Low-melting-point high-temperature molten salt heat transfer and storage medium and preparation method thereof
By using KNO3-NaNO3 to add K2CO3 to form multi-eutectic salts in solar thermal power generation technology, the problem of insufficient decomposition temperature and melting point of Solar salt and Hitec salt is solved, and efficient energy storage density and safety are achieved, suitable for higher Supercritical generator sets at temperatures and reduce energy storage costs.
Patent Information
- Application Number
- CN202411413710.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing solar thermal power generation technology, the decomposition temperature of Solar salt and Hitec salt is low and the melting point is high, resulting in the phenomenon of "freezing pipe" easily condensation in circulation pipelines, which increases the cost of heat storage and heat transfer and reduces the efficiency of energy storage. And it cannot meet the needs of supercritical generator sets with higher temperature requirements.
Using a low-melting point, high-temperature molten salt heat transfer heat storage medium, by adding K2CO3 to KNO3-NaNO3, a multi-eutectic salt is formed, which increases its decomposition temperature and specific heat capacity, and reduces the melting point. The preparation method includes drying, mixing, melting, Cooling and pulverizing and drying to form a low-melting point high-temperature molten salt heat transfer heat storage medium with a particle size of 20 to 200 mesh.
The decomposition temperature is increased to 730℃ and the melting point is reduced to 140℃, which significantly reduces the risk of 'freezing tube' and improves the efficiency and safety of the power generation system. It is suitable for supercritical generator sets at higher temperatures and reduces energy storage costs. , and the decomposition of nitrate is significantly inhibited by adding potassium carbonate, extending the service life of the medium.
Smart Images

Figure CN118931506A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar thermal power generation, and in particular to a low-melting-point high-temperature molten salt heat transfer and storage medium and a preparation method thereof. Background Art
[0002] At present, the decomposition temperature of Solar salt and Hitec salt is relatively low, but the main steam and re-steam temperature of the unit needs to reach 600℃ or above.
[0003] To solve this problem, different types of molten salts are usually added to make mixed molten salts in the prior art. For example, in patent CN108003845B, KNO2 is added to KNO3-NaNO3-NaNO2, and the melting point of the mixed molten salt is between 146.4°C and 198.4°C, and the decomposition temperature is between 601.8°C and 658.1°C. In patent CN113831899A, NaNO2 in KNO3-NaNO3-NaNO2 is changed to K2CO3, the decomposition temperature reaches 715.4°C, the melting point is about 313°C, and the average specific heat is about 1.236 J / (g·K). The decomposition temperature of the above-mentioned mixed molten salt is increased, but the melting point is not significantly lower than that of Solar salt and Hitec salt.
[0004] In the molten salt heat storage system, the high melting point of molten salt makes it easy to condense in the circulation pipes and cause the "frozen pipe" phenomenon. For normal operation, the pipes need to be insulated and continuously heated, which increases the cost of heat storage and heat transfer, resulting in reduced energy storage benefits.
[0005] Therefore, there is an urgent need for a mixed molten salt with high decomposition temperature and low melting point to solve the above problems. Summary of the invention
[0006] In view of the defects in the prior art, the purpose of the present invention is to provide a low-melting-point high-temperature molten salt heat transfer and storage medium, which has a high decomposition temperature and high specific heat capacity, and also has a low melting point characteristic. The material can reduce the risk of molten salt "frozen pipes" in industrial energy storage and improve energy storage efficiency, and its high decomposition temperature can be suitable for supercritical power generation units with higher temperature requirements; in addition, the present invention also provides a preparation method of the above-mentioned low-melting-point high-temperature molten salt heat transfer and storage medium.
[0007] A first aspect of the present invention provides a low melting point high temperature molten salt heat transfer and storage medium, wherein the low melting point high temperature molten salt heat transfer and storage medium comprises the following single component salts in weight percentage: KNO3 55~63wt.%, NaNO2 20~26wt.% or 43wt.%, and K2CO3 2~19wt.%.
[0008] In one embodiment, the low melting point high temperature molten salt heat transfer and heat storage medium includes the following single component salt components in weight percentage: KNO3 59wt.%, NaNO2 23wt.%, K2CO3 18wt.%.
[0009] In one embodiment, the low melting point high temperature molten salt heat transfer and storage medium includes the following components in weight percentage: KNO3 55wt.%, NaNO2 43wt.%, and K2CO3 2wt.%.
[0010] The second aspect of the present invention provides a method for preparing the above-mentioned low melting point high temperature molten salt heat transfer and heat storage medium, comprising the following steps: S1, drying the single-component salt raw materials respectively; S2, weighing the single-component salts in the formula, mixing them evenly to obtain a solid mixed molten salt, and placing the solid mixed molten salt in a muffle furnace to melt to obtain a molten salt; S3, cooling the molten salt to room temperature, crushing and / or grinding it into molten salt powder, and drying it to obtain a low melting point and high temperature molten salt heat transfer and heat storage medium.
[0011] In one embodiment, the temperature rising program of the muffle furnace in step S2 is as follows: from room temperature to 110°C, keep constant temperature for 12 hours, from 110°C to 320°C, keep constant temperature for 12 hours, from 320°C to 500°C, keep constant temperature for 12 hours, and the temperature rising rate of the muffle furnace is set to 5~15°C / min.
[0012] In one embodiment, in step S3, the particle size of the molten salt powder is 20-200 mesh.
[0013] Compared with the prior art, the embodiments of the present invention have the following beneficial effects: 1. The low-melting-point high-temperature molten salt heat transfer and storage medium provided by the present invention is a multi-element eutectic salt made of no precious metal salts. It shows significant advantages in wide temperature range, high heat storage density, high decomposition temperature, low melting point and high specific heat capacity. It can effectively improve the efficiency and safety of the power generation system and reduce the energy storage cost.
[0014] 2. The low-melting-point high-temperature molten salt heat transfer and storage medium provided by the present invention has an average decomposition temperature of 730°C. Compared with Solar salt (565°C) and Hitec salt (535°C), it can be applied to supercritical power generation units with higher temperature requirements, molten salt heat pump energy storage, and thermal power flexibility transformation, which helps to reduce energy storage costs and improve the efficiency of power generation systems.
[0015] 3. The low melting point and high temperature molten salt heat transfer and heat storage medium provided by the present invention has a low melting point, with an average melting point of 140°C, which is significantly lower than that of patent CN113831899B (KNO3-NaNO2-K2CO3, melting point 313°C, specific heat capacity 1.236J / (g·K)), which can effectively reduce the risk of molten salt "frozen pipe" in the power generation system. Thereby increasing the stability of safe operation of the power generation system.
[0016] 4. The low melting point and high temperature molten salt heat transfer and storage medium provided by the present invention has an average specific heat capacity of 1.9 J / (g·K) in liquid state. Compared with patent CN113831899B (KNO3-NaNO2-K2CO3, melting point 313°C, specific heat capacity 1.236 J / (g·K)), the energy storage density is improved, which further reduces the energy storage cost.
[0017] 5. The low melting point and high temperature molten salt heat transfer and storage medium provided by the present invention can significantly improve the deterioration of nitrate molten salt. As a high temperature heat storage medium, the thermal stability of nitrate molten salt will deteriorate after long-term use. - 3. Easy to thermally decompose and deteriorate. Through the improvement measures of introducing carbonates in the present invention, the Raman spectrum research results of the mixed molten salt show that the addition of carbonate components can significantly inhibit the decomposition of nitrates. In particular, by adding potassium carbonate, not only the thermal decomposition of nitrates is greatly reduced, but also the oxidation reaction of nitrites is significantly reduced. This optimization greatly improves the chemical stability of molten salts in long-term use, slows down and prevents their decomposition and deterioration, thereby extending their service life and performance retention period.
[0018] 6. The low-melting-point high-temperature molten salt heat transfer and heat storage medium provided by the present invention can improve the energy storage density of the molten salt. The density of the molten salt will continue to decrease with the increase of temperature, and the addition of potassium carbonate in different mass ratios can increase the density of the molten salt. The unit volume of molten salt can store more heat, which helps to reduce the container cost and improve the energy storage efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings: Figure 1 This is the DSC curve of the high stability multi-element eutectic molten salt in Example 5 of the present invention; Figure 2 TG curve of the high stability multi-element eutectic molten salt in Example 5 of the present invention; Figure 3 The specific heat curve of the liquid phase of the high-stability multi-element eutectic molten salt in Example 5 of the present invention; Figure 4 The DSC curve of the high-stability multi-element eutectic molten salt in Comparative Example 1 of the present invention; Figure 5 TG curve of the high stability multi-element eutectic molten salt in Comparative Example 1 of the present invention; Figure 6 This is the specific heat curve of the liquid phase of the high-stability multi-element eutectic molten salt in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0020] The following examples will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0021] In this application, the inventors proposed a low melting point and high temperature molten salt heat transfer and storage medium. The decomposition temperature of a single component molten salt is low, and its decomposition temperature can be increased by mixing multiple molten salts to form a eutectic molten salt. The present invention increases its decomposition temperature by adding potassium carbonate with a higher melting point to a two-component nitrate formula. Finally, a eutectic mixed molten salt with a low melting point and a high decomposition temperature is screened out through parallel experiments.
[0022] The present invention is described in detail below with reference to specific embodiments.
[0023] Example 1 This embodiment provides a low melting point and high temperature molten salt heat transfer and heat storage medium. The composition and content of the single component salt are shown in Table 1.
[0024] Table 1 Example 1-Example 5 and Comparative Examples 1-7
[0025] This embodiment also provides a method for preparing the above-mentioned low melting point high temperature molten salt heat transfer and heat storage medium, comprising the following steps: S1. Place each single-component salt raw material in an oven at 120° C. for drying for 48 hours; S2. Weigh the above-mentioned dried single-component salt in the formula amount, mix them evenly to obtain a solid mixed molten salt, and place the solid mixed molten salt in a muffle furnace to melt to obtain a molten salt; the heating program of the muffle furnace is as follows: from room temperature to 110°C, constant temperature for 12h, from 110°C to 320°C, constant temperature for 12h, from 320°C to 500°C, constant temperature for 12h, and the heating rate of the muffle furnace is set to 5-15°C / min; S3, taking the molten salt out of the muffle furnace and crushing it into 100 mesh molten salt powder by a pulverizer; S4. Put the molten salt powder into an evaporating dish and place it in a drying oven at 110°C for 24 hours to obtain a low melting point and high temperature molten salt heat transfer and storage medium; wherein the drying oven temperature program is set at 110~130°C, and the constant temperature drying time is greater than 48 hours.
[0026] Example 2 This embodiment provides a low melting point high temperature molten salt heat transfer and storage medium. The composition and content of the single component salt are shown in Table 1. The preparation method of the low melting point high temperature molten salt heat transfer and storage medium provided in this embodiment is the same as that in Example 1.
[0027] Example 3 This embodiment provides a low melting point high temperature molten salt heat transfer and storage medium. The composition and content of the single component salt are shown in Table 1. The preparation method of the low melting point high temperature molten salt heat transfer and storage medium provided in this embodiment is the same as that in Example 1.
[0028] This embodiment provides a low melting point high temperature molten salt heat transfer and storage medium. The composition and content of the single component salt are shown in Table 1. The preparation method of the low melting point high temperature molten salt heat transfer and storage medium provided in this embodiment is the same as that in Example 1.
[0029] Example 5 This embodiment provides a low melting point high temperature molten salt heat transfer and storage medium. The composition and content of the single component salt are shown in Table 1. The preparation method of the low melting point high temperature molten salt heat transfer and storage medium provided in this embodiment is the same as that in Example 1.
[0030] Comparative Example 1 This comparative example provides a mixed molten salt heat transfer and heat storage medium, and the composition and content of the single component salt are shown in Table 1. The preparation method of the mixed molten salt heat transfer and heat storage medium provided in this comparative example is the same as that of Example 1.
[0031] Comparative Example 2 This comparative example provides a mixed molten salt heat transfer and heat storage medium, and the composition and content of the single component salt are shown in Table 1. The preparation method of the mixed molten salt heat transfer and heat storage medium provided in this comparative example is the same as that of Example 1.
[0032] Comparative Example 3 This comparative example provides a mixed molten salt heat transfer and heat storage medium, and the composition and content of the single component salt are shown in Table 1. The preparation method of the mixed molten salt heat transfer and heat storage medium provided in this comparative example is the same as that of Example 1.
[0033] Comparative Example 4 This comparative example provides a mixed molten salt heat transfer and heat storage medium, and the composition and content of the single component salt are shown in Table 1. The preparation method of the mixed molten salt heat transfer and heat storage medium provided in this comparative example is the same as that of Example 1.
[0034] Comparative Example 5 This comparative example provides a mixed molten salt heat transfer and heat storage medium, and the composition and content of the single component salt are shown in Table 1. The preparation method of the mixed molten salt heat transfer and heat storage medium provided in this comparative example is the same as that of Example 1.
[0035] Comparative Example 6 This comparative example provides a mixed molten salt heat transfer and heat storage medium, and the composition and content of the single component salt are shown in Table 1. The preparation method of the mixed molten salt heat transfer and heat storage medium provided in this comparative example is the same as that of Example 1.
[0036] Comparative Example 7 This comparative example provides a mixed molten salt, which contains 52.25wt% potassium nitrate, 42.75wt% sodium nitrite, and 5wt% potassium carbonate.
[0037] The mixed molten salt in this comparative example is prepared by the following steps: Weigh the formula amount of the above-mentioned dried single-component salt, mix them evenly, and place them in a muffle furnace and heat them to 450°C for 12 hours to completely melt the mixture and mix them evenly; after the mixed molten salt is cooled, take the molten salt out of the muffle furnace and crush it into 100-mesh molten salt powder with a pulverizer.
[0038] Experimental example In this experimental example, the physical properties of the molten salt heat transfer and heat storage medium obtained in Examples 1-5 and Comparative Examples 1-7 were tested, and the melting point of the mixed molten salt was tested using a differential scanning calorimeter (DSC). The specific test temperature procedure is: from room temperature to 100 ° C, constant temperature for 10 minutes, continue to heat up to 400 ° C, constant temperature for 10 minutes, cool to 90 ° C, constant temperature for 10 minutes, the heating and cooling rates are both 10K / min, repeat the test 3 times, and the second and third test values shall prevail. The specific heat capacity of the mixed molten salt is also tested using a differential scanning calorimeter (DSC), detected by the sapphire method, and the specific heat capacity is calculated by the specific heat comparison method. The specific temperature procedure is: room temperature rises to 500 ° C, constant temperature for 10 minutes. The decomposition temperature of the molten salt is measured using a synchronous thermal analyzer (TG-DSC), and the intersection of the baseline and the tangent of the inflection point of the loss-of-weight curve is used as the thermal decomposition temperature.
[0039] The present invention is further described below in conjunction with the test results. The melting points, specific heat capacities, and decomposition temperatures of the above-mentioned Examples 1-5 and Comparative Examples 1-7 are listed in Table 2: Table 2 Examples 1-5 and Comparative Examples 1-7 serial number Melting point(℃) Decomposition temperature(℃) Specific heat (J / g∙K) Is it eutectic? Example 1 141.1 688.9 1.65 yes Example 2 141.2 696.0 1.67 yes Example 3 141.0 682.8 1.65 yes Example 4 140.5 703.7 1.72 yes Example 5 140.5 733.1 1.94 yes Comparative Example 1 225.5 655.5 1.60 yes Comparative Example 2 318.2 679.7 1.55 no Comparative Example 3 225.3 703.5 1.49 yes Comparative Example 4 213.5 586.3 1.51 yes Comparative Example 5 290.0 565.0 1.44 yes Comparative Example 6 200.0 535.0 1.54 yes Comparative Example 7 137.7 659.2 1.23 yes In the present invention, the low-melting-point high-temperature molten salt heat transfer and storage medium obtained in Example 4 has a melting point of 140.5°C and a specific heat of 1.72 (J / g∙K) as tested by DSC (differential scanning calorimetry), and a decomposition temperature of 703.7°C as tested by TG (thermogravimetric analysis). Compared with Solar salt and Hitec salt, the decomposition temperature is increased by nearly 138°C, and the melting point is reduced by about 60°C; the low-melting-point high-temperature molten salt heat transfer and storage medium obtained in Example 5 has a melting point of 140.5°C and a specific heat of 1.94 (J / g∙K) as tested by DSC (differential scanning calorimetry), and a decomposition temperature of 733.1°C as tested by TG (thermogravimetric analysis). Compared with Solar salt and Hitec salt, the decomposition temperature is increased by nearly 138°C, and the melting point is reduced by about 60°C. Figure 1 Shown is the DSC curve of Example 5, Figure 2 Shown is the TG curve of Example 5, Figure 3 is the specific heat test curve of Example 5, In the present invention, the low melting point and high temperature molten salt heat transfer and heat storage medium obtained in Comparative Example 1 has a melting point of 264.3°C and a specific heat of 1.52 (J / g∙K) as tested by DSC (differential scanning calorimetry), and a decomposition temperature of 646.2°C as tested by TG (thermogravimetric analysis). Figure 4 Shown is the DSC curve of Comparative Example 1, Figure 5 Shown is the TG curve of Comparative Example 1, Figure 6 This is the specific heat test curve of comparative example 1. Compared with Solar salt and Hitec salt, the decomposition temperature is increased by nearly 80°C, and the melting point is reduced by about 30°C.
[0040] In the present invention, the addition of a certain amount of K2CO3 can significantly increase the decomposition temperature of the molten salt, and can effectively reduce the melting point while adjusting the ratio. It can be seen from the data of the above embodiments and comparative examples that the decomposition temperature is significantly increased when the addition amount of K2CO3 is 2~19wt.%, but a small amount of K2CO3 addition cannot increase the decomposition temperature, and when the addition amount of K2CO3 exceeds 18wt.%, the effect of increasing the decomposition temperature decreases. In addition, the mass ratio of KNO3 has a greater impact on the melting point. When the ratio of KNO3 is in the range of 55~63wt.%, the melting point is greatly reduced and stabilized at about 140°C. When the ratio of KNO3 is less than 55wt.%, the melting point cannot be effectively reduced.
[0041] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A low melting point high temperature molten salt heat transfer and heat storage medium, characterized in that: The low melting point high temperature molten salt heat transfer and heat storage medium includes the following single component salts in weight percentage: KNO3 55-63wt.%, NaNO2 20-26wt.% or 43wt.%, K2CO3 2-19wt.%.
2. The low melting point and high temperature molten salt heat transfer and storage medium according to claim 1, characterized in that: The low melting point high temperature molten salt heat transfer and heat storage medium includes the following single component salt components in weight percentage: KNO3 59wt.%, NaNO2 23wt.%, K2CO3 18wt.%.
3. The low melting point and high temperature molten salt heat transfer and storage medium according to claim 1, characterized in that: The low melting point high temperature molten salt heat transfer and heat storage medium includes the following components in weight percentage: KNO3 55wt.%, NaNO2 43wt.%, K2CO3 2wt.%.
4. A method for preparing the low melting point high temperature molten salt heat transfer and storage medium according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, drying the single-component salt raw materials separately; S2, weighing the single-component salts in the formula, mixing them evenly to obtain a solid mixed molten salt, and placing the solid mixed molten salt in a muffle furnace to melt to obtain a molten salt; S3. Cool the molten salt to room temperature, crush and / or grind it into molten salt powder, and dry it to obtain a low melting point and high temperature molten salt heat transfer and storage medium.
5. The method for preparing the low melting point high temperature molten salt heat transfer and storage medium according to claim 4, characterized in that: The temperature rise program of the muffle furnace in step S2 is as follows: from room temperature to 110°C, keep constant temperature for 12h, from 110°C to 320°C, keep constant temperature for 12h, from 320°C to 500°C, keep constant temperature for 12h, and the temperature rise rate of the muffle furnace is set to 5~15°C / min.
6. The method for preparing the low melting point high temperature molten salt heat transfer and heat storage medium according to claim 4, characterized in that: In step S3, the particle size of the molten salt powder is 20-200 mesh.
Citation Information
Patent Citations
A ternary nitrate molten salt and its preparation method
CN108003845B
High-decomposition-temperature mixed molten salt heat transfer and storage medium
CN113831899A
High decomposition temperature mixed molten salt heat transfer and storage medium
CN113831899B
Mixed molten salt as heat transfer and storage medium low in melting point
CN103074040A
Quartz sand compound binary molten nitrate salt heat transfer and storage medium and its preparation method
CN103923612A