Russian standard P65 section heat treatment steel rail production method
Through the online heat treatment process, including LF furnace refining and air spray cooling, the problems of the Russian standard P65 section heat treatment rail in tensile strength, elongation after break and hardness are solved, achieving efficient and low-cost production results.
Patent Information
- Application Number
- CN202411145328.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
When producing Russian standard P65 section heat treatment rails, it is difficult to meet the requirements of high tensile strength, elongation after break and hardness at the same time, and online heat treatment equipment is investment high, but production efficiency and cost control are difficult to optimize.
The online heat treatment process is adopted, including LF furnace refining, heating, rolling and air spray cooling, to control the alkalinity, heating temperature and time of the furnace slag, to ensure that the rails are evenly cooled and straightened during the heat treatment process, and the chemical composition and hardness meet specific standards.
The high tensile strength, elongation after break and hardness of the rail are achieved, the production cost and deformation are reduced, and the mechanical properties and economic benefits of the rail are improved.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical materials, and in particular relates to a method for producing a Russian standard P65 cross-section heat-treated rail. Background Art
[0002] The laying and use practices at home and abroad have shown that the use of 1200-1300MPa full-length quenched rails on small half-warp curves can increase their service life by 2-5 times, which has significant economic benefits. The advantages of online heat treatment of rails are as follows:
[0003] 1) Online heat treatment of rails increases production efficiency. The hourly output of online heat treatment of rails is 3 to 4 times higher than that of offline heat treatment.
[0004] 2) Low production cost. Although the investment in online quenching equipment is higher than that in offline quenching, its production cost (manpower, time, energy consumption per ton of product, etc.) is much less.
[0005] 3) The quality of the rails is good. Since the entire rail structure is cooled from austenite, there will be no coarse-grained softening zone at the junction of the rail head / rail waist, and the rail waist and rail bottom are also properly strengthened. During residual heat quenching, while the rail head is accelerated to cool, compressed air or water is also sprayed on the rail bottom to cool it, so that the contraction, expansion and transformation stresses are balanced during the quenching process, and the conveying guide rollers are used to limit the deformation of the rails in a hot state. Therefore, the straightness of the rails is better when they leave the quenching equipment, and the deformation and residual stress are small during straightening. Summary of the invention
[0006] The purpose of the present invention is to provide a method for producing a Russian standard P65 cross-section heat-treated steel rail. The P65 heat-treated steel rail obtained by the production method has the following mechanical properties: rail tensile strength Rm≥1180MPa; elongation after fracture A≥10%; tread hardness 350-390HB; rail head cross-section hardness 1 point ≥340HB, 2 points ≥331HB, 3 points ≥321HB, 4 points ≥340HB.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] The present invention discloses a method for producing a Russian standard P65 cross-section heat-treated rail, comprising: smelting, heating, rolling, and online heat treatment processes;
[0009] During LF furnace refining, the slag basicity is controlled to be ≥2.0, the off-site temperature is 1580~1590℃; the deep vacuum degassing time is ≥16min, and the soft blowing time after vacuum degassing is ≥16min;
[0010] The total heating time of the steel billet is ≥ 3 hours and 10 minutes, of which the preheating temperature of the heating furnace is ≤ 800°C, the first heating temperature is ≤ 1200°C, the second heating temperature is 1100-1280°C, and the soaking temperature is 1150-1260°C;
[0011] The ingot is rolled into rails by a universal rolling mill, with the starting rolling temperature controlled at 1080-1150°C and the final rolling temperature at 920-950°C;
[0012] The rails are air-cooled to 750-820℃ before entering the heat treatment line. The cooling method is air jet cooling. The rails are quickly cooled to 510-550℃ in the heat treatment line, and then the cooling intensity is reduced to maintain the rail temperature at 510-550℃ for a period of time before leaving the heat treatment line. After leaving the heat treatment line, the rails are naturally air-cooled to room temperature. The total online heat treatment time is 100-140s. The rail temperature after leaving the heat treatment line is 510-550℃, and then slowly cooled to room temperature for straightening and ultrasonic flaw detection.
[0013] The chemical composition of the steel rail includes, by mass percentage: C 0.72-0.80%, Si 0.15-0.58%, Mn 0.70-1.20%, Cr 0.04-0.15%, P≤0.020%, S≤0.020%, and the rest is Fe and unavoidable impurities.
[0014] Furthermore, the rail meets the following requirements: tensile strength Rm≥1180MPa; elongation after fracture A≥10%.
[0015] Furthermore, the rails meet the following requirements: tread hardness 350-390HB; rail head cross-sectional hardness 1 point ≥ 340HB, 2 points ≥ 331HB, 3 points ≥ 321HB, 4 points ≥ 340HB.
[0016] Furthermore, the chemical composition of the steel rail includes, by mass percentage, C: 0.76%; Si: 0.50%; Mn: 0.95%; P: 0.006%; S: 0.016%; Cr: 0.06%, and the rest is Fe and unavoidable impurities.
[0017] Furthermore, the mechanical properties of the rails are as follows: tensile strength reaches 1255MPa, elongation after fracture reaches 12.5%, tread hardness is 374HB, and the cross-sectional hardness of the rail head is 374HB at 1 point, 367HB at 2 points, 358HB at 3 points, and 368HB at 4 points.
[0018] Furthermore, the metallographic structure of the rail head is pearlite.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] The purpose of the present invention is to provide a method for producing a P65 heat-treated steel rail with a Russian standard cross section. The P65 heat-treated steel rail obtained by the production method has the following mechanical properties: rail tensile strength Rm≥1180MPa; elongation after fracture A≥10%; tread hardness 350-390HB; rail head cross-sectional hardness 1 point ≥340HB, 2 points ≥331HB, 3 points ≥321HB, 4 points ≥340HB. DETAILED DESCRIPTION
[0021] The present invention will be further described in detail below in conjunction with specific embodiments to facilitate a clearer understanding of the present invention (all percentages in the following embodiments are by weight).
[0022] A method for producing a Russian standard P65 section online heat-treated rail comprises the following steps:
[0023] 1) Hot metal pretreatment: The sulfur content in the hot metal is 0.011% and the phosphorus content is 0.10%.
[0024] 2) Converter smelting: Control the C content of steel to 0.1% and the tapping temperature to 1646°C. Add lime, silicon calcium barium and fluorite after tapping to modify the slag. Ensure the argon blowing effect during the tapping process. Avoid agglomeration of the top slag when the molten steel is refined in place.
[0025] 3) LF furnace refining: During LF refining, the slag basicity is controlled to be ≥2.1 and the off-site temperature is 1592°C;
[0026] 4) VD vacuum degassing: Deep vacuum degassing time is 17 minutes, and soft blowing is performed for 17 minutes after vacuum degassing. During the soft blowing process, the argon flow rate is stable, and the molten steel creeps without exposure.
[0027] 5) Continuous casting: The continuous casting process adopts protective casting, low-aluminum protective slag, weak cooling water distribution in the secondary cooling section, constant pulling speed operation throughout the process, pulling speed 0.60m / min, electromagnetic stirring and light pressure of the casting machine are turned on to ensure the quality of the casting.
[0028] 6) Billet heating: The total heating time is 3 hours and 20 minutes. The heating time and heating temperature of each section are shown in Table 1.
[0029] Table 1 Heating process of P65 heat-treated rails
[0030] Preheating section Heating 1 stage Heating 2 stages Heat soaking section Heating time 25min 50min 55min 30min temperature 723℃ 935℃ 1212℃ 1244℃
[0031] 7) Rolling: The ingot is rolled into rails by a universal rolling mill, with the starting rolling temperature at 1100°C and the final rolling temperature at 936°C.
[0032] 8) Online heat treatment: The rails are finally rolled and air-cooled to 780℃ before entering the heat treatment line. Air jet cooling is used to quickly cool the rails to 520℃ in the heat treatment line. Then the air cooling intensity is reduced to balance the internal temperature return and cooling intensity of the rails. The rail temperature is maintained at 520℃ for a certain period of time before leaving the heat treatment line. The total online heat treatment time is 140s. After leaving the heat treatment line, the rails are naturally air-cooled to room temperature and then straightened and inspected.
[0033] After inspection, the chemical composition percentages of P65 heat-treated rails are as follows: C: 0.76%; Si: 0.50%; Mn: 0.95%; P: 0.006%; S: 0.016%; Cr: 0.06%, and the rest are Fe and unavoidable impurities.
[0034] The mechanical properties of P65 heat-treated rails are as follows: tensile strength reaches 1255MPa, elongation after fracture reaches 12.5%, tread hardness is 374HB, cross-sectional hardness of rail head is 374HB at 1 point, 367HB at 2 points, 358HB at 3 points, and 368HB at 4 points. The metallographic structure of the rail head is pearlite.
[0035] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing heat-treated rails with a Russian standard P65 section, characterized in that: include: Smelting, heating, rolling, online heat treatment processes; During LF furnace refining, the slag basicity is controlled to be ≥2.0, the off-site temperature is 1580~1590℃; the deep vacuum degassing time is ≥16min, and the soft blowing time after vacuum degassing is ≥16min; The total heating time of the steel billet is ≥ 3 hours and 10 minutes, of which the preheating temperature of the heating furnace is ≤ 800°C, the first heating temperature is ≤ 1200°C, the second heating temperature is 1100-1280°C, and the soaking temperature is 1150-1260°C; The ingot is rolled into rails by a universal rolling mill, with the starting rolling temperature controlled at 1080-1150°C and the final rolling temperature at 920-950°C; The rails are air-cooled to 750-820℃ before entering the heat treatment line. The cooling method is air jet cooling. The rails are quickly cooled to 510-550℃ in the heat treatment line, and then the cooling intensity is reduced to maintain the rail temperature at 510-550℃ for a period of time before leaving the heat treatment line. After leaving the heat treatment line, the rails are naturally air-cooled to room temperature. The total online heat treatment time is 100-140s. The rail temperature after leaving the heat treatment line is 510-550℃, and then slowly cooled to room temperature for straightening and ultrasonic flaw detection. The chemical composition of the steel rail includes, by mass percentage: C 0.72-0.80%; Si 0.15-0.58%; Mn 0.70~1.20%; Cr 0.04~0.15%; P≤0.020%; S≤0.020%, and the rest are Fe and unavoidable impurities.
2. The method for producing heat-treated rails with a Russian standard P65 section according to claim 1, characterized in that: The rails meet the following requirements: tensile strength Rm ≥ 1180MPa; elongation after fracture A ≥ 10%.
3. The method for producing heat-treated rails with a Russian standard P65 section according to claim 1, characterized in that: The rails meet the following requirements: tread hardness 350~390HB; rail head cross-section hardness 1 point ≥340HB, 2 points ≥331HB, 3 points ≥321HB, 4 points ≥340HB.
4. The method for producing heat-treated rails with a Russian standard P65 section according to claim 1, characterized in that: The chemical composition of the steel rail includes, by mass percentage, C: 0.76%, Si: 0.50%, Mn: 0.95%, P: 0.006%, S: 0.016%, Cr: 0.06%, and the rest is Fe and unavoidable impurities.
5. The method for producing heat-treated rails with a Russian standard P65 section according to claim 4, characterized in that: The mechanical properties of the rails are: tensile strength reaches 1255MPa, elongation after fracture reaches 12.5%, tread hardness is 374HB, cross-sectional hardness of the rail head is 374HB at 1 point, 367HB at 2 points, 358HB at 3 points, and 368HB at 4 points.