Viscose fiber with high carbonization rate as well as preparation method and application thereof

By adding carbonaceous substances and wet strength agents in the online production process of viscose fibers, combined with modification treatment, the carbonization yield of viscose fibers is improved, the problem of low carbonization yield in the existing technology is solved, and energy saving is achieved Reduce consumption and widely used in the field of thermal insulation.

CN118932515APending Publication Date: 2024-11-12WEIFANG XINLONG BIOMATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989896.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the carbonization rate of viscose fibers is low, resulting in raw material consumption and energy waste, and there are no reports of modification processing in the online production process to improve the carbonization rate.

Method used

During the online production process of viscose fiber, the carbonization yield of the fiber is improved by adding carbonaceous substance dispersion and wet strength agent, and the stability and carbonization of the fiber are enhanced by modification treatment to prepare high carbonation viscosity Colloidal fiber.

Benefits of technology

The carbonization rate of viscose fiber has been improved from 16.2% to 28.5% to 33.6%, saving raw material consumption and energy consumption, reducing steam consumption, and making the fiber suitable for photovoltaic and thermal insulation fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a high-carbonization-rate viscose fiber and a preparation method and application thereof. The surface color depth value K / S value of the viscose fiber is 26.8-35.1, and the carbonization yield is 28.5%-33.6%. The preparation method comprises the following steps: preparation of a carbon-containing substance dispersion liquid, preparation of a blended spinning stock solution, spinning and post-treatment. In the post-treatment, wet strength agent treatment and modification treatment procedures are added after the last water washing procedure and before the drying procedure. According to the invention, by utilizing an online production mode, the fiber is prevented from being re-treated by downstream customers during use, the raw material consumption and the energy consumption are reduced, the raw material consumption can be reduced by 3.0-5.0%, and the steam consumption can be reduced by 6.5-8.5 tons per ton of viscose. After being carbonized, the viscose fiber prepared by the method can be widely applied to the thermal insulation fields of photovoltaic materials, single crystal furnace thermal insulation materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of viscose fibers, and in particular to a viscose fiber with a high carbonization rate and a preparation method and application thereof. Background Art

[0002] Viscose fiber is a cellulose fiber obtained by extracting cellulose from natural cellulose that exists in large quantities in nature and reshaping the fiber molecules using the viscose process. It contains C, H, and O elements, of which the carbon content is 44.44%, the hydrogen content is 6.17%, and the oxygen content is 49.39%. (The molecular formula of cellulose is (C6H10O5)n). The specific structural formula of viscose fiber is as follows: .

[0003] As one of the three major raw material systems for preparing carbon fiber materials, viscose fiber has excellent ablation resistance and heat insulation properties compared with polyacrylonitrile-based carbon fiber materials and asphalt-based carbon fiber materials, and is an important military material. At the same time, viscose-based carbon fiber, which is soft, conductive, and has a developed pore structure, is used as electric heating, environmental protection, thermal insulation, and medical and sanitary materials, and also has a place in the civilian market.

[0004] However, the carbon content of viscose fiber is low, and the carbonization yield is also low. The actual carbonization yield is generally less than one-fifth. In order to improve the carbonization yield of viscose fiber in the prior art, carbon fiber manufacturers generally reprocess the purchased viscose fiber, which results in significant raw material consumption and energy waste.

[0005] There is no report in the prior art on performing modification treatment in the online production process of viscose fibers to improve the carbonization yield of the produced viscose fibers. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a viscose fiber with a high carbonization rate and a preparation method and application thereof, to achieve the following invention objectives: to carry out treatment and modification during the online production process of the viscose fiber, to improve the carbonization yield of the viscose fiber, and to save raw material consumption and energy consumption, and the prepared viscose fiber can be directly carbonized for use.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions: A high carbonization rate viscose fiber, wherein the surface color depth value K / S value of the viscose fiber is 26.8-35.1, and the carbonization yield is 28.5%-33.6%.

[0008] A method for preparing viscose fiber with a high carbonization rate comprises the following steps: 1. Preparation of carbonaceous material dispersion A certain amount of dispersant, wetting agent, defoamer, carbon-containing material and water are added to a dispersion sand mill, and the grinding speed and time are controlled to prepare a carbon-containing material dispersion system, and the particle size D90 of the dispersion system is 0.851-1.095 microns. A thickener is added to the prepared carbon-containing material dispersion system to obtain a carbon-containing material dispersion liquid, and its viscosity is 25-35s (falling ball viscosity) to increase the stability of the carbon-containing material dispersion and prevent the carbon-containing material from precipitating.

[0009] The dispersant is one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium methylene bisnaphthalene sulfonate and sodium hexametaphosphate; The wetting agent is one of diethylene glycol, BX powder, and BYK-164 of BYK Chemical; The defoaming agent is one of polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether, and polydimethylsiloxane; The carbon-containing material is one or more of carbon black, bamboo charcoal, graphite and graphene; The mass ratio of the dispersant, wetting agent, defoamer, carbon-containing substance and water is 15-28:3-8:2-5:100-200:500; The grinding speed is 3000-5000 r / min; The grinding time is 4h to 8h.

[0010] The thickener is one of sodium carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone and sodium alginate; the added amount is 2-4.5% of the mass of the water used.

[0011] 2. Preparation of blended spinning solution With cellulose pulp as raw material, viscose fiber spinning stock solution is prepared through conventional viscose preparation process, wherein the composition is as follows: type A cellulose: 8.93%-9.25%, sodium hydroxide: 4.51%-4.82%, and the falling ball viscosity is 35-52s. By means of a flexible pre-spinning injection adding device, the prepared carbon-containing substance dispersion is added to the viscose fiber spinning stock solution at a ratio of 4.0%-10.0% of the mass of the carbon-containing substance to the type A cellulose in the spinning stock solution, to obtain a blended spinning solution.

[0012] The flexible pre-spinning injection adding device is composed of a filtering device, a metering device and a mixing and dispersing device; the filtering device is a bag type with a filtering area of ​​1 to 2 m 2 The metering device adopts a mechanical diaphragm pump (Q=1500L / h) with an outlet pressure of 0.7-0.9MPa; the mixing and dispersing device is composed of a dynamic mixing device and a static mixing device connected in series, the dynamic mixing device is a planetary gear dynamic mixer, and the static mixing device is an SK type static mixing device.

[0013] 3. Spinning and post-processing The blended spinning stock solution is spun through an adjusted coagulation bath, and the primary filament bundle is cut, desulfurized, washed, pickled, washed, treated with a wet strength agent, and modified after being drawn. After each of the above treatments, the fiber cotton layer is pressed with a small pressing roller, and the above-treated fibers are dried to obtain viscose fibers with a high carbonization rate.

[0014] The coagulation bath comprises the following components: 100-120 g / L sulfuric acid, 10.0-18.5 g / L zinc sulfate, and 290-330 g / L sodium sulfate; The desulfurization bath is a 4.0-10.0 g / L sodium hydroxide solution at a temperature of 55-75°C; The pickling is carried out by using a sulfuric acid solution with a concentration of 2 to 6 g / L and a temperature of 40 to 55° C. The cleanliness of the fiber is improved by pickling.

[0015] The wet strength agent treatment method is to use a mixed solution of a wet strength agent and a penetrant to immerse the fiber for 3 to 5 minutes; the concentration of the wet strength agent in the mixed solution is 10 to 20 g / L, and the concentration of the penetrant is 0.5 to 3 g / L; The wet strength agent is one of melamine formaldehyde resin and polyepichlorohydrin resin; the penetrant is castor oil or polyoxyethylene fatty amine; The characteristics of the thermosetting resin formed after the wet strength agent is dried are used to form a three-dimensional network structure during drying, which increases the stability and carbonization of the fiber. The penetrant is used to enhance the penetration ability of the wet strength agent, further enhancing the effect of the wet strength agent.

[0016] The modification treatment is to control the temperature of the modifier solution with a mass concentration of 5% to 10% at 50 to 95°C, pump it into the overflow tank, and treat the fiber cotton layer by overflow. The overflow speed is 500 to 720L / min and the treatment time is 5 to 10min.

[0017] The modifier is one or more of ammonium chloride, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium sulfate; Preferably, the modifier is ammonium chloride; a mixture of ammonium chloride and ammonium sulfate in a mass ratio of 1:0.8-1.2; a mixture of diammonium hydrogen phosphate and ammonium dihydrogen phosphate in a mass ratio of 1:0.8-1.2.

[0018] The modified agent can be evenly deposited on the fiber surface after modification; The oil bath: concentration is 2.0-6.0 g / L, temperature is 50-60° C., pH value is 8.5-10.5; The pressing pressure is 0.10-0.15 MPa.

[0019] The drying is performed by steam drying, the drying temperature is 105-120° C., and the drying time is 35-50 minutes.

[0020] The beneficial effects achieved by the present invention using the above technical solution are as follows: (1) The present invention increases the carbon content of the fiber itself by adding carbon-containing substances in the early stage. These carbon-containing substances are 100% carbonized during the later carbonization. At the same time, the carbon-forming substances protect and induce carbonization of the fibers during the later carbonization of the fibers, and play the role of "carbon frame"; by treating the viscose fibers with a wet strength agent during the refining process, the stability of the fibers is increased, and the three-dimensional network structure after drying makes the carbon layer more stable during carbonization, reducing dimensional shrinkage, and the wet strength agent has the effect of promoting carbonization; the modification treatment during the refining process allows the viscose fibers to proceed at a relatively moderate speed within a longer temperature range during high-temperature carbonization, promoting the dehydration reaction, thereby increasing the carbonization yield; through the above methods, the carbonization yield of the viscose fibers is increased from 16.2% to 28.5% to 33.6%.

[0021] (2) The present invention utilizes an online production method to avoid downstream customers from having to reprocess the fibers when using them, thereby saving raw material consumption and energy consumption. It can reduce raw material consumption by 3.0 to 5.0% and steam consumption by 6.5 to 8.5 tons / ton of viscose fiber.

[0022] (3) The specifications of the viscose fiber prepared by the present invention can be adjusted according to user needs. The preferred linear density is from 1.0D to 10.0D, the fiber surface color depth value K / S value is from 26.8 to 35.1, and the carbonization yield is increased from 16.2% to 28.5% to 33.6%.

[0023] (4) The viscose fiber prepared by the technology of the present invention is made into felt, which can be widely used in photovoltaic, single crystal furnace insulation materials and other thermal insulation fields after carbonization. DETAILED DESCRIPTION

[0024] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0025] The carbonization yield is the ratio of the mass of the carbonized viscose fiber to the mass of the input viscose fiber. After drying the viscose fiber with a mass of m1, slowly heat it to 245℃ within 1.5h and fully oxidize it in the air. After cooling at room temperature, place the sample in a nitrogen-protected tubular high-temperature furnace, heat it from room temperature to 850℃ within 1h, maintain it for 30min, gradually heat it up and carbonize it for a total of 1.5h, and weigh it as m2 after carbonization.

[0026] .

[0027] Embodiment 1: A method for preparing high carbonization rate viscose fiber with a specification of 2.0D*38mm, comprising the following steps: 1. Preparation of carbonaceous material dispersion A certain amount of dispersant, wetting agent, defoamer, carbon-containing substance and water are added to a dispersion sand mill, and the grinding speed and time are controlled to prepare a carbon-containing substance dispersion system, and the particle size D90 of the dispersion system is 0.851 microns. A thickener is added to the prepared carbon-containing substance dispersion system to obtain a carbon-containing substance dispersion liquid, and its viscosity is 25s (falling ball viscosity) to increase the stability of the carbon-containing substance dispersion and prevent the carbon-containing substance from precipitating.

[0028] The dispersant is sodium dodecyl sulfate; the wetting agent is diethylene glycol; the defoaming agent is polyoxyethylene polyoxypropanolamine ether; the carbon-containing substance is carbon black; the mass ratio of the dispersant, wetting agent, defoaming agent, carbon-containing substance and water is 15:3:2:100:500; the grinding speed is 5000r / min; the grinding time is 4h; the thickener is sodium carboxymethyl cellulose, and the addition amount thereof is 2.0% of the mass of the water used.

[0029] 2. Preparation of blended spinning solution Using cellulose pulp as raw material, viscose fiber spinning stock solution was prepared through conventional viscose preparation process, whose composition was: type A cellulose: 8.93%, sodium hydroxide: 4.51%, and falling ball viscosity of 35s. Using a flexible pre-spinning injection adding device, the prepared carbon-containing substance dispersion was added to the viscose fiber spinning stock solution at a ratio of 4.0% of the mass of type A cellulose in the spinning stock solution to obtain a blended spinning solution containing carbon-containing substances.

[0030] The flexible pre-spinning injection adding device is composed of a filtering device, a metering device and a mixing and dispersing device; the filtering device is a bag type with a filtering area of ​​1m 2 The metering device adopts a mechanical diaphragm pump (Q=1500L / h) with an outlet pressure of 0.7MPa; the mixing and dispersing device is composed of a dynamic mixing device and a static mixing device connected in series, the dynamic mixing device is a planetary gear dynamic mixer, and the static mixing device is an SK type static mixing device.

[0031] 3. Spinning and post-processing The blended spinning stock solution is spun through an adjusted coagulation bath, and the primary filament bundle is cut, desulfurized, washed, pickled, washed, treated with a wet strength agent, and modified after being drawn. After each of the above treatments, the fiber cotton layer is pressed with a small pressing roller, and the above-treated fibers are dried to obtain viscose fibers with a high carbonization rate.

[0032] The pressing pressure is 0.10 MPa; The coagulation bath includes the following components: 100 g / L sulfuric acid, 10.0 g / L zinc sulfate, and 290 g / L sodium sulfate; The desulfurization bath is a 4.0 g / L sodium hydroxide solution, and the temperature of the desulfurization bath is 75°C; The pickling is carried out by using a sulfuric acid solution with a concentration of 2 g / L and a temperature of 55° C. The cleanliness of the fiber is improved by pickling.

[0033] The wet strength agent treatment method is to use a mixed solution of a wet strength agent and a penetrant to immerse for 5 minutes; the concentration of the wet strength agent in the mixed solution is 10g / L, and the concentration of the penetrant is 0.5g / L; the wet strength agent is melamine formaldehyde resin; and the penetrant is castor oil; The characteristics of the thermosetting resin formed after the wet strength agent is dried are used to form a three-dimensional network structure during drying, which increases the stability and carbonization of the fiber. The penetrant is used to enhance the penetration ability of the wet strength agent, further enhancing the effect of the wet strength agent.

[0034] The modification treatment method is to heat a 5.0wt% modifier solution to 95°C, pump it into an overflow tank, and treat the fiber cotton layer by overflow, with an overflow rate of 720L / min and a treatment time of 10min; The modifier is ammonium chloride; The modified agent can be evenly deposited on the fiber surface after modification; The oil bath: concentration 2.0 g / L, temperature 60° C., pH 8.5; The drying is performed by steam drying, the drying temperature is 105° C., and the drying time is 50 min.

[0035] The viscose fiber prepared in this embodiment 1 has a specification of 2.0D*38mm, a fiber surface color depth value K / S value of 26.8, and a carbonization yield of 28.5%. The viscose fiber is made into felt, which can be widely used in photovoltaic, single crystal furnace insulation materials and other thermal insulation fields after carbonization.

[0036] Embodiment 2: A method for preparing high carbonization rate viscose fiber with a specification of 4.3D*51mm, comprising the following steps: 1. Preparation of carbonaceous material dispersion A certain amount of dispersant, wetting agent, defoamer, carbon-containing substance and water are added to a dispersion sand mill, and the grinding speed and time are controlled to prepare a carbon-containing substance dispersion system, and the particle size D90 of the dispersion system is 0.952 microns. A thickener is added to the prepared carbon-containing substance dispersion system to obtain a carbon-containing substance dispersion liquid, and its viscosity is 31s (falling ball viscosity) to increase the stability of the carbon-containing substance dispersion and prevent the carbon-containing substance from precipitating.

[0037] The dispersant is sodium methylene bisnaphthalene sulfonate; the wetting agent is pull-opening powder BX; the defoaming agent is polyoxypropylene polyoxyethylene glycerol ether; the carbon-containing substance is bamboo charcoal; the mass ratio of the dispersant, wetting agent, defoaming agent, carbon-containing substance and water is 20:5:4:150:500; the grinding speed is 4215r / min; the grinding time is 6h; the thickener is polyvinyl pyrrolidone, and its addition amount is 3.6% of the mass of the water used.

[0038] 2. Preparation of blended spinning solution Using cellulose pulp as raw material, viscose fiber spinning stock solution was prepared through conventional viscose preparation process, whose composition was: type A cellulose: 9.06%, sodium hydroxide: 4.68%, and falling ball viscosity of 45s. Using a flexible pre-spinning injection adding device, the prepared carbon-containing substance dispersion was added to the viscose fiber spinning stock solution at a ratio of 7.2% of the mass of type A cellulose in the spinning stock solution to obtain a blended spinning solution containing carbon-containing substances.

[0039] The flexible pre-spinning injection adding device is composed of a filtering device, a metering device and a mixing and dispersing device; the filtering device is a bag type with a filtering area of ​​1.5m 2 The metering device adopts a mechanical diaphragm pump (Q=1500L / h) with an outlet pressure of 0.8MPa; the mixing and dispersing device is composed of a dynamic mixing device and a static mixing device connected in series, the dynamic mixing device is a planetary gear dynamic mixer, and the static mixing device is an SK type static mixing device.

[0040] 3. Spinning and post-processing The blended spinning stock solution is spun through an adjusted coagulation bath, and the primary filament bundle is cut, desulfurized, washed, pickled, washed, treated with a wet strength agent, and modified after being drawn. After each of the above treatments, the fiber cotton layer is pressed with a small pressing roller, and the above-treated fibers are dried to obtain viscose fibers with a high carbonization rate.

[0041] The pressing pressure is 0.13 MPa; The coagulation bath includes the following components: 112 g / L sulfuric acid, 15.6 g / L zinc sulfate, and 316 g / L sodium sulfate; The desulfurization bath is a 6.8 g / L sodium hydroxide solution, and the temperature of the desulfurization bath is 62°C; The pickling is carried out by using a sulfuric acid solution with a concentration of 4.5 g / L and a temperature of 49° C. The cleanliness of the fiber is improved by pickling.

[0042] The wet strength agent treatment method is to use a mixed solution of a wet strength agent and a penetrant to immerse for 4 minutes; The concentration of the wet strength agent in the mixed solution is 16.2 g / L, and the concentration of the penetrant is 1.8 g / L; the wet strength agent is polyepichlorohydrin resin; and the penetrant is polyoxyethylene fatty amine; The characteristics of the thermosetting resin formed after the wet strength agent is dried are used to form a three-dimensional network structure during drying, which increases the stability and carbonization of the fiber. The penetrant is used to enhance the penetration ability of the wet strength agent, further enhancing the effect of the wet strength agent.

[0043] The modification treatment method is to heat 8.0% of the modifier solution to 65°C, pump it into the overflow tank by means of a pump, and treat the fiber cotton layer by overflow, the overflow speed is 600L / min, and the treatment time is 7.5min; the modifier is ammonium chloride and ammonium sulfate, and the mass ratio is 1:1; The modified agent can be evenly deposited on the fiber surface after modification; The oil bath: 4.5 g / L, temperature 56° C., pH 9.5; The drying is performed by steam drying, the drying temperature is 112° C., and the drying time is 41 minutes.

[0044] The viscose fiber prepared in this embodiment 2 has a specification of 4.3D*51mm, a fiber surface color depth value K / S value of 31.2, and a carbonization yield of 31.5%. The viscose fiber is made into felt, which can be widely used in photovoltaic, single crystal furnace insulation materials and other thermal insulation fields after carbonization.

[0045] Embodiment 3: A method for preparing high carbonization rate viscose fiber with a specification of 10.0D*76mm, comprising the following steps: 1. Preparation of carbonaceous material dispersion A certain amount of dispersant, wetting agent, defoamer, carbon-containing substance and water are added to a dispersion sand mill, and the grinding speed and time are controlled to prepare a carbon-containing substance dispersion system, and the particle size D90 of the dispersion system is 1.095 microns. A thickener is added to the prepared carbon-containing substance dispersion system to obtain a carbon-containing substance dispersion liquid, and its viscosity is 35s (falling ball viscosity) to increase the stability of the carbon-containing substance dispersion and prevent the carbon-containing substance from precipitating.

[0046] The dispersant is sodium hexametaphosphate; the wetting agent is BYK-164; the defoaming agent is polydimethylsiloxane; the carbon-containing substance is graphene; the mass ratio of the dispersant, wetting agent, defoaming agent, carbon-containing substance and water is 28:8:5:200:500; the grinding speed is 3000r / min; the grinding time is 8h; the thickener is sodium alginate, and the addition amount thereof is 4.5% of the mass of the water used.

[0047] 2. Preparation of blended spinning solution With cellulose pulp as raw material, viscose fiber spinning solution was prepared through conventional viscose preparation process. Its composition was: type A cellulose: 9.25%, sodium hydroxide: 4.82%, and falling ball viscosity was 52 s. The prepared carbon-containing substance dispersion was added to the viscose fiber spinning solution by a flexible pre-spinning injection adding device at a ratio of 10.0% of the mass of type A cellulose in the spinning solution to obtain a blended spinning solution containing carbon-containing substances.

[0048] The flexible pre-spinning injection adding device is composed of a filtering device, a metering device and a mixing and dispersing device; the filtering device is of bag type with a filtering area of ​​2m2; the metering device adopts a mechanical diaphragm pump (Q=1500L / h) with an outlet pressure of 0.9MPa; the mixing and dispersing device is composed of a dynamic mixing device and a static mixing device connected in series, the dynamic mixing device is a planetary gear dynamic mixer, and the static mixing device is an SK type static mixing device.

[0049] 3. Spinning and post-processing The blended spinning stock solution is spun through an adjusted coagulation bath, and the primary filament bundle is cut, desulfurized, washed, pickled, washed, treated with a wet strength agent, and modified after being drawn. After each of the above treatments, the fiber cotton layer is pressed with a small pressing roller, and the above-treated fibers are dried to obtain viscose fibers with a high carbonization rate.

[0050] The pressing pressure is 0.15MPa; The coagulation bath includes the following components: 120 g / L sulfuric acid, 18.5 g / L zinc sulfate, and 330 g / L sodium sulfate; The desulfurization bath is a 10.0 g / L sodium hydroxide solution, and the temperature of the desulfurization bath is 55°C; The pickling is carried out by using a sulfuric acid solution with a concentration of 6 g / L and a temperature of 40° C. The cleanliness of the fiber is improved by pickling.

[0051] The wet strength agent treatment method is to use a mixed solution of a wet strength agent and a penetrant to immerse for 3 minutes; The concentration of the wet strength agent in the mixed solution is 20 g / L, and the concentration of the penetrant is 3 g / L; the wet strength agent is melamine formaldehyde resin; the penetrant is polyoxyethylene fatty amine; The characteristics of the thermosetting resin formed after the wet strength agent is dried are used to form a three-dimensional network structure during drying, which increases the stability and carbonization of the fiber. The penetrant is used to enhance the penetration ability of the wet strength agent, further enhancing the effect of the wet strength agent.

[0052] The modification treatment method is to heat a 10wt% modifier solution to 50°C, pump it into an overflow tank, and treat the fiber cotton layer by overflow, with an overflow speed of 500L / min and a treatment time of 5min; The modifier is diammonium hydrogen phosphate and ammonium dihydrogen phosphate, with a mass ratio of 1:2; The modified agent can be evenly deposited on the fiber surface after modification; The oil bath: 6.0 g / L, temperature 50° C., pH 10.5; The drying is performed by steam drying, the drying temperature is 120° C., and the drying time is 35 min.

[0053] The viscose fiber prepared in this embodiment 3 has a specification of 10.0D*76mm, a fiber surface color depth value K / S value of 35.1, and a carbonization yield of 33.6%. The viscose fiber is made into felt, which can be widely used in photovoltaic, single crystal furnace insulation materials and other thermal insulation fields after carbonization.

[0054] Comparative Example 1: On the basis of Example 1, the wet strength agent treatment and modification treatment steps were omitted, and the remaining processes were the same as those in Example 1.

[0055] The viscose fiber prepared in Comparative Example 1 has a specification of 2.0D*38mm, a fiber surface color depth value K / S value of 26.7, and a carbonization yield of 20.5%.

[0056] Comparative Example 2: On the basis of Example 1, no carbon-containing dispersion is added to the spinning solution, the modification step is omitted in the post-treatment, and the remaining processes are the same as in Example 1.

[0057] The viscose fiber prepared in Comparative Example 2 has a specification of 2.0D*38mm, a fiber surface color depth value K / S value of 0, and a carbonization yield of 21.1%.

[0058] Comparative Example 3 On the basis of Example 1, no carbon-containing dispersion was added to the spinning solution, the wet strength agent treatment step was omitted in the post-treatment, and the remaining processes were the same as in Example 1.

[0059] The viscose fiber prepared in Comparative Example 3 has a specification of 2.0D*38mm, a fiber surface color depth value K / S value of 0, and a carbonization yield of 23.2%.

[0060] Comparative Example 4 On the basis of Example 1, no carbon-containing dispersion is added to the spinning solution, the wet strength agent treatment and modification treatment steps are omitted in the post-treatment, and the remaining processes are the same as those in Example 1.

[0061] The viscose fiber prepared in Comparative Example 4 has a specification of 2.0D*38mm, a fiber surface color depth value K / S value of 0, and a carbonization yield of 16.2%.

[0062] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high carbonization rate viscose fiber, characterized in that: The surface color depth value K / S value of the viscose fiber is 26.8-35.1, and the carbonization yield is 28.5%-33.6%.

2. A method for preparing viscose fiber with high carbonization rate, characterized in that: The preparation method comprises the following steps: preparation of a carbon-containing dispersion, preparation of a blended spinning solution, spinning and post-treatment; the post-treatment comprises adding a wet strength agent treatment and a modification treatment process after the last washing process and before the drying process.

3. The method for preparing a high carbonization rate viscose fiber according to claim 2, characterized in that: The preparation method of the carbon-containing substance dispersion is to disperse and grind a dispersant, a wetting agent, a defoamer, a carbon-containing substance and water to prepare a carbon-containing substance dispersion system, wherein the particle size D90 of the dispersion system is 0.851 to 1.095 microns, and then add a thickener to make its viscosity 25 to 35s to obtain a carbon-containing substance dispersion.

4. The method for preparing a high carbonization rate viscose fiber according to claim 3, characterized in that: The carbon-containing material is one or more of carbon black, bamboo charcoal, graphite and graphene.

5. The method for preparing viscose fiber with high carbonization rate according to claim 2, characterized in that: The preparation method of the blended spinning solution is as follows: the carbon-containing substance dispersion is added to the viscose fiber spinning solution according to the ratio of the carbon-containing substance to the mass of the type A cellulose in the spinning solution being 4.0% to 10.0%, so as to obtain the blended spinning solution.

6. The method for preparing a high carbonization rate viscose fiber according to claim 2, characterized in that: The wet strength agent treatment method is to use a mixed solution of a wet strength agent and a penetrant to immerse the fiber for 3 to 5 minutes; the concentration of the wet strength agent in the mixed solution is 10 to 20 g / L, and the concentration of the penetrant is 0.5 to 3 g / L; the wet strength agent is one of melamine formaldehyde resin and polyepichlorohydrin resin; the penetrant is castor oil or polyoxyethylene fatty amine.

7. The method for preparing viscose fiber with high carbonization rate according to claim 2, characterized in that: The modification treatment method is to use a modifier solution with a mass concentration of 5% to 10%, control the temperature to 50 to 95°C, treat the fiber cotton layer by overflow, the overflow speed is 500 to 720L / min, and the treatment time is 5 to 10min.

8. The method for preparing viscose fiber with high carbonization rate according to claim 7, characterized in that: The modifier is one or more of ammonium chloride, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, and ammonium sulfate.

9. The method for preparing viscose fiber with high carbonization rate according to claim 3, characterized in that: The mass ratio of the dispersant, wetting agent, defoamer, carbon-containing substance and water is 15-28:3-8:2-5:100-200:500; the added amount of the thickener is 2-4.5% of the mass of water.

10. Use of the viscose fiber according to claim 1 or the viscose fiber prepared by the preparation method according to claims 2 to 9 in the preparation of carbon fiber materials.