Low-silicon vanadium liquid and preparation method thereof
By preparing hydroxypropyl methylcellulose and tetraacetylethylenediamine solutions to treat vanadium containing liquid, the colloid precipitation is formed, and the problem of silicon removal in alkaline and acidic vanadium liquid is solved, achieving high-efficiency and low-energy-consuming silicon removal effect , guarantees product purity and economic benefits.
Patent Information
- Application Number
- CN202411143127.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to efficiently remove silicon impurities in alkaline and acidic vanadium-containing liquids at the same time, and it is often necessary to adjust pH and high temperature conditions, complex operations, affecting product purity and economic benefits.
By preparing hydroxypropyl methylcellulose and tetraacetylethylenediamine solutions, the vanadium containing silicon is treated without adjusting the pH value and the temperature conditions are not high, forming micelle precipitation, significantly improving the silicon removal effect, ensuring product purity and mass, reduce vanadium loss.
Simplify the operation process, reduce energy consumption, improve silicon removal efficiency, ensure product purity and economic benefits, and are suitable for vanadium-containing liquids of different properties, reducing resource waste.
Smart Images

Figure CN118932192A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vanadium chemical industry, and in particular to a low-silicon vanadium liquid and a preparation method thereof. Background Art
[0002] Vanadium slag is mainly produced in the process of smelting vanadium-containing pig iron in the comprehensive utilization of vanadium-titanium magnetite. There are currently two main industrial applications for extracting vanadium from vanadium slag: sodium method and calcium method.
[0003] In the vanadium slag sodium method of vanadium extraction, the vanadium slag is roasted with sodium salt, soaked in water, and then sodium vanadium liquid is obtained. The vanadium liquid generally contains silicon, and the silicon content is high. During the precipitation process, it will enter the product and affect the quality. Therefore, the sodium vanadium liquid needs to be desiliconized.
[0004] In the vanadium slag calcium method of vanadium extraction, the vanadium slag is roasted with calcium salt and leached with sulfuric acid to obtain a calcified acid leaching vanadium liquid. The vanadium liquid generally contains silicon. Silicon is generally not removed during the precipitation process, and vanadium is directly precipitated. The silicon in the vanadium liquid will affect the vanadium precipitation rate. Silicon removal is required when preparing high-purity products.
[0005] At present, aluminum sulfate is generally used to remove silicon from alkaline vanadium liquid, and ammonium magnesium method is generally used for high-efficiency silicon removal; silicon removal from acidic vanadium liquid is more troublesome. Currently, there are patents showing that polycarboxylic acid polymers containing carboxylic acid groups, sulfonic acid groups and polyoxyethylene side chains can remove silicon from vanadium liquid with a content of less than 1g / L and a pH value of less than 5, with a silicon removal rate of more than 92%.
[0006] In the literature of "Experimental Study on Direct Preparation of High-purity V2O5 from Vanadium-rich Solution", the ammonium magnesium phosphate method was used to purify vanadium-rich solution to remove silicon and phosphorus, and the effects of factors such as the amount of impurity remover, temperature, pH value, ammonium-magnesium ratio, and reaction time on the impurity removal rate were investigated. The results show that the optimal purification and impurity removal conditions are: 8 mL of 200 g / L ammonium chloride solution was added to 100 mL of vanadium-rich solution, and ammonium chloride was added at an ammonium-magnesium ratio of 1.4. The original solution (pH≈10.2) was directly used for stirring and purification at room temperature for 30 min and then filtered to obtain the purified solution. The phosphorus removal rate reached more than 96%, the silicon removal rate reached 87%, and the vanadium loss rate could be controlled at about 2%. After vanadium precipitation, filtration, washing, drying, and calcination, high-purity vanadium pentoxide with a purity of 99.93% was obtained. Verified by repeatability tests, this process is stable and reliable, the process is simple, and the production cost is low, which can provide a technical solution for the preparation of high-purity V2O5.
[0007] For example, a Chinese patent application numbered 201510155152.3 discloses a method and application for removing silicon from a vanadium-containing silicon solution, the method comprising: contacting the vanadium-containing silicon solution with a silicon removal agent and filtering after co-precipitation under a pH value of less than 5; wherein the silicon removal agent comprises a polycarboxylic acid polymer containing carboxylic acid groups, sulfonic acid groups and polyoxyethylene side chains; the amount of the polycarboxylic acid polymer is 0.2-4 g relative to 1 g of silicon element contained in the vanadium-containing silicon solution calculated as silicon dioxide; the method enables the silicon removal rate of the vanadium-containing silicon solution to be more than 92% and the vanadium loss rate to be less than 0.25%; the contact conditions include: a temperature of 20-100°C and a time of 15-60 min.
[0008] The above patent is only applicable to alkaline silicon-vanadium liquid. The silicon remover generally adopts the ammonium magnesium method combined with the silicon removal method or the silicon remover in the acidic silicon-vanadium liquid contains a polycarboxylic acid polymer containing carboxylic acid groups, sulfonic acid groups and polyoxyethylene side chains.
[0009] Therefore, there is an urgent need for a method for removing silicon from silicon-containing vanadium liquid that can be used for both alkaline silicon-containing vanadium liquid and acidic silicon-containing vanadium liquid. In view of this, improvements should be made to the existing technology. Summary of the invention
[0010] The main purpose of the present invention is to provide a low-silicon vanadium liquid and a preparation method thereof. The silicon in the silicon-containing vanadium liquid is treated by preparing a hydroxypropyl methylcellulose solution and a tetraacetylethylenediamine solution. There is no need to adjust the pH value, the operation process is simplified, the temperature condition requirement is not high, the silicon removal effect is significant, the purity and quality of the product are guaranteed, the vanadium loss is small, the waste of resources is reduced, and the economic benefit is improved.
[0011] According to one aspect of the present invention, a method for preparing low-silicon vanadium liquid is provided, which comprises the following steps: S1, weighing hydroxypropyl methylcellulose and dissolving it in water to prepare a first solution, weighing tetraacetylethylenediamine and dissolving it in hot water to prepare a second solution; S2, measuring the silicon-vanadium liquid, adding the second solution to the silicon-vanadium liquid and stirring for t1, then adding the first solution and stirring for t2; S3, heating to T1 and stirring t3; Keep warm under conditions of S4 and T2, stop stirring, age for t4 and filter to obtain low-silicon vanadium liquid.
[0012] According to one embodiment of the present invention, the concentration range of the first solution is 5-10 g / L, and the concentration range of the second solution is 50-100 g / L.
[0013] According to an embodiment of the present invention, the temperature range of the hot water is 90-95°C.
[0014] According to one embodiment of the present invention, the silicon-vanadium liquid is an alkaline silicon-vanadium liquid and / or an acidic silicon-vanadium liquid, and the silicon content in the silicon-vanadium liquid is 0.2-3 g / L, and the vanadium content is 0.2-50 g / L.
[0015] According to one embodiment of the present invention, in step S2, the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium-containing solution is in the range of 20-30:1.
[0016] According to one embodiment of the present invention, in step S2, the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium liquid is in the range of 1 to 3:100.
[0017] According to an embodiment of the present invention, the range of t1 is 10 to 20 minutes, and the range of t2 is 10 to 20 minutes.
[0018] According to an embodiment of the present invention, the range of T1 is 45-60° C., and the range of t3 is 20-30 minutes.
[0019] According to an embodiment of the present invention, the range of T2 is 45-50° C., and the range of t4 is 30-60 minutes.
[0020] According to another aspect of the present invention, a low-silicon vanadium liquid is provided, which is prepared by using any of the above technical solutions. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 A process flow chart of a method for preparing low-silicon vanadium liquid according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION
[0023] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
[0024] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.
[0025] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0026] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.
[0027] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.
[0028] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and equipment should be considered part of the specification.
[0029] like Figure 1 As shown, the present invention provides a method for preparing low-silicon vanadium liquid, which comprises the following steps: S1, weighing hydroxypropyl methylcellulose and dissolving it in water to prepare a first solution, weighing tetraacetylethylenediamine and dissolving it in hot water to prepare a second solution; S2, measuring the silicon-vanadium liquid, adding the second solution to the silicon-vanadium liquid and stirring for t1, then adding the first solution and stirring for t2; S3, heating to T1 and stirring t3; Keep warm under conditions of S4 and T2, stop stirring, age for t4 and filter to obtain low-silicon vanadium liquid.
[0030] In the preparation method of low-silicon vanadium liquid according to an embodiment of the present invention, the silicon in the silicon-containing vanadium liquid is treated by preparing a hydroxypropyl methylcellulose solution and a tetraacetylethylenediamine solution, without adjusting the pH value, simplifying the operation process, and not requiring high temperature conditions. The silicon removal effect is significant, the purity and quality of the product are guaranteed, the vanadium loss is small, the waste of resources is reduced, and the economic benefits are improved.
[0031] Among them, tetraacetylethylenediamine releases hydrogen ions in the solution, forms micelles with silicon and then combines with cellulose to form colloidal precipitation. If the order of adding the first solution and the second solution is changed, the effect is not good, the part formed by cellulose is precipitated, and the colloidal particles formed by tetraacetylethylenediamine are very small, and the suspension is difficult to settle.
[0032] Setting T1 to 45-60°C is conducive to tetraacetylethylenediamine releasing hydrogen ions in the solution, which is conducive to reacting with silicon to form micelles; setting T2 to 45-50°C is conducive to cellulose adsorbing micelles to the surroundings and then settling together. This temperature does not destroy the overall molecular structure of hydroxypropyl methylcellulose and helps to maintain good performance.
[0033] Hydroxypropyl methylcellulose has good thickening and stability, and can form a viscous colloid in the solution, which helps to suspend and disperse solid particles, including silicon particles. In the process of silicon removal, if silicon exists in the form of suspended particles, hydroxypropyl methylcellulose helps to stabilize the dispersion of these particles, thus facilitating subsequent processing or separation.
[0034] In the complex silicon removal process, tetraacetylethylenediamine helps to maintain the stability of the process system and avoid the negative impact of interactions between different components on the silicon removal effect.
[0035] Tetraacetylethylenediamine releases hydrogen ions in the solution and reacts with silicon to form micelles. Hydroxypropyl methylcellulose plays a role in suspension polymerization. During the suspension polymerization process, it is first reflected in the presence of a large number of hydroxyl and methyl functional groups in its molecular structure. These functional groups can interact with hydrogen bonds or other interaction forces in the silica gel group to form an adsorption layer. After the silica gel group is adsorbed, the mass becomes larger and the sedimentation rate is accelerated, making it easy to precipitate the silica gel.
[0036] Silicon-vanadium liquid includes acidic vanadium liquid leached from calcified clinker with sulfuric acid or silicon-vanadium liquid leached from sodium clinker. Silicon in both silicon-vanadium liquids can be removed by the method of this patent.
[0037] The silicon content in the low-silicon vanadium liquid in the present application is ≤0.012 g / L.
[0038] Within a certain range, increasing the concentration of the reaction solution can increase the collision frequency and reaction rate between the reactants, thereby improving the desiliconization efficiency. A high concentration of the reaction solution generally means a faster reaction rate, so the reaction time required to achieve the desired desiliconization effect can be shortened. This is of great significance for improving production efficiency and reducing costs. In some specific embodiments, the concentration range of the first solution is 5-10 g / L, and the concentration range of the second solution is 50-100 g / L.
[0039] In some specific embodiments, the temperature of the hot water ranges from 90 to 95°C. Increasing the water temperature can significantly accelerate the chemical reaction rate during the desiliconization process. This is because as the temperature increases, the movement speed of the reactant molecules increases, the collision frequency increases, and thus the reaction rate increases. Hot water also helps to enhance the activity of the desiliconizer, making it easier to react with the silicon-containing vanadium liquid. Hot water can also appropriately shorten the reaction time.
[0040] On the basis of the above embodiments, the silicon-vanadium liquid is an alkaline silicon-vanadium liquid and / or an acidic silicon-vanadium liquid, and the silicon content in the silicon-vanadium liquid is 0.2~3g / L, and the vanadium content is 0.2~50g / L. Since vanadium slag or vanadium-containing raw materials from different sources may produce silicon-vanadium liquids with different pH values during the leaching process, the method of the present application can deal with these liquids of different properties respectively, without the need for additional pH adjustment of the raw materials, thereby simplifying the process flow. Through the optimized silicon removal method and conditions of the present application, the generation and emission of waste can be reduced, and pollution to the environment can be reduced.
[0041] Reasonable reaction step time setting can ensure that the desiliconizer fully reacts with the silicon in the solution, thereby improving the desiliconization efficiency. Too short a reaction time may lead to incomplete desiliconization, while too long a reaction time may increase energy consumption and costs. By accurately controlling the reaction step time, the entire desiliconization process can be optimized.
[0042] In some specific embodiments, in step S2, the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium-containing solution is in the range of 20-30:1.
[0043] Based on the above embodiment, in step S2, the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium-containing liquid is in the range of 1 to 3:100.
[0044] Based on the above embodiment, the range of t1 is 10 to 20 minutes, and the range of t2 is 10 to 20 minutes.
[0045] Based on the above embodiment, the range of T1 is 45-60° C., and the range of t3 is 20-30 minutes.
[0046] Based on the above embodiment, the range of T2 is 45-50° C., and the range of t4 is 30-60 minutes.
[0047] The scheme of the present application is described below through specific examples and comparative examples.
[0048] Table 1 Main components of silicon-vanadium liquid (g / L) Table 2 Main components of desiliconization liquid after desiliconization application g / L V <![CDATA[Na + ]]> <![CDATA[SO4 2- ]]> Si Mn Mg Low silicon vanadium liquid 1 44.95 38.55 1.23 0.012 <0.01 <0.01 Low silicon vanadium liquid 2 27.98 1.35 28.68 0.013 8.75 1.23 Low silicon vanadium liquid 3 44.96 38.54 1.22 0.008 <0.01 <0.01 Low silicon vanadium liquid 4 27.98 1.35 28.67 0.009 8.65 1.22 Low silicon vanadium liquid 5 44.98 38.53 1.21 0.005 <0.01 <0.01 Low silicon vanadium liquid 6 27.97 1.34 28.67 0.004 8.65 1.13 Example 1 When adding alkaline silicon-vanadium liquid: First, hydroxypropyl methylcellulose and water are prepared into a first solution with a concentration of 5 g / L; then tetraacetylethylenediamine and 90°C hot water are weighed to prepare a second solution with a concentration of 50 g / L; 100 mL of the alkaline silicon-vanadium liquid in Table 1 is measured, and the second solution is first added according to the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium liquid of 20:1, and stirred for 10 minutes; then the first solution is added according to the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium liquid of 1:100, and stirred for 10 minutes; then the temperature is raised to 45°C, and stirring is continued for 20 minutes; the temperature is kept at 45°C, stirring is stopped, aging is carried out for 30 minutes, and filtering is carried out to obtain low silicon vanadium liquid 1. The contents of each component in the low silicon vanadium liquid 1 are shown in Table 2.
[0049] When adding acidic silicon-vanadium liquid: First, hydroxypropyl methylcellulose and water are prepared into a first solution with a concentration of 5 g / L; then tetraacetylethylenediamine and 90°C hot water are weighed to prepare a second solution with a concentration of 50 g / L; 100 mL of the acidic silicon-vanadium liquid in Table 1 is measured, and the second solution is first added according to the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium liquid of 20:1, and stirred for 10 minutes; then the first solution is added according to the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium liquid of 1:100, and stirred for 10 minutes; then the temperature is raised to 45°C, and stirring is continued for 20 minutes; the temperature is kept at 45°C, stirring is stopped, aging is carried out for 30 minutes, and filtering is carried out to obtain low silicon vanadium liquid 2. The contents of each component in the low silicon vanadium liquid 2 are shown in Table 2.
[0050] Example 2 When adding alkaline silicon-vanadium liquid: First, hydroxypropyl methylcellulose and water were prepared into a first solution with a concentration of 8 g / L; then, tetraacetylethylenediamine and 92°C hot water were weighed to prepare a second solution with a concentration of 80 g / L; 500 mL of the alkaline silicon-vanadium liquid in Table 1 were measured, and the second solution was first added according to the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium liquid of 25:1, and stirred for 15 minutes; then, the first solution was added according to the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium liquid of 2:100, and stirred for 15 minutes; then, the temperature was raised to 50°C, and stirring was continued for 25 minutes; the temperature was kept at 47°C, stirring was stopped, and the solution was aged for 40 minutes, and filtered to obtain low silicon vanadium liquid 3. The contents of each component in the low silicon vanadium liquid 3 are shown in Table 2.
[0051] When adding acidic silicon-vanadium liquid: First, hydroxypropyl methylcellulose and water are prepared into a first solution with a concentration of 8 g / L; then tetraacetylethylenediamine and 92°C hot water are weighed to prepare a second solution with a concentration of 80 g / L; 500 mL of the acidic silicon-vanadium liquid in Table 1 are measured, and the second solution is first added according to the ratio of the volume of the second solution (mL) to the silicon content (g) in the silicon-vanadium liquid of 25:1, and stirred for 15 minutes; then the first solution is added according to the ratio of the volume of the first solution (mL) to the volume of the silicon-vanadium liquid (mL) of 2:100, and stirred for 15 minutes; then the temperature is raised to 50°C, and stirring is continued for 25 minutes; the temperature is kept at 47°C, stirring is stopped, aging is carried out for 40 minutes, and filtering is carried out to obtain low silicon vanadium liquid 4. The contents of each component in low silicon vanadium liquid 4 are shown in Table 2.
[0052] Example 3 When adding alkaline silicon-vanadium liquid: First, hydroxypropyl methylcellulose and water are prepared into a first solution with a concentration of 10 g / L; then tetraacetylethylenediamine and 95°C hot water are weighed to prepare a second solution with a concentration of 100 g / L; 2000 mL of the alkaline silicon-vanadium liquid in Table 1 is measured, and the second solution is first added according to the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium liquid of 30:1, and stirred for 20 minutes; then the first solution is added according to the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium liquid of 3:100, and stirred for 20 minutes; then the temperature is raised to 60°C, and stirring is continued for 30 minutes; the temperature is kept at 50°C, stirring is stopped, and the mixture is aged for 60 minutes, and filtered to obtain low silicon vanadium liquid 5. The contents of each component in the low silicon vanadium liquid 5 are shown in Table 2.
[0053] When adding acidic silicon-vanadium liquid: First, hydroxypropyl methylcellulose and water are prepared into a first solution with a concentration of 10 g / L; then tetraacetylethylenediamine and 95°C hot water are weighed to prepare a second solution with a concentration of 100 g / L; 2000 mL of the acidic silicon-vanadium liquid in Table 1 is measured, and the second solution is first added according to the ratio of the volume of the second solution (mL) to the silicon content (g) in the silicon-vanadium liquid of 30:1, and stirred for 20 minutes; then the first solution is added according to the ratio of the volume of the first solution (mL) to the volume of the silicon-vanadium liquid (mL) of 3:100, and stirred for 20 minutes; then the temperature is raised to 60°C, and stirring is continued for 30 minutes; the temperature is kept at 50°C, stirring is stopped, and the temperature is aged for 60 minutes, and low silicon vanadium liquid 6 is obtained by filtering. The contents of each component in the low silicon vanadium liquid 6 are shown in Table 2.
[0054] After the implementation of the present invention, at least the following beneficial effects are achieved: (1) No need to tediously adjust the pH value to a precise range. Operators can save the steps of frequently monitoring and adjusting the pH value, which not only simplifies the operation process, but also significantly reduces the risk of side reactions or reduced efficiency caused by pH fluctuations, thereby ensuring the stability and reliability of the entire process.
[0055] (2) It also shows great tolerance in temperature control, that is, the temperature does not need to reach a very high level to achieve efficient operation. This feature is of great significance for saving energy and reducing production costs. Under high temperature conditions, additional energy input is often required to maintain the reaction temperature, while this process can be effectively carried out within a relatively low and easier to control temperature range, reducing energy consumption and avoiding material degradation or safety hazards that may be caused by high temperature.
[0056] (3) Silicon impurities can be efficiently separated from the target substance, ensuring the purity and quality of the product, and the process has minimal loss of valuable elements such as vanadium. This means that during the purification or purification process, the useful components in the raw materials can be retained to the maximum extent, reducing resource waste and improving economic benefits. This high efficiency and environmentally friendly feature makes the process have broad application prospects and important economic value in related fields.
[0057] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0058] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for preparing low-silicon vanadium liquid, characterized in that: The following steps are involved: S1, weighing hydroxypropyl methylcellulose and dissolving it in water to prepare a first solution, weighing tetraacetylethylenediamine and dissolving it in hot water to prepare a second solution; S2, measuring the silicon-vanadium liquid, adding the second solution to the silicon-vanadium liquid and stirring for t1, then adding the first solution and stirring for t2; S3, heating to T1 and stirring t3; Keep warm under conditions of S4 and T2, stop stirring, age for t4 and filter to obtain low-silicon vanadium liquid.
2. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: The concentration range of the first solution is 5-10 g / L, and the concentration range of the second solution is 50-100 g / L.
3. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: The temperature of the hot water is in the range of 90-95°C.
4. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: The silicon-vanadium liquid is an alkaline silicon-vanadium liquid or an acidic silicon-vanadium liquid, and the silicon content in the silicon-vanadium liquid is 0.2-3 g / L, and the vanadium content is 0.2-50 g / L.
5. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: In step S2, the ratio of the volume (mL) of the second solution to the silicon content (g) in the silicon-vanadium-containing solution is in the range of 20-30:
1.
6. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: In step S2, the ratio of the volume (mL) of the first solution to the volume (mL) of the silicon-vanadium liquid is in the range of 1 to 3:
100.
7. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: The range of t1 is 10 to 20 minutes, and the range of t2 is 10 to 20 minutes.
8. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: The range of T1 is 45-60° C., and the range of t3 is 20-30 minutes.
9. The method for preparing low-silicon vanadium liquid according to claim 1, characterized in that: The range of T2 is 45-50° C., and the range of t4 is 30-60 minutes.
10. A low-silicon vanadium liquid, characterized in that: The method is prepared by any one of claims 1 to 9.