove the eluent by rotary evaporation to obtain intermediate 2; the ratio of 1-aminobenzotriazole, intermediate 1, dicyclohexylcarbodiimide and toluene is 13.4g:28.7g:20.6g:150mL;

[0022] Under the action of a dehydrating agent, 1-aminobenzotriazole and intermediate 1 undergo an amidation reaction. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of intermediate 1, only one carboxyl group on intermediate 1 participates in the reaction to obtain intermediate 2. The specific reaction process is as follows:

[0023]

[0024] S3. In a three-necked flask equipped with a stirring device, the intermediate 2, pentamethylpiperidinol and N,N-dimethylformamide (DMF) were mixed and stirred uniformly, and then dibutyltin oxide (catalyst) and dicyclohexylcarbodiimide (DCC) were added, and the temperature was raised to 85°C for reaction for 4 hours. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / benzene in a volume ratio of 3:2), and the eluent was removed by rotary evaporation to obtain an auxiliary agent; the ratio of the amount of intermediate 2, pentamethylpiperidinol, N,N-dimethylformamide, dibutyltin oxide and dicyclohexylcarbodiimide was 38.1 g:17.1 g:150 mL:0.2 g:20.6 g;

[0025] Under the catalysis of dibutyltin oxide and DCC, the hydroxyl group on pentamethylpiperidinol and the carboxyl group on intermediate 2 undergo esterification reaction to obtain an auxiliary agent; the specific reaction process is as follows:

[0026]

[0027] The prepared auxiliary agent molecule contains hindered amine, benzotriazole and carbon-carbon double bond structure, among which the hindered amine plays the role of light stabilizer, decomposes hydrogen dioxide to produce stable nitroxide free radicals in light protection, and this compound can very effectively capture the free radicals produced in photo-oxidative degradation, can effectively inhibit the photo-oxidative degradation of the matrix, and can be regenerated under stable conditions, which significantly improves the light stability of the matrix, can play a synergistic role with benzotriazole, and further enhances the anti-ultraviolet aging performance of the matrix; in addition, one end of the auxiliary agent contains a carbon-carbon double bond, which can be cross-linked with the matrix during the blending process, thereby improving the migration resistance and exudation resistance of the auxiliary agent, making the performance of the auxiliary agent more stable.

[0028] Beneficial effects of the present invention:

[0029] 1. The material prepared by the present invention uses SEBS with a high degree of hydrogenation, which gives the material good stability and aging resistance;

[0030] 2. Polypropylene with high crystallinity has good heat resistance and stability, and the addition of paraffin oil with high CP value and low CN value will make its yellowing resistance more prominent, thus enhancing the heat resistance and aging resistance of the material.

[0031] 3. The prepared additive can greatly enhance the anti-ultraviolet aging performance and light stability of the substrate, and the performance is long-term and stable;

[0032] Therefore, the material prepared by the present invention has stable and efficient aging resistance, UV resistance, and light stability, and therefore has high color fastness under high light, and has important application value in the field of automotive interior materials. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] Preparation aids:

[0036] S1. Add 7.1 g of 3-butene-1-amine, 22.1 g of trimesic acid, 20.6 g of dicyclohexylcarbodiimide and 100 mL of toluene into a three-necked flask equipped with a stirring device, stir and mix well, place in a 55° C. water bath, and heat in a water bath for 4 h. After the reaction is completed, remove the solvent by distillation under reduced pressure, wash with ethanol 3 times, and dry in vacuo to obtain intermediate 1;

[0037] S2, in a three-necked flask equipped with a stirring device, add 13.4g 1-aminobenzotriazole, 28.7g intermediate 1, 20.6g dicyclohexylcarbodiimide and 150mL toluene, stir and mix well, place in a 55°C water bath, heat in a water bath for 8h, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0038] S3. In a three-necked flask equipped with a stirring device, 38.1 g of intermediate 2, 17.1 g of pentamethylpiperidinol and 150 mL of N,N-dimethylformamide were mixed and stirred evenly, and then 0.2 g of dibutyltin oxide and 20.6 g of dicyclohexylcarbodiimide were added, and the temperature was raised to 85°C for reaction for 4 hours. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / benzene in a volume ratio of 3:2), and the eluent was removed by rotary evaporation to obtain an auxiliary agent.

[0039] Example 2

[0040] Preparation aids:

[0041] S1. Add 14.2 g of 3-butene-1-amine, 44.2 g of trimesic acid, 41.2 g of dicyclohexylcarbodiimide and 200 mL of toluene into a three-necked flask equipped with a stirring device, stir and mix well, place in a 55° C. water bath, and heat in a water bath for 4 h. After the reaction is completed, remove the solvent by distillation under reduced pressure, wash with ethanol twice, and dry in vacuo to obtain intermediate 1;

[0042] S2, in a three-necked flask equipped with a stirring device, add 26.8g 1-aminobenzotriazole, 57.4g intermediate 1, 41.2g dicyclohexylcarbodiimide and 300mL toluene, stir and mix well, place in a 55°C water bath, heat in a water bath for 8h, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 3:2), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0043] S3. In a three-necked flask equipped with a stirring device, 76.2 g of intermediate 2, 34.2 g of pentamethylpiperidinol and 300 mL of N,N-dimethylformamide were mixed and stirred evenly, and then 0.4 g of dibutyltin oxide and 41.2 g of dicyclohexylcarbodiimide were added, and the temperature was raised to 85°C for reaction for 4 hours. Stirring was continued during the reaction. After the reaction was completed, the product was filtered, and part of the solvent was removed by rotary evaporation. The product was purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / benzene in a volume ratio of 3:2), and the eluent was removed by rotary evaporation to obtain an auxiliary agent.

[0044] Example 3

[0045] 15g SEBS (hydrogenation degree of 99.98%) and 10g paraffin oil (CP value of 65%, CN value of 35%) were placed in a high mixing device and fully mixed. After the paraffin oil was completely absorbed by the SEBS, 10g homopolypropylene (crystallinity of 65%), 0.1g cyclohexanone peroxide, 4g of the auxiliary agent prepared in Example 1, 2g silicone powder and 15g calcium carbonate were added and stirred for 30 minutes. The mixture was added to a twin-screw extruder and the temperature was controlled at 160°C, the rotation speed was 300rpm, and the screw aspect ratio was 55. The mixture was melt-blended and extruded to obtain a thermoplastic elastomer material for automotive interior with high light color fastness.

[0046] Example 4

[0047] 25g SEBS (hydrogenation degree of 99.98%) and 30g paraffin oil (CP value of 75%, CN value of 30%) were placed in a high mixing device and fully mixed. After the paraffin oil was completely absorbed by the SEBS, 10-20g homopolypropylene (crystallinity of 70%), 0.2g cyclohexanone peroxide, 8g of the auxiliary agent prepared in Example 2, 3g stearic acid and 20g calcined clay were added and stirred for 30 minutes. The mixture was added to a twin-screw extruder with the temperature controlled at 180°C, the rotation speed at 350rpm, and the screw aspect ratio of 60. The mixture was melt-blended and extruded to obtain a thermoplastic elastomer material for automotive interior with high light color fastness.

[0048] Example 5

[0049] 30g SEBS (hydrogenation degree of 99.98%) and 60g paraffin oil (CP value of 75%, CN value of 30%) were placed in a high mixing device and fully mixed. After the paraffin oil was completely absorbed by the SEBS, 20g homopolypropylene (crystallinity of 75%), 0.2g cyclohexanone peroxide, 12g of the auxiliary agent prepared in Example 2, 4g calcium stearate and 30g barium sulfate were added and stirred for 30min. The mixture was added to a twin-screw extruder and the temperature was controlled at 210°C, the rotation speed was 400rpm, and the screw aspect ratio was 64. The mixture was melt-blended and extruded to obtain a thermoplastic elastomer material for automotive interior with high light color fastness.

[0050] Comparative Example 1

[0051] The additive in Example 5 was replaced by a commercially available anti-ultraviolet additive of equal quality, and the remaining steps were the same as those in Example 5 to obtain the material.

[0052] Comparative Example 2

[0053] Use commercially available, high color fastness thermoplastic elastomer materials.

[0054] Examples 3-5 and comparative examples 1-2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:

[0055] The elongation at break is determined using the national standard GB / T 1040.1-2018 "Determination of tensile properties of plastics Part 1: General principles";

[0056] The sample was placed in a xenon lamp aging test chamber for accelerated aging for 7 days. The aging conditions were air atmosphere, a xenon lamp wavelength of 500nm, and an irradiation intensity of 550W / m 2 , test the tensile strength of the sample before and after aging (GB / T1040-2006); compare the fading degree of the sample with the standard color sample, and determine the color fastness (the color fastness rating is divided into 8 levels, 8 is the best, and 1 is the worst); finally, test the grayscale level;

[0057] The measured results are shown in the following table:

[0058]

[0059] It can be seen from the above table that the material prepared in the embodiment of the present invention has high color fastness, high grayscale, excellent UV resistance, and has important application value in the field of automotive interior materials.

[0060] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0061] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a thermoplastic elastomer material for automobile interior with high light color fastness, characterized in that: The following steps are involved: SEBS and paraffin oil are placed in a high-mixing device and fully mixed. After the paraffin oil is completely absorbed by SEBS, homopolymer polypropylene, initiator, additive, lubricant and filler are added and stirred and mixed, and then added to a twin-screw extruder, melt blended, and extruded to obtain a thermoplastic elastomer material for automotive interior with high light color fastness.

2. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 1, characterized in that: The auxiliary agent is prepared by the following steps: S1. Add 3-butene-1-amine, trimesic acid, dicyclohexylcarbodiimide and toluene into a three-necked flask, stir and mix evenly, heat at 55° C. for 4 h, and when the reaction is complete, evaporate under reduced pressure, wash, and dry in vacuum to obtain intermediate 1. S2. Add 1-aminobenzotriazole, intermediate 1, dicyclohexylcarbodiimide and toluene into a three-necked flask, stir and mix well, heat at 55° C. for 8 h, and when the reaction is complete, filter, distill under reduced pressure, purify by column chromatography, and rotary evaporate to obtain intermediate 2; S3. Mix the intermediate 2, pentamethylpiperidinol and N,N-dimethylformamide and stir evenly, then add dibutyltin oxide and dicyclohexylcarbodiimide, and react at 85°C for 4 hours with continuous stirring during the reaction. After the reaction is completed, filter, rotary evaporate, purify by column chromatography, and rotary evaporate to obtain an auxiliary agent.

3. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 2, characterized in that: In step S1, the ratio of 3-butene-1-amine, trimesic acid, dicyclohexylcarbodiimide and toluene is 7.1 g: 22.1 g: 20.6 g: 100 mL.

4. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 2, characterized in that: In step S2, the ratio of 1-aminobenzotriazole, intermediate 1, dicyclohexylcarbodiimide and toluene is 13.4 g: 28.7 g: 20.6 g: 150 mL.

5. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 2, characterized in that: In step S3, the ratio of the amount of intermediate 2, pentamethylpiperidinol, N,N-dimethylformamide, dibutyltin oxide, and dicyclohexylcarbodiimide is 38.1 g:17.1 g:150 mL:0.2 g:20.6 g.

6. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 1, characterized in that: The raw materials are calculated in parts by weight as follows: 15-30 parts of SEBS, 10-60 parts of paraffin oil, 10-20 parts of homopolypropylene, 0.1-0.3 parts of initiator, 4-12 parts of auxiliary agent, 2-4 parts of lubricant, and 15-30 parts of filler.

7. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 1, characterized in that: The SEBS is a high-hydrogenation SEBS, and its hydrogenation degree is required to be ≥99.98%.

8. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 1, characterized in that: The CP value of the paraffin oil is ≥65%, and the CN value is ≤35%.

9. The method for preparing a thermoplastic elastomer material for automotive interior decoration with high light color fastness according to claim 1, characterized in that: The homopolymer polypropylene is a high-crystallinity homopolymer polypropylene, and the crystallinity is ≥65%.

10. A thermoplastic elastomer material for automobile interior decoration with high light color fastness, characterized in that: Prepared according to the method according to any one of claims 1 to 9.