High-heat-conductivity and high-elasticity heat-conducting silica gel as well as preparation method and application thereof

Through the self-polymerization and cross-linking reaction of expanded graphite, aluminum powder and other raw materials, a high thermal conductivity and high elasticity thermal conductivity silicone is formed, which solves the problem of reduced elasticity after the increase of thermal filler, achieves the balance of thermal conductivity and elasticity, and enhances the buffering of silicone and adhesion properties.

CN118931185AInactive Publication Date: 2024-11-12DONGGUAN HONGYI THERMAL CONDUCTMTY MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411027189.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

After adding thermal filler to thermal silicone, thermal conductivity is improved but elasticity is reduced, affecting its buffering effect and service life.

Method used

The raw materials such as expanded graphite, aluminum powder, methacrylic monomers, unsaturated silanes, bis(2-ethylhexyl)maleate are used to form a thermally conductive silicone with high thermal conductivity and high elasticity through self-polymerization and cross-linking reaction. Improves its thermal conductivity and elasticity while enhancing adhesion and flexibility.

Benefits of technology

The thermally conductive silicone has good thermal conductivity, elasticity and adhesion, reducing bumps between parts, improving heat dissipation effect and installation stability, and reducing the possibility of falling off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to high-heat-conductivity and high-elasticity heat-conducting silica gel as well as a preparation method and application thereof. The heat-conducting rubber is prepared from the following raw materials in percentage by weight: 20-50% of raw rubber, 1-3% of a platinum vulcanizing agent, 3-17% of a filler and 40-76% of a modified heat-conducting filler, the modified heat-conducting filler is prepared from expanded graphite, aluminum powder, hydrogen-containing silane, a methallyl monomer, unsaturated silane, bis (2-ethylhexyl) maleate and an initiator. The preparation method comprises the following steps: self-polymerizing a methylacrylic monomer, and further compounding with unsaturated silane, hydrogen-containing silane and bis (2-ethylhexyl) maleate to prepare a compound, so that the compatibility of aluminum powder and expanded graphite in raw rubber can be further improved, and meanwhile, the compound can be further subjected to a cross-linking reaction with the raw rubber; therefore, the obtained heat-conducting silica gel has better heat-conducting property and elasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of thermally conductive silicone, and more specifically, to a thermally conductive silicone with high thermal conductivity and high elasticity, and a preparation method and application thereof. Background Art

[0002] Thermal conductive silicone is commonly used in a wide range of applications such as electronics, electrical appliances, and automobiles, such as the bottom or frame of radiators, high-speed hard disk drives, automobile engine control devices, and semiconductor automatic test equipment, to improve heat dissipation performance, extend service life, or act as a buffer to reduce collisions and damage between components.

[0003] Usually, metal oxides, graphene, and hexagonal boron nitride are added to thermally conductive silicone to improve its thermal conductivity. However, with the increase of thermally conductive fillers, the elasticity of the thermally conductive silicone is significantly reduced, thereby reducing the buffering effect of the thermally conductive silicone. Further research is needed for this. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a thermally conductive silicone with high thermal conductivity and high elasticity, and a preparation method and application thereof.

[0005] In a first aspect, the present application provides a thermally conductive silicone with high thermal conductivity and high elasticity, which is made from the following raw materials in percentage by weight: Raw rubber 20-50% Platinum vulcanizing agent 1-3% Filler 3-17% Modified thermal conductive filler 40-76%; The modified thermal conductive filler is prepared from expanded graphite, aluminum powder, hydrogen-containing silane, methacrylic monomer, unsaturated silane, bis(2-ethylhexyl) maleate and an initiator.

[0006] In the above technical solution, the expanded graphite is a porous worm-like structure, which has softness and compression resilience that natural graphite does not have, and has good thermal conductivity; and the aluminum powder has high thermal conductivity. When the aluminum powder is compounded with the expanded graphite, the thermal conductive silica gel has both good thermal conductivity and elasticity. The methacrylic monomer can form a macromolecular polymer by self-polymerization, and after the unsaturated silane, hydrogen-containing silane, and bis(2-ethylhexyl) maleate are blended with it, the formed composite can modify the surface of the expanded graphite and aluminum powder, thereby improving the compatibility of the expanded graphite, aluminum powder and raw rubber. At the same time, the composite can further cross-link with the raw rubber to form a cross-linked network structure, thereby making the prepared thermal conductive silica gel have both good elasticity and thermal conductivity. When used in a heat dissipation device, it plays a better buffering role and reduces its damage.

[0007] Among them, unsaturated silane, hydrogen-containing silane, and bis(2-ethylhexyl) maleate can all be used as crosslinking agents to promote the crosslinking of thermal conductive silicone grease to form a network structure, and interact with methacrylic monomers to improve the compatibility of expanded graphite and aluminum powder in thermal conductive silicone. Bis(2-ethylhexyl) maleate can also increase flexibility and wear resistance, making the thermal conductive silicone have better adhesion, flexibility, elasticity and thermal conductivity.

[0008] In summary, after the methacrylic monomers are self-polymerized, they are further compounded with unsaturated silane, hydrogen-containing silane, and bis(2-ethylhexyl) maleate to obtain a compound that can further improve the compatibility of aluminum powder and expanded graphite in raw rubber, and can further undergo a cross-linking reaction with the raw rubber, so that the thermally conductive silicone rubber has better thermal conductivity, elasticity, and adhesion. This makes the silicone rubber have better elasticity during use, reduces the collision between parts, and has better heat dissipation. It is easy to adhere to the surface of metal and plastic, reduces the possibility of falling off, and provides installation stability.

[0009] Preferably, the weight ratio of the expanded graphite, aluminum powder, hydrogen-containing silane, methacrylic monomer, unsaturated silane, bis(2-ethylhexyl)maleate, and initiator is (2.0-3.5):(0.3-0.5):(1-3):(0.25-0.13):(0.15-0.28):(0.0898-0.3995):(0.0002-0.0005).

[0010] When expanded graphite, aluminum powder, hydrogen-containing silane, methacrylic monomer, unsaturated silane, bis(2-ethylhexyl) maleate and initiator are compounded in the above dosage ratio, a better synergistic effect is achieved, so that the thermal conductive silicone obtains better elasticity, thermal conductivity and adhesion.

[0011] Preferably, the expanded graphite particle size is 200-325 mesh.

[0012] The expanded graphite is obtained by expanding nano-scale expandable graphite by 125-200 times, and the expanded graphite is obtained by screening through a 200-325 mesh sieve. Under the particle size, it has better thermal conductivity and softness. Therefore, when the composite material prepared by compounding hydrogen-containing silane, methacrylate monomer, unsaturated silane and bis(2-ethylhexyl) maleate is used to modify the surface of the expanded graphite and aluminum powder, the dispersibility and compatibility thereof are improved, and the surface modifier is further cross-linked with the raw rubber, so that the prepared thermal conductive silica gel has better elasticity, thermal conductivity and adhesion.

[0013] Preferably, the methacrylic monomer is one or more of trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate.

[0014] Trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate can all undergo self-polymerization and react with the silanol groups in silicone rubber to improve the flexibility, elasticity, and adhesion of silicone rubber. In addition, unsaturated silanes, hydrogen-containing silanes, and bis(2-ethylhexyl) maleate are combined to make the modified thermally conductive filler easily dispersed in silicone rubber and further cross-linked with silicone rubber, so that the obtained thermally conductive silicone has better wear resistance, flexibility, adhesion, elasticity, and thermal conductivity.

[0015] When trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate are compounded, a better synergistic effect is achieved, thereby improving the thermal conductivity, adhesion, and elasticity of the thermally conductive silicone.

[0016] Preferably, the unsaturated silane is 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and / or 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane.

[0017] 1,3-bis(3-methacryloyloxypropyl)tetrakis(trimethylsiloxy)disiloxane or 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane can be used as a crosslinking agent to improve the performance of thermally conductive silicone. At the same time, it has a better dispersing effect on inorganic substances, and then combined with hydrogen-containing silane, methacrylic monomers, and bis(2-ethylhexyl)maleate, the prepared modified thermally conductive filler can have better compatibility and can further cross-link with silicone rubber, so that the expanded graphite, aluminum powder and silicone rubber raw material system are closely combined, thereby making the thermally conductive silicone have better thermal conductivity, elasticity, flexibility and adhesion.

[0018] When 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane or 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane plays a better synergistic role, the thermal conductive silicone has better thermal conductivity, elasticity and adhesion.

[0019] Preferably, the hydrogen-containing silane is hydroxyalkyl double-terminated polydimethylsiloxane and / or double-terminated methacryloxypropyl polydimethylsiloxane.

[0020] Hydroxyl double-terminated polydimethylsiloxane and / or double-terminated methacryloxypropyl polydimethylsiloxane can further cross-link with the raw rubber, and can also be compounded with hydroxyl double-terminated polydimethylsiloxane and double-terminated methacryloxypropyl polydimethylsiloxane to play a synergistic role and further improve the performance of thermal conductive silicone.

[0021] Preferably, the raw rubber is one or more of α,ω dihydroxy polydimethyl diphenylsiloxane, vinyl-terminated dimethyl methyl vinyl, and cyclic dimethyl polysiloxane.

[0022] α, ω dihydroxy polydimethyl diphenylsiloxane, vinyl-terminated dimethyl methyl vinyl, and cyclic dimethyl polysiloxane have better flexibility, elasticity, and adhesion, and are further cross-linked with hydrogen-containing silane, methacrylic monomers, unsaturated silane, and bis (2-ethylhexyl) maleate, and are combined with expanded graphene and aluminum powder to make the prepared thermally conductive silicone have better thermal conductivity and elasticity.

[0023] In a second aspect, a method for preparing a thermally conductive silicone with high thermal conductivity and high elasticity is prepared by the following method: According to the weight percentage, methacrylic monomer and initiator are weighed and mixed, heated and reacted for 2-3 hours, and then hydrogen-containing silane, unsaturated silane, and bis(2-ethylhexyl) maleate are added and mixed evenly, and then expanded graphite is added and mixed evenly to obtain a modified thermal conductive filler; According to parts by weight, raw rubber, filler and modified thermal conductive filler are weighed and mixed evenly, heated and polycondensed to obtain a rubber mixture, and then a platinum vulcanizer is added to the rubber mixture and mixed evenly to obtain a thermal conductive silica gel.

[0024] The above process is simple to operate, and the thermally conductive silicone obtained has better elasticity and thermal conductivity. The thermally conductive silicone obtained in the present application has a rebound rate of 30-36% and a thermal conductivity of 4.3-7.1. When it is used to adhere to an aluminum plate, after vulcanization, its peeling force is 33-40.8 g / inch.

[0025] Thirdly, a thermally conductive silicone with high thermal conductivity and high elasticity is applied, which is rolled into a thermally conductive silicone piece, adhered to the surface of a carrier, and vulcanized to make the thermally conductive silicone piece stably adhere to the surface of the carrier.

[0026] In the above technical solution, the thermally conductive silicone is rolled into a thermally conductive silicone piece, which is convenient for being attached to the surface of a carrier. After vulcanization, the thermally conductive silicone piece is cross-linked and stably adhered to the surface of the carrier.

[0027] At present, the application process of thermal conductive silicone needs to be vulcanized into a sheet, and then attached to the heat dissipation device through double-sided tape, adhesive, etc. This process requires auxiliary bonding, which is relatively cumbersome, and it is difficult to control during the operation, and it is easy to misalign. This reduces the convenience of the application of thermal conductive silicone.

[0028] The high thermal conductivity and high elasticity thermal conductive silicone of the present application is not vulcanized during the production process, but is vulcanized after being adhered to the support during the application process, and after being cured, it is also stably adhered to the support. This saves the use of other materials to assist the adhesion process, simplifies the process, and improves the convenience of the application process.

[0029] For example, the thermal conductive silicone of the present application can be used in auxiliary parts of electronic products, such as support frames, brackets, radiators, etc. for computers, tablets, and mobile phones. It can be used in the contact positions between computers, mobile phones, and tablets to play a buffering role and assist in heat dissipation.

[0030] In summary, this application has the following beneficial effects: After self-polymerization of methacrylic monomers, further compounding with unsaturated silane, hydrogen-containing silane, and bis(2-ethylhexyl) maleate, the obtained compound can further improve the compatibility of aluminum powder and expanded graphite in raw rubber, and can further undergo cross-linking reaction with raw rubber, so that the obtained thermal conductive silica gel has better thermal conductivity, elasticity and adhesion. The silicone rubber has better elasticity during use, reduces the collision between parts, and has better heat dissipation. It is easy to adhere to the surface of metal and plastic, reduces the possibility of falling off, and provides installation stability. DETAILED DESCRIPTION

[0031] The present application is further described in detail below with reference to the embodiments.

[0032] Introduction of some raw materials; Table 1 Introduction of some raw materials Example

[0033] Example 1 The preparation of thermally conductive silicone with high thermal conductivity and high elasticity is prepared by the following method: According to the weight parts, 0.25kg of methacrylic monomer and 0.0005kg of initiator were weighed and put into a stirring device, mixed at a speed of 50r / min for 10min, heated to 65°C, reacted for 2h, and then 0.3kg of hydrogen-containing silane, 0.15kg of unsaturated silane, and 0.3995kg of bis(2-ethylhexyl)maleate were added, and stirring was continued for 10min to fully mix them to obtain a surface modifier, 3.5kg of expanded graphite and 3.0kg of graphite were added to the surface modifier, and stirred at a speed of 30r / min for 30min to fully mix them to obtain a modified thermally conductive filler; According to weight, 2.0 kg of raw rubber, 0.3 kg of filler and 7.6 kg of modified thermal conductive filler were weighed and put into a kneader, and the temperature was increased to 150 ° C at 5 ° C / min, and the reaction was carried out for 1 hour. The material was discharged and cooled to 40 ° C to obtain a mixed rubber; all the mixed rubbers were mixed on a double-roll rubber mixer, and 0.1 kg of platinum vulcanizer was added to all the mixed rubbers and mixed evenly to obtain thermal conductive silica gel.

[0034] The particle size of the expanded graphite is 325 meshes, the methacrylic monomer is tetrahydrofuran methacrylate; the unsaturated silane is 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane; the raw rubber is α, ω dihydroxy polydimethyldiphenylsiloxane; and the hydrogen-containing silane is hydroxyalkyl di-terminated polydimethylsiloxane.

[0035] Embodiment 2-5 The difference between Example 2-5 and Example 1 is that the amount of raw materials used is different as shown in Table 2; Table 2 Raw material dosage of Examples 1-5 (kg) Example 4 The difference between Example 4 and Example 2 is that the particle size of the expanded graphite is 300 meshes.

[0036] Example 5 The difference between Example 5 and Example 2 is that the particle size of the expanded graphite is 200 meshes.

[0037] Example 6 The difference between Example 6 and Example 2 is that the methacrylate monomer consists of trimethylolpropane triacrylate and tetrahydrofuran methacrylate in a weight ratio of 1:0.8.

[0038] Example 7 The difference between Example 7 and Example 2 is that the methacrylate monomer is composed of trimethylolpropane triacrylate and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate in a weight ratio of 1:0.8.

[0039] Example 8 The difference between Example 8 and Example 2 is that the methacrylate monomer is composed of trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate in a weight ratio of 1:0.4:0.4.

[0040] Example 9 The difference between Example 9 and Example 2 is that the methacrylate monomer is composed of trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate in a weight ratio of 5:5:8.

[0041] Example 10 The difference between Example 10 and Example 8 is that the unsaturated silane is 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane.

[0042] Embodiment 11 The difference between Example 11 and Example 8 is that the unsaturated silane is composed of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane in a weight ratio of 1:1.

[0043] Example 12 The difference between Example 12 and Example 8 is that the unsaturated silane is composed of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane in a weight ratio of 1:1.2.

[0044] Example 13 The difference between Example 13 and Example 8 is that the unsaturated silane is composed of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane in a weight ratio of 0.5:1.7.

[0045] Embodiment 14 The difference between Example 14 and Example 12 is that the hydrogen-containing silane is a dual-terminal methacryloxypropyl polydimethylsiloxane.

[0046] Embodiment 15 The difference between Example 15 and Example 12 is that the hydrogen-containing silane is composed of hydroxyalkyl double-terminated polydimethylsiloxane and double-terminated methacryloxypropyl polydimethylsiloxane in a weight ratio of 1:1.

[0047] Example 16 The difference between Example 16 and Example 12 is that the hydrogen-containing silane is composed of hydroxyalkyl double-terminated polydimethylsiloxane and double-terminated methacryloxypropyl polydimethylsiloxane in a weight ratio of 1:2.8.

[0048] Embodiment 17 The difference between Example 17 and Example 12 is that the hydrogen-containing silane is composed of hydroxyl bi-terminated polydimethylsiloxane and bi-terminated methacryloxypropyl polydimethylsiloxane in a weight ratio of 0.8:3.

[0049] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that an equal amount of methacrylic monomer is replaced by unsaturated silane.

[0050] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the unsaturated silane is replaced by an equal amount of methacrylic monomer.

[0051] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that an equal amount of bis(2-ethylhexyl)maleate is replaced by hydrogen-containing silane.

[0052] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that an equal amount of aluminum powder is replaced with hexagonal boron nitride having a particle size of 325 mesh.

[0053] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that the methacrylic monomer, unsaturated silane, bis(2-ethylhexyl)maleate, and initiator are replaced by hydrogen-containing silane in equal amounts.

[0054] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that the expanded graphite is replaced by aluminum powder in equal amount.

[0055] Comparative Example 7 The difference between Comparative Example 7 and Example 1 is that an equal amount of aluminum powder is replaced by expanded graphite.

[0056] Application Examples Application Example 1 An application of a thermally conductive silicone with high thermal conductivity and high elasticity. The thermally conductive silicone with high thermal conductivity and high elasticity obtained in Example 1 is calendered by a calender, and then die-cut by a die-cutting machine to form a thermally conductive silicone piece with a thickness of 1.5 mm, a width of 2 cm, and a length of 10 cm. The thermally conductive silicone piece is then adhered to the surface of an aluminum plate, and then the thermally conductive silicone piece on the aluminum plate is further vulcanized at 150°C for 5 minutes to make the thermally conductive silicone piece stably adhere to the surface of the aluminum plate, thereby obtaining an experimental sample.

[0057] Application Example 2-24 The difference between Application Example 2-24 and Example 1 is that the sources of the thermally conductive silicone with high thermal conductivity and high elasticity are different, as shown in Table 3: Table 3 The sources of high thermal conductivity and high elasticity thermal conductive silicone are different Application comparison Application Comparative Example 1 The difference between the comparative example 1 and the application example 1 is that: the application process is different The thermally conductive silicone obtained in Example 1 was calendered to form a sheet, and then further vulcanized at 150°C for 5 minutes, and demolded to obtain a thermally conductive silicone piece with a thickness of 1.5 mm, a width of 2 cm, and a length of 10 cm. The thermally conductive silicone piece was then adhered to the surface of the aluminum plate with double-sided tape so that the thermally conductive silicone piece was stably adhered to the surface of the aluminum plate to obtain an experimental sample.

[0058] Performance testing The thermally conductive silica gel obtained in Examples 1-17 and Comparative Examples 1-5 was subjected to the following tests.

[0059] Detection method / test method Test 1: The thermally conductive silica gel obtained in Examples 1-17 and Comparative Examples 1-5 was placed in a mold, and further vulcanized at 150° C. for 5 min. After demolding, various types of test samples were obtained; The test samples are then subjected to the following performance tests: Rebound rate: The test was conducted with reference to GB / T 1681-2009, and the thickness of the test sample was 5 mm.

[0060] Thermal conductivity: Tested according to ASTM D5470, with the thickness of the test sample being 3 mm.

[0061] The above experimental data are shown in Table 4. Table 4 Experimental data of Examples 1-17 and Comparative Examples 1-5 Experimental items Rebound rate (%) Thermal conductivity Example 1 30.1 5.8 Example 2 31.2 5.1 Example 3 32.3 4.3 Example 4 31.9 5.5 Example 5 31.5 5.4 Example 6 32.8 5.7 Example 7 32.3 5.8 Example 8 33.1 6.1 Example 9 32.9 6.1 Example 10 32.8 5.7 Embodiment 11 34.5 6.5 Example 12 34.8 6.8 Example 13 34.3 6.9 Embodiment 14 35.2 6.7 Embodiment 15 36.7 7.0 Example 16 36.9 7.1 Embodiment 17 36.4 7.0 Comparative Example 1 25.8 4.5 Comparative Example 2 23.6 4.3 Comparative Example 3 26.8 4.8 Comparative Example 4 16.8 3.9 Comparative Example 5 21.6 4.1 Comparative Example 6 20.7 7.5 Comparative Example 7 29.6 2.3 Combining Example 1 and Comparative Examples 1-7, and combining Table 4, it can be seen that the rebound rates of Comparative Examples 1-7 are all lower than 30%, the rebound rate of Example 1 is above 30%, and the thermal conductivity coefficients of Comparative Examples 1-5 and Comparative Example 7 are all below 5, indicating that the composite obtained by compounding methacrylic monomers, unsaturated silanes, bis(2-ethylhexyl) maleate, and initiators has better compatibility with expanded graphite and aluminum powder, promotes its mixing with the raw rubber system, and further cross-links with the raw rubber, so that the thermally conductive silicone has better elasticity and thermal conductivity after vulcanization. In Comparative Example 6, only aluminum powder is added, although it has a better thermal conductivity, but the elasticity is significantly reduced, and in Comparative Example 5, hexagonal boron nitride is used to replace aluminum powder, and its thermal conductivity and elasticity are reduced, indicating that the compounding of expanded graphite and aluminum powder has a better synergistic effect, thereby making the thermally conductive silicone better in elasticity and thermal conductivity after vulcanization.

[0062] By comparing Example 2 and Example 8 and combining with Table 4, it can be seen that the rebound rate of Example 8 is 3% higher than that of Example 2, and the thermal conductivity is also higher than that of Example 2, indicating that the compounding of trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate has a synergistic effect, thereby making the elasticity and thermal conductivity of the thermal conductive silicone after vulcanization better.

[0063] By comparing Example 8 and Example 12 and combining with Table 4, it can be seen that the rebound rate and thermal conductivity of Example 8 are lower than the rebound rate of Example 12, indicating that the compounding of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane has a synergistic effect, so that the thermally conductive silicone has better elasticity and thermal conductivity.

[0064] By comparing Example 12 and Example 16 and combining with Table 4, it can be seen that the rebound rate and thermal conductivity of Example 12 are lower than the rebound rate of Example 16, indicating that the compounding of hydroxyl double-terminated polydimethylsiloxane and double-terminated methacryloxypropyl polydimethylsiloxane has a synergistic effect, so that the thermal conductive silicone has better elasticity and thermal conductivity.

[0065] Test 2 (1) The experimental samples obtained from Application Examples 1-24 and Comparative Example 1 were placed in an environment with a humidity of 80% and a temperature of 120° C. for 7 days, and then observed to see if any shedding occurred. The experimental results were recorded.

[0066] (2) The experimental samples obtained in Application Examples 1-24 and Application Comparative Example 1 were tested with reference to JIS Z 0237 (300 mm / min, 180°) to obtain the peeling force of the thermally conductive silicone members of the experimental samples obtained in Application Examples 1-24 and Application Comparative Example 1.

[0067] The above specific data are shown in Table 5; Table 5 Application Examples 1-24 and Application Comparative Example 1 In combination with Example 1, Application Comparative Example 1, Application Examples 18-24 and Table 5, it can be seen that there is no shedding phenomenon in Example 1 and Application Comparative Example 1, and the peeling force is above 30g / inch, while Application Examples 18-24 are all below 30g / inch, indicating that the composite obtained by compounding methacrylic monomers, unsaturated silanes, bis(2-ethylhexyl) maleate and initiators described in this application has better compatibility with expanded graphite and aluminum powder, promotes mixing with the raw rubber system, and further cross-links with the raw rubber, so that the thermal conductive silicone has better elasticity, thermal conductivity and adhesion after vulcanization.

[0068] In addition, it can also be explained that the application method of the thermally conductive silicone of the present application can not only introduce the adhesive material, but also is simple to operate. After it is vulcanized, it can stably adhere to the aluminum plate to reduce the possibility of falling off. If the application method of the thermally conductive silicone of the present application is used, it is suitable for plastics, rubbers, metals and other carriers with a melting temperature above 150°C.

[0069] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A thermally conductive silicone with high thermal conductivity and high elasticity, It is characterized in that Made from the following raw materials in weight percentage: Raw rubber 20-50% Platinum vulcanizing agent 1-3% Filler 3-17% Modified thermal conductive filler 40-76%; The modified thermal conductive filler is prepared from expanded graphite, aluminum powder, hydrogen-containing silane, methacrylic monomer, unsaturated silane, bis(2-ethylhexyl) maleate and an initiator.

2. A thermally conductive silicone with high thermal conductivity and high elasticity according to claim 1, Features: The weight ratio of the expanded graphite, aluminum powder, hydrogen-containing silane, methacrylic monomer, unsaturated silane, bis(2-ethylhexyl)maleate, and initiator is (2.0-3.5): (0.3-0.5): (1-3): (0.25-0.13): (0.15-0.28): (0.0898-0.3995): (0.0002-0.0005).

3. A thermally conductive silicone with high thermal conductivity and high elasticity according to claim 1, Features: The expanded graphite particle size is 200-325 meshes.

4. The thermally conductive silicone with high thermal conductivity and high elasticity according to claim 1, Features: The methacrylic monomer is one or more of trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate.

5. A thermally conductive silicone with high thermal conductivity and high elasticity according to claim 4, Features: The weight ratio of trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate is 1:(0.4-1):(0.4-1.6).

6. The thermally conductive silicone with high thermal conductivity and high elasticity according to claim 1, Features: The unsaturated silane is 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and / or 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane.

7. The thermally conductive silicone with high thermal conductivity and high elasticity according to claim 1, Features: The hydrogen-containing silane is hydroxyalkyl double-terminated polydimethylsiloxane and / or double-terminated methacryloxypropyl polydimethylsiloxane.

8. The thermally conductive silicone with high thermal conductivity and high elasticity according to claim 1, Features: The raw rubber is one or more of α,ω dihydroxy polydimethyl diphenyl siloxane, vinyl-terminated dimethyl methyl vinyl, and cyclic dimethyl polysiloxane.

9. A method for preparing the thermally conductive silicone with high thermal conductivity and high elasticity as claimed in any one of claims 1 to 8, It is characterized in that Prepared by the following method: According to the weight percentage, methacrylic monomer and initiator are weighed and mixed, heated and reacted for 2-3 hours, and then hydrogen-containing silane, unsaturated silane, and bis(2-ethylhexyl)maleate are added and mixed evenly, and then expanded graphite and aluminum powder are added and mixed evenly to obtain a modified thermal conductive filler; According to weight parts, raw rubber, filler and modified thermal conductive filler are weighed and mixed evenly, reacted to obtain a mixed rubber, and then a platinum vulcanizing agent is added to the mixed rubber and mixed evenly to obtain a thermal conductive silica gel.

10. An application of a thermally conductive silicone with high thermal conductivity and high elasticity, wherein the thermally conductive silicone with high thermal conductivity and high elasticity as claimed in any one of claims 1 to 8 is rolled into a thermally conductive silicone piece, adhered to the surface of a carrier, and vulcanized to make the thermally conductive silicone piece stably adhered to the surface of the carrier.

Citation Information

Patent Citations

  • Polyacrylate modified expanded graphite as well as preparation method and application thereof

    CN109438760A

  • Low-filler high-thermal-conductivity flexible silicone rubber and preparation method thereof

    CN116904036A

  • Thermally conductive composition and a production method of a thermal conductive component using the composition

    WO2023194054A1