Coating with self-cleaning function and self-repairing effect and preparation method thereof

By introducing photocatalytic nanoarray modified nanometer microspheres on the surface of the hydrophobic substrate and performing surface fluorination, rapid self-cleaning and repair of ultra-double coatings is achieved, and pollution, low cleaning efficiency and self-repair in the prior art are solved. The problem of low efficiency has achieved environmentally friendly and low-cost coating recycling.

CN118931270AActive Publication Date: 2024-11-12SHANXI UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411093476.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing ultra-double coatings have contamination during long-term operation, low physical cleaning efficiency and high energy consumption, chemical pickling and alkaline washing will damage the coating, and the self-cleaning and self-repairing efficiency is not clear enough, making it difficult to achieve simple cleaning and Recycling.

Method used

By introducing photocatalytic nanoarray modified nanometer microspheres on the surface of hydrophobic substrates and constructing a super double-sparse coating through surface fluorination, ultra-double-sparse coating is achieved by induced self-cleaning with ultra-blipidity and restoring in the dark, rapid self-sparseness is achieved Clean and repair and reuse.

Benefits of technology

The super-double-sparing coating is achieved quickly self-cleaning and repairing. The coating changes from super-hydrophobic to super-hydrophilic within 30 minutes under ultraviolet light. The super-hydrophobic coating can be restored for 3-8 days of dark treatment, avoiding the dispersion of nanomaterials. The phenomenon of agglomeration reduces production costs and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931270A_ABST
    Figure CN118931270A_ABST
Patent Text Reader

Abstract

The invention discloses a coating with a self-cleaning function and a self-repairing effect and a preparation method of the coating, and belongs to the technical field of material surface treatment. Aiming at the problem of coating pollution in the technical field of current material surface treatment, the invention provides a preparation method of a coating with a self-cleaning function and a self-repairing effect. Nano microspheres modified by photocatalytic nano arrays are introduced to the surface of a hydrophobic base material through covalent bonds, and the super-amphiphobic coating is constructed through surface fluorination. The super-amphiphobic coating has excellent pollution resistance; meanwhile, a light-induced self-cleaning effect is achieved, the surface is converted into a super-hydrophilic state from a super-hydrophobic state within 30 minutes under ultraviolet irradiation, wetting switching and catalysis occur, and rapid self-cleaning is achieved; and meanwhile, the super-amphiphobic performance of the super-hydrophilic coating can be recovered after the super-hydrophilic coating is dried for 20-60 minutes or subjected to light-shielding treatment for 3-8 days, so that the coating is repaired and reused.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material surface treatment, and in particular relates to a coating with self-cleaning function and self-repairing effect and a preparation method thereof. Background Art

[0002] Inspired by the "lotus effect", constructing a superhydrophobic coating by constructing a micro / nanoscale rough structure on a low surface energy hydrophobic material and modifying a low surface energy substance on the surface of the micro / nano rough structure is an effective solution to the problem of coating contamination. The static contact angle of a superhydrophobic coating is usually greater than 150° and the rolling angle is less than 10°. This superhydrophobicity makes it difficult for liquid water and pollutants to interact with the coating surface. However, in actual applications, in addition to hydrophilic pollutants, the coating surface also needs to have a high repulsive force against low surface tension lipophilic substances such as surfactants, oils and ethanol. Therefore, a super-amphiphobic coating is further proposed. However, studies have shown that super-amphiphobic coatings can also be contaminated during long-term operation. Physical cleaning has low efficiency and high energy consumption, while chemical acid and alkali washing will damage the surface morphology, structure and function of the coating. Because the surface of the super-amphiphobic coating is highly liquid-repellent, the cleaning effect is often difficult to meet the standard. Therefore, achieving simple cleaning and recycling of super-amphiphobic coatings is still an urgent problem to be solved in engineering practice.

[0003] Photocatalytic coatings with adjustable wettability provide a good solution to the above problems. Photocatalysis can achieve self-cleaning of the coating without contact, leaving the coating surface intact. Photoresponsive wettability regulation can provide a good cleaning environment for highly liquid-repellent superamphiphobic coatings, allowing water flow to fully contact the catalyst and pollutants, shortening the diffusion distance of free radicals and flushing the catalytically degraded pollutants in a timely manner.

[0004] Patent CN 110183880 A discloses a photocatalytic super-amphiphobic coating and its preparation method and application. The specific process involves directly dispersing the photocatalytic nanomaterials in the spray solution, which is prone to uneven dispersion and agglomeration, thereby affecting the photocatalytic effect. Patent CN 109082230 B discloses a self-healing super-amphiphobic and photocatalytic dual self-cleaning coating and its preparation method, mainly by directly dispersing fluorinated cage-type silsesquioxane and photocatalytic particles in a fluorinated solvent for the preparation of a self-cleaning coating. In the embodiment, it is mentioned that the hydrophobicity of the coating surface is destroyed after being contaminated with oleic acid, and the hydrophobicity is restored after being irradiated with ultraviolet light, but the time required to achieve the self-cleaning effect is not specifically stated. At the same time, the description of the self-healing performance only mentions that the coating surface restores hydrophobicity after being placed at room temperature or appropriately heated, and no specific description is made about the specific self-cleaning and self-healing efficiency. Patent CN 103409028 A discloses a photocatalytic self-healing super-hydrophobic coating and a preparation method thereof. Hydrophobic nanoparticles and photocatalytic nanoparticles are directly dispersed in the coating and sprayed to obtain a super-hydrophobic coating. After the coating surface is worn, it takes 190 hours to recover to the super-hydrophobic state. This excessively long repair time affects the protective effect of the coating.

[0005] Although there have been studies on photocatalytic self-cleaning, self-repairing and super-amphiphobic coatings in recent years, there are currently the following problems with such coatings: 1) Hydrophobic nanoparticles and photocatalytic nanoparticles are directly dispersed in the matrix material by physical means, which are prone to agglomeration and affect other properties of the material; 2) Photocatalytic nanoparticles are distributed inside the coating. While the photocatalytic effect removes surface organic pollutants, it also causes the gradual degradation of low surface energy substances that play a role in super-hydrophobic properties, thereby causing a decrease in super-hydrophobic properties; 3) The time required for the self-cleaning and self-repairing process of super-amphiphobic coatings is not clear enough, and the efficiency of self-cleaning and self-repairing needs to be further improved. At present, the above problems have not been well solved in the existing research work on self-cleaning and self-repairing super-amphiphobic coatings. Summary of the invention

[0006] In order to solve the coating pollution problem in the current material surface treatment technology field, the present invention provides a method for preparing a coating with self-cleaning function and self-repairing effect, wherein nano-microspheres modified with photocatalytic nano-arrays are introduced on the surface of a hydrophobic substrate by covalent bonds, and a super-amphiphobic coating is constructed by surface fluorination; the super-amphiphobic coating has excellent anti-pollution properties; at the same time, it has light-induced self-cleaning effect, and wetting switching and catalysis occur under ultraviolet light irradiation to achieve rapid self-cleaning; and the super-amphiphobic property can be restored by standing in the dark, thereby achieving repair and reuse of the coating.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions: A coating with self-cleaning and self-repairing effects, in which nano-microspheres modified with photocatalytic nano-arrays are introduced on the surface of a hydrophobic substrate through covalent bonds, and a super-amphiphobic coating is constructed through surface fluorination. The super-amphiphobic coating has excellent anti-pollution properties; it also has light-induced self-cleaning properties, and wetting switching and catalysis occur under ultraviolet light irradiation, achieving rapid self-cleaning; and the super-amphiphobic properties can be restored by standing in the dark, achieving repair and reuse of the coating.

[0008] The photocatalytic nanoarray-modified nanospheres are nanoarrays of nanomaterials with photocatalytic properties that grow vertically on the surface of the nanospheres; The nanoarray of the nanomaterial with photocatalytic properties has an average length of about 2-10 μm and presents a nanoflower morphology; The nanospheres modified by the photocatalytic nanoarray form a NRs layer on the surface of the hydrophobic substrate, and the thickness of the layer is 10-20 μm.

[0009] A method for preparing a coating with self-cleaning function and self-repairing effect: preparing a photocatalytic nanocrystal seed layer by a sol-gel method, then calcining and hydrothermal reaction, and vacuum drying to obtain nano-microspheres modified with a photocatalytic nano-array; introducing hydroxyl bridging groups into a hydrophobic substrate by alkali etching to complete substrate surface pretreatment; utilizing the dehydration condensation between a silane coupling agent and the hydroxyl groups on the surface of the hydrophobic substrate to introduce the nano-microspheres modified with the photocatalytic nano-array into the surface of the hydrophobic substrate through chemical bonds to obtain a composite material; and utilizing fluorinated siloxane to complete the surface fluorination of the composite coating by dehydration condensation to obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect.

[0010] Further, the method specifically includes the following steps: Step 1, preparing nanospheres modified with photocatalytic nanoarrays: dispersing the nanospheres into a nanomaterial precursor solution having photocatalytic properties, mixing evenly by magnetic stirring, collecting by filtration, washing with water and an organic solvent for multiple times, and drying to obtain a photocatalytic nanocrystal seed layer; calcining the photocatalytic nanocrystal seed layer, and then preparing nanospheres modified with photocatalytic nanoarrays by hydrothermal reaction; Step 2, using an alkaline solution to alkali-etch the hydrophobic substrate to introduce a hydroxyl bridging group, and then rinsing with deionized water for standby use; Step 3, prepare a super-amphiphobic composite coating: add the nano-microspheres modified by the photocatalytic nano-array to a mixed solution of ethanol, silane coupling agent and glacial acetic acid, disperse them evenly by ultrasonication, and graft the mixed solution to the surface of the pre-treated hydrophobic substrate by vacuum filtration; after the composite coating is fully dried, completely immerse the coating in a fluorosilicone-ethanol solution, and complete the fluorination of the coating surface by dehydration condensation. Then rinse the excess fluorosilicone with ethanol, dry it naturally at room temperature, and finally obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect.

[0011] Furthermore, the nano-microspheres in step 1 are any one or more of silicon dioxide particles, calcium oxide particles, carbon black particles, calcium carbonate particles, polytetrafluoroethylene particles, polystyrene microspheres, polypropylene microspheres, and polyvinyl alcohol microspheres; the nano-materials with photocatalytic properties in step 1 are any one or more of titanium dioxide, zinc oxide, ferric oxide, cuprous oxide, tungsten trioxide, tin oxide, zirconium dioxide, cadmium sulfide, and zinc sulfide.

[0012] Furthermore, in the step 1, the mass ratio of the nanospheres to the nanomaterial precursor solution with photocatalytic properties is 1: 5-20, and the mass fraction of the nanomaterial precursor solution with photocatalytic properties is 10-50%; the calcination temperature in the step 1 is 400°C-700°C, and the calcination time is 2-4 h; the temperature of the hydrothermal reaction in the step 1 is 100°C-200°C, and the reaction time is 4 h-10 h.

[0013] Furthermore, the alkaline solution in step 2 is any one or more of potassium hydroxide, sodium hydroxide, calcium hydroxide, and barium hydroxide aqueous solutions, and the concentration of the alkaline solution is 5 mol / L-10 mol / L; the hydrophobic substrate in step 2 is any one of polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl chloride, polypropylene, polyether sulfone, polycarbonate, polyamide, and polyacrylonitrile.

[0014] Furthermore, the general structural formula of the silane coupling agent in step 3 is YR-Si(OX)3, wherein Y is vinyl, amino, epoxy, methacryloxy, thiol or urea, R is alkyl or aryl, and X is methoxy, ethoxy, methoxyethoxy or acetoxy.

[0015] Furthermore, in the step 3, the volume fraction of the silane coupling agent in the mixed solvent of ethanol, silane coupling agent and glacial acetic acid is 1%-6%; the volume fraction of the fluorinated silicone in the fluorinated silicone-ethanol solution in the step 3 is 5%-20%, and the fluorination time is 2 h-10 h.

[0016] Furthermore, the fluorinated siloxane in step 3 is heptadecafluorodecyltrimethylsiloxane, tridecafluorooctyltriethoxysilane, nonafluorohexyltriethoxysilane, or trifluoropropyltrimethylsiloxane.

[0017] Compared with the prior art, the present invention has the following advantages: 1) The present invention uses conventional raw materials such as nano-microspheres, nano-materials with photocatalytic properties, silane coupling agents, fluorinated silanes, and hydrophobic substrates to prepare a coating with self-cleaning and self-repairing effects. It does not contain any toxic organic solvents, does not cause any harm to the human body and the environment, meets environmental protection requirements, and reduces production costs; 2) First, the nanomaterials with photocatalytic properties are grown on the surface of nanospheres in an array form, and then combined with the hydrophobic substrate through chemical bonds, avoiding uneven dispersion and agglomeration of the nanomaterials; 3) The super-amphiphobic composite coating has excellent self-cleaning and self-repairing effects. The surface of the coating changes from super-hydrophobic to super-hydrophilic within 30 minutes under ultraviolet light irradiation, and can achieve self-cleaning. At the same time, the super-hydrophilic coating can be restored to super-hydrophobicity after 3-8 days of dark treatment, achieving repair and regeneration. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The surface and cross-sectional SEM images of the nano-SiO2 microspheres modified with the photocatalytic TiO2 nanoarrays prepared in Example 1; Figure 2 The surface and cross-sectional SEM images of the super-amphiphobic composite coating 17F-STNRs / PVDF prepared in Example 1; Figure 3 (a) Fourier transform infrared spectrum of the super-amphiphobic composite coating 17F-STNRs / PVDF and the original PVDF coating prepared in Example 1; (b) full spectrum of X-ray photoelectron energy spectrum; (c) Si2p high-resolution spectrum; Figure 4 The wettability of different liquids to the super-amphiphobic composite coating 17F-STNRs / PVDF prepared in Example 1; Figure 5 This is the photocatalytic self-cleaning process of the super-amphiphobic composite coating 17F-STNRs / PVD prepared in Example 1.

[0019] Figure 6 The repeatability of the photoresponsive wettability switching of the super-amphiphobic composite coating 17F-STNRs / PVD prepared in Example 1. DETAILED DESCRIPTION

[0020] In order to gain a deeper understanding of the present invention, we will provide a comprehensive and detailed description of the present invention. However, the present invention has multiple implementations and is not limited to the specific examples listed herein. The presentation of these examples is intended to deepen the comprehensive understanding of the disclosure of the present invention.

[0021] Example 1

[0022] 1) Disperse 1 g of silica powder into 10 g of a 20 wt% titanium dioxide precursor solution, stir magnetically for 30 minutes to mix evenly, collect by filtration, wash with ethanol and water several times, and dry to obtain a titanium dioxide seed layer. The titanium dioxide seed layer was calcined at 600 °C in a muffle furnace for 2 hours, and then hydrothermally reacted at 150 °C for 6 hours to prepare photocatalytic titanium dioxide nanoarray-modified silica nanospheres, denoted as STNRs.

[0023] Scanning electron microscopy revealed that vertically grown titanium dioxide nanoarrays were formed on the surface of the silicon dioxide nanospheres. The average length of the titanium dioxide nanoarrays was about 3 μm and the diameter was about 25 nm, showing a nanoflower morphology. Figure 1 shown.

[0024] 2) using 6 mol / L sodium hydroxide solution to alkaline-etch the polyvinylidene fluoride (PVDF) hydrophobic coating to introduce hydroxyl bridging groups, and then rinsing with deionized water for later use; 3) Add the STNRs material to a mixed solution of ethanol, aminopropyltriethoxysilane (KH550) and glacial acetic acid, with a volume fraction of KH550 of 2%, and ultrasonically disperse for 30 minutes. The mixed solution is grafted onto the pretreated hydrophobic PVDF coating surface by vacuum filtration. After the composite coating is fully dried, the coating is completely immersed in a perfluorodecyltriethoxysilane (17F)-ethanol solution with a volume fraction of 17F of 12%. The reaction is carried out at room temperature for 7 hours to complete the fluorination of the coating surface. Then, the excess 17F is rinsed with ethanol and naturally air-dried at room temperature to finally obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect, which is recorded as 17F-STNRs / PVDF. The structure and performance are compared with the PVDF substrate.

[0025] The surface and cross-sectional morphology of 17F-STNRs / PVDF coating were observed by scanning electron microscopy. Figure 2 As shown, STNRs are evenly distributed on the coating surface, and the thickness of the STNRs layer is observed to be about 12.38 μm in the cross-sectional view.

[0026] The chemical structure of 17F-STNRs / PVDF composite coating was characterized by Fourier transform infrared spectroscopy (FTIR) and X-ray photoelectron spectroscopy (XPS). Figure 3As shown, new characteristic absorption peaks corresponding to Si-OC and Ti-O-Si appeared in the FTIR spectrum, and Ti-O-Si groups appeared at 101.4 eV in the XPS spectrum, indicating that STNRs were connected to KH550 and the hydroxylated PVDF coating through covalent bonds; The 17F-STNRs / PVDF composite coating exhibits super hydrophobicity and oleophobicity, with contact angles of 153.91±2.07° and 153.07±2.18° for water and ethylene glycol, respectively, and its ultra-low surface energy has high wettability to a variety of liquids (such as water, ethylene glycol, milk, humic acid, sodium dodecyl sulfate, etc.), such as Figure 4 shown.

[0027] The 17F-STNRs / PVDF composite coating exhibits photocatalytic self-cleaning properties. Figure 5 As shown in the figure, the coating surface contaminated by humic acid was restored to cleanliness after being exposed to ultraviolet light for 2 hours.

[0028] The 17F-STNRs / PVDF composite coating exhibits self-healing properties. Figure 6 As shown, the coating can be converted from a highly hydrophobic interface of 155.49° to a super hydrophilic interface under ultraviolet light in 30 minutes. The modified coating is then dried and self-repaired after 60 minutes. The contact angles of water and ethylene glycol in the air on its surface can be restored to more than 150°. This reversible wettability switching can be repeated at least five times.

[0029] Example 2

[0030] 1) Disperse 1 g of calcium oxide powder into 15 g of a 15 wt% titanium dioxide precursor solution, stir magnetically for 30 minutes to mix evenly, collect by filtration, wash with ethanol and water several times, and dry to obtain a titanium dioxide seed layer. The titanium dioxide seed layer was calcined at 500 °C in a muffle furnace for 3 hours, and then subjected to a hydrothermal reaction at 180 °C for 5 hours to prepare calcium oxide nanospheres modified with photocatalytic titanium dioxide nanoarrays, denoted as CTNRs. Vertically grown titanium dioxide nanoarrays were formed on the surface of the calcium oxide nanospheres, with an average length of about 5 μm, showing a nanoflower morphology.

[0031] 2) using 5 mol / L sodium hydroxide solution to alkaline-etch the polytetrafluoroethylene (PTFE) hydrophobic coating to introduce hydroxyl bridging groups, and then rinsing with deionized water for later use; 3) Add the CTNRs material to a mixed solution of ethanol, vinyl triethoxysilane and glacial acetic acid, with a volume fraction of 4% vinyl triethoxysilane, and ultrasonically disperse for 40 minutes. The mixed solution is grafted onto the pre-treated hydrophobic PFTE coating surface by vacuum filtration. After the composite coating is fully dried, the coating is completely immersed in a tridecafluorooctyl triethoxysilane (13F)-ethanol solution with a volume fraction of 8% 13F. The reaction is performed at room temperature for 8 hours to complete the fluorination of the coating surface. Then, the excess 13F is rinsed with ethanol and naturally air-dried at room temperature to finally obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect, which is recorded as 13F-CTNRs / PTFE. The thickness of CTNRs in the 13F-CTNRs / PTFE super-amphiphobic composite coating is 15 μm.

[0032] Example 3

[0033] 1) Disperse 1 g of silica powder into 5 g of 40 wt% zinc oxide precursor solution, stir magnetically for 30 minutes to mix evenly, collect by filtration, wash with acetone and water several times, and dry to obtain a zinc oxide seed layer. The zinc oxide seed layer was calcined at 700 °C in a muffle furnace for 2 hours, and then hydrothermally reacted at 140 °C for 7 hours to prepare silica nanospheres modified with photocatalytic zinc oxide nanoarrays, denoted as SZnNRs. Vertically grown zinc oxide nanoarrays were formed on the surface of the silica nanospheres, and the average length of the zinc oxide nanoarrays was about 7 μm.

[0034] 2) using 5 mol / L potassium hydroxide solution to alkaline-etch the polypropylene (PP) hydrophobic coating to introduce hydroxyl bridging groups, and then rinsing with deionized water for later use; 3) The SZnNRs material was added to a mixed solution of ethanol, methacryloxypropyltrimethoxysilane and glacial acetic acid, with a volume fraction of 2.5% of methacryloxypropyltrimethoxysilane, and ultrasonically dispersed for 35 minutes. The mixed solution was grafted onto the pretreated hydrophobic PP coating surface by vacuum filtration. After the composite coating was fully dried, the coating was completely immersed in a nonafluorohexyltriethoxysilane (9F)-ethanol solution with a volume fraction of 5% of 9F, and reacted at room temperature for 5 hours to complete the fluorination of the coating surface. Then, the excess 9F was rinsed with ethanol and naturally air-dried at room temperature to finally obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect, which was recorded as 9F-SZnNRs / PP. The thickness of SZnNRs in the 9F-SZnNRs / PP super-amphiphobic composite coating was 17 μm.

[0035] Example 4

[0036] 1) Disperse 1 g of carbon black powder into 18 g of 12 wt% tin oxide precursor solution, stir magnetically for 30 minutes to mix evenly, collect by filtration, wash with ethanol and water several times, and dry to obtain a tin oxide seed layer. The tin oxide seed layer was calcined at 400 °C in a muffle furnace for 4 hours, and then hydrothermally reacted at 100 °C for 10 hours to prepare carbon black nanospheres modified with photocatalytic tin oxide nanoarrays, denoted as CSnNRs. Vertically grown tin oxide nanoarrays were formed on the surface of the carbon black nanospheres, and the average length of the tin oxide nanoarrays was about 10 μm.

[0037] 2) using 8 mol / L calcium hydroxide solution to alkaline-etch the polyamide (PA) hydrophobic coating to introduce hydroxyl bridging groups, and then rinsing with deionized water for later use; 3) The CSnNRs material was added to a mixed solution of ethanol, vinyl tri(β-methoxyethoxy) silane and glacial acetic acid, with a volume fraction of 5% vinyl tri(β-methoxyethoxy) silane, and ultrasonically dispersed for 50 minutes. The mixed solution was grafted onto the pretreated hydrophobic PA coating surface by vacuum filtration. After the composite coating was fully dried, the coating was completely immersed in a tridecafluorooctyl triethoxysilane (13F)-ethanol solution with a volume fraction of 15%. The reaction was performed at room temperature for 8 hours to complete the fluorination of the coating surface. The excess 13F was then rinsed with ethanol and naturally air-dried at room temperature to finally obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect, which was recorded as 13F-CSnNRs / PA. The thickness of CSnNRs in the 13F-CSnNRs / PA super-amphiphobic composite coating was 20 μm.

[0038] Example 5

[0039] 1) Disperse 1 g of polystyrene microspheres into 20 g of a 10 wt% zinc sulfide precursor solution, stir magnetically for 30 minutes to mix evenly, collect by filtration, wash with acetone and water several times, and dry to obtain a zinc sulfide seed layer. The zinc sulfide seed layer was calcined at 650 °C in a muffle furnace for 2 hours, and then hydrothermally reacted at 120 °C for 9 hours to prepare polystyrene microsphere nanospheres modified with photocatalytic zinc sulfide nanoarrays, denoted as PZnNRs. Vertically grown zinc sulfide nanoarrays were formed on the surface of the polystyrene nanospheres, and the average length of the zinc sulfide nanoarrays was about 3 μm.

[0040] 2) using 9 mol / L sodium hydroxide solution to alkaline-etch the polyethersulfone (PES) hydrophobic coating to introduce hydroxyl bridging groups, and then rinsing with deionized water for later use; 3) PZnNRs material was added to a mixed solution of ethanol, aminopropyltriethoxysilane and glacial acetic acid, with a volume fraction of 6% aminopropyltriethoxysilane, and ultrasonically dispersed for 40 minutes. The mixed solution was grafted onto the pretreated hydrophobic PES coating surface by vacuum filtration. After the composite coating was fully dried, the coating was completely immersed in a perfluorodecyltriethoxysilane (17F)-ethanol solution with a volume fraction of 17F of 20%, and reacted at room temperature for 10 hours to complete the fluorination of the coating surface. Then, the excess 17F was rinsed with ethanol and naturally air-dried at room temperature to finally obtain a super-amphiphobic composite coating with self-cleaning function and self-repairing effect, which was recorded as 17F-PZnNRs / PES. The thickness of PZnNRs in the 17F-PZnNRs / PES super-amphiphobic composite coating was 13 μm.

[0041] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

Claims

1. A coating with self-cleaning and self-repairing effects, Features: Nanospheres modified with photocatalytic nanoarrays are introduced onto the surface of a hydrophobic substrate via covalent bonds, and a super-amphiphobic coating is constructed by surface fluorination.

2. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 1, Features: The photocatalytic nanoarray-modified nanospheres are nanoarrays of nanomaterials with photocatalytic properties that grow vertically on the surface of the nanospheres; The nanoarray of the nanomaterial with photocatalytic properties has an average length of about 2-10 μm and presents a nanoflower morphology; The nanospheres modified by the photocatalytic nanoarray form a NRs layer on the surface of the hydrophobic substrate, and the thickness of the layer is 10-20 μm.

3. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 2, Features: A photocatalytic nanocrystalline seed layer is prepared by a sol-gel method, and then calcined and hydrothermally reacted, and then vacuum dried to obtain nanospheres modified with photocatalytic nanoarrays; a hydrophobic substrate is introduced with hydroxyl bridging groups by alkaline etching to complete the surface pretreatment of the substrate; By utilizing the dehydration condensation between the silane coupling agent and the hydroxyl groups on the surface of the hydrophobic substrate, the nano-microspheres modified with the photocatalytic nano-array are introduced to the surface of the hydrophobic substrate through chemical bonds to obtain a composite material; Fluorine-containing siloxane is then used to complete the surface fluorination of the composite coating through dehydration condensation to obtain a super-amphiphobic composite coating with self-cleaning and self-repairing effects.

4. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, It is characterized in that The following steps are involved: Step 1, preparing nanospheres modified with photocatalytic nanoarrays: dispersing the nanospheres into a nanomaterial precursor solution having photocatalytic properties, mixing evenly by magnetic stirring, collecting by filtration, washing with water and an organic solvent for multiple times, and drying to obtain a photocatalytic nanocrystal seed layer; calcining the photocatalytic nanocrystal seed layer, and then preparing nanospheres modified with photocatalytic nanoarrays by hydrothermal reaction; Step 2, using an alkaline solution to alkali-etch the hydrophobic substrate to introduce a hydroxyl bridging group, and then rinsing with deionized water for standby use; Step 3, preparing a super-amphiphobic composite coating: adding the nanospheres modified with the photocatalytic nanoarray into a mixed solution of ethanol, a silane coupling agent and glacial acetic acid, uniformly dispersing by ultrasonication, and grafting the mixed solution onto the pretreated hydrophobic substrate surface by vacuum filtration; After the composite coating is fully dried, the coating is completely immersed in a fluorinated silicone-ethanol solution to complete the fluorination of the coating surface through dehydration condensation. The excess fluorinated silicone is then rinsed with ethanol and naturally air-dried at room temperature to finally obtain a super-amphiphobic composite coating with self-cleaning and self-repairing effects.

5. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, Features: The nano-microspheres in step 1 are any one or more of silicon dioxide particles, calcium oxide particles, carbon black particles, calcium carbonate particles, polytetrafluoroethylene particles, polystyrene microspheres, polypropylene microspheres, and polyvinyl alcohol microspheres; the nano-materials with photocatalytic properties in step 1 are any one or more of titanium dioxide, zinc oxide, ferric oxide, cuprous oxide, tungsten trioxide, tin oxide, zirconium dioxide, cadmium sulfide, and zinc sulfide.

6. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, Features: In the step 1, the mass ratio of the nanospheres to the nanomaterial precursor solution with photocatalytic properties is 1:5-20, and the mass fraction of the nanomaterial precursor solution with photocatalytic properties is 10-50%; the calcination temperature in the step 1 is 400°C-700°C, and the calcination time is 2 h-4 h; the temperature of the hydrothermal reaction in the step 1 is 100°C-200°C, and the reaction time is 4 h-10 h.

7. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, Features: The alkaline solution in step 2 is any one or more of potassium hydroxide, sodium hydroxide, calcium hydroxide, and barium hydroxide aqueous solutions, and the concentration of the alkaline solution is 5 mol / L-10 mol / L; the hydrophobic substrate in step 2 is any one of polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl chloride, polypropylene, polyether sulfone, polycarbonate, polyamide, and polyacrylonitrile.

8. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, Features: The general structural formula of the silane coupling agent in step 3 is YR-Si(OX) 3 , wherein Y is vinyl, amino, epoxy, methacryloxy, mercapto or urea, R is alkyl or aryl, and X is methoxy, ethoxy, methoxyethoxy or acetoxy.

9. The method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, Features: In the step 3, the volume fraction of the silane coupling agent in the mixed solvent of ethanol, silane coupling agent and glacial acetic acid is 1%-6%; the volume fraction of the fluorinated silicone in the fluorinated silicone-ethanol solution in the step 3 is 5%-20%, and the fluorination time is 2h-10h.

10. A method for preparing a coating having self-cleaning function and self-repairing effect according to claim 3, Features: The fluorine-containing siloxane in step 3 is heptadecafluorodecyltrimethylsiloxane, tridecafluorooctyltriethoxysilane, nonafluorohexyltriethoxysilane, or trifluoropropyltrimethylsiloxane.

Citation Information

Patent Citations

  • Photocatalytic type self-repairing super-hydrophobic coating and preparation method thereof

    CN103409028A

  • A self-healing superhydrophobic and photocatalytic dual self-cleaning coating and its preparation method

    CN109082230B

  • Photocatalysis super-amphiphobic coating as well as preparation method and application thereof

    CN110183880A

  • Hierarchical micro-nanostructure omentum based light-operated oil-water separator and its application method

    CN102380230A

  • Preparation method of nano-structure oil-water separation net membrane with self-cleaning and underwater super-oleophobic characteristics

    CN105641973A