Preparation method of flexible degradable melt-blown filter material

Through the synergistic toughening of thermoplastic polyetherester block copolymer and hydrophobic nanoparticles, combined with corona electret technology, the problem of polylactic acid meltblown filter is solved, and the hand feel is not good and the flexibility of the polylactic acid meltblown filter is significantly improved. Extension strength and elongation at break achieve efficient toughening and good dispersion of the material.

CN118932534AActive Publication Date: 2024-11-12CHINA TEXTILE ACAD JIANGNAN BRANCH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410997571.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing polylactic acid meltblown filter material has a brittle feel and poor flexibility. The low molecular weight PEG reduces the upper limit of the use temperature and is easy to exudate. The polymer elastomer is incompatible with PLA, and the glass transition temperature and softness are low. , poor drafting performance and nanoparticles are not easily dispersed, resulting in limited toughening effect.

Method used

By synthesizing thermoplastic polyetherester copolymers, adding hydrophobic nanoparticles and polylactic acid slices, the block copolymers of hard and flexible chain segments are formed by transesterification reaction, and combined with corona electret technology, meltblown filtration is enhanced The tensile strength and elongation of the material can improve flexibility.

Benefits of technology

It significantly improves the flexibility and feel quality of the polylactic acid meltblown filter material, enhances its drafting performance under high-speed air flow field, ensures effective toughening and good dispersion of the material, while maintaining degradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960674330000061
    Figure BDA0004960674330000061
  • Figure BDA0004960674330000062
    Figure BDA0004960674330000062
  • Figure BDA0004960674330000071
    Figure BDA0004960674330000071
Patent Text Reader

Abstract

The invention provides a preparation method of a flexible degradable melt-blown filter material, and belongs to the technical field of composition preparation with a high-molecular compound as a base material, wherein polyester is obtained from hydroxy acid on a main chain of the high-molecular compound. Synthesizing a thermoplastic polyether ester copolymer: taking tetrabutyl titanate as a catalyst, taking dimethyl 1, 4-phthalate and diol as melting raw materials, then adding polyethylene glycol and an antioxidant to obtain a thermoplastic polyether ester block copolymer, and performing melt extrusion on the polylactic acid slices, the thermoplastic polyether ester block copolymer and hydrophobic nanoparticles to obtain composite master batches; and carrying out melt extrusion, melt blowing and drafting on the prepared composite master batch to obtain the micro-nano melt-blown filter material, and finally, carrying out corona electret melt-blown filter material. The method is applied to melt-blown filter material processing, and has the advantages of degradability, good flexibility and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a method for preparing a flexible and degradable melt-blown filter material, and belongs to the technical field of preparing a composition based on a polymer compound of polyester obtained from a hydroxy acid on the main chain. Background Art

[0002] Masks are effective protective materials for isolating virus transmission. Wearing masks when going out has become a habit for everyone. Currently, masks after use are non-degradable and need to be incinerated, which seriously pollutes the environment. The core layer of the mask is composed of micro-nano melt-blown filter material, which replaces the traditional non-degradable polypropylene resin with degradable polylactic acid PLA, which meets the current needs of social development. However, polylactic acid resin is a high molecular polymer obtained from lactic acid or lactide as a raw material, with a high glass transition temperature and a low crystallization rate. Although the polylactic acid melt-blown filter material is degradable, it is brittle and has poor hand flexibility. It needs to be toughened by physical or chemical methods to improve the mechanical properties of the material.

[0003] "Preparation and Properties of PEG-Toughened Polylactic Acid Melt-Blown Nonwoven Materials" (Dong Yujia et al., Journal of Basic Sciences of Textile Universities, 2022, 35(1), 14-23.) and CN105885374A both mentioned that polyethylene glycol PEG can effectively improve the flexibility of polylactic acid melt-blown materials. The lower the relative molecular weight, the better the toughening effect. Although the addition of low molecular weight PEG significantly reduces the glass transition temperature of PLA, it also reduces the upper limit of the use temperature of PLA and is prone to seepage and loses the toughening effect.

[0004] CN103003360A and “The Effect of Hot Air Temperature on the Structure and Properties of PP / TPU Melt-blown Nonwoven Fabrics” (Peng Mengna et al., Silk, 2018, 55(8), 35-40.) use thermoplastic polyurethane for toughening to improve the flexibility of PLA melt-blown fabrics, but polylactic acid is incompatible with thermoplastic polyurethane, and the toughening effect is limited, requiring the use of a compatibilizer. CN105442187A and “The Structure and Properties of PLA Toughened with PCL of Different Molecular Weights” (Meng Bing et al., Engineering Plastics Application, 2016, 44(5), 107-111.) use biodegradable resin PCL to toughen PLA, but there is obvious phase separation between PLA and PCL, which is not conducive to melt spinning processing. In the study “The Effect of PLA-PCL-PLA on the Compatibility and Spinnability of PLA / PCL Blends for Meltblowing” (Cao Yongmin, Zhejiang Sci-Tech University, Master’s thesis), PLA-PCL-PLA block copolymers were used as compatibilizers. However, these polymers have low glass transition temperatures and softness properties. In high-speed airflow fields, their drawing properties are poor, making it difficult to form meltblown fiber webs.

[0005] CN108440926A and CN103052672A directly graft polylactic acid molecular chains with elastomer molecular chains to improve the flexibility of polylactic acid. However, this chain structure grafting modification will greatly increase the molecular weight and sharply reduce the melt index, which will affect the preparation of polylactic acid melt-blown filter material.

[0006] "Preparation and properties of electret-plasticizer composite modified polylactic acid melt-blown nonwoven materials" (Huang Haichao et al., Journal of Composite Materials, 2019, 36(3), 533-541) and CN103189131A. Adding inorganic nanoparticles can improve the strength, stiffness and toughness of the polymer, but it is related to the fact that they cannot be effectively dispersed in the PLA polymer, and the degree of effective toughening is low.

[0007] The above patent documents or journal documents propose preparation methods of toughened polylactic acid melt-blown filter materials from different angles. The general direction is to use low molecular weight PEG with good compatibility with PLA to toughen, use polymer elastomers or degradable polymers with good toughness to toughen polylactic acid melt-blown filter materials, modify the polylactic acid molecular chain structure by elastic molecular chain grafting to improve the flexibility of polylactic acid filter materials, add nanoparticles to toughen and strengthen polylactic acid melt-blown filter materials, or a combination of these. The first technical problem is that low molecular weight PEG lowers the upper limit of the operating temperature of PLA, and it is easy to seep out of PLA and lose the toughening effect; the second technical problem is that polymer elastomers are incompatible with polylactic acid, and the polymer glass transition temperature and softness properties of toughened PLA are low. Under high-speed airflow field, the drawing performance is poor, and it is more difficult to form a melt-blown fiber web; the third technical problem is that the polylactic acid molecular chain is grafted with elastomer, which affects the preparation of melt-blown filter materials; the fourth technical problem is that although the addition of nanoparticles can improve the strength and toughness of PLA filter materials to a certain extent, they are not easy to be effectively dispersed in the PLA polymer, and the effective toughening degree is low. Summary of the invention

[0008] In view of this, the present application provides a method for preparing a flexible and degradable melt-blown filter material to improve the problem of brittle feel and poor flexibility of the polylactic acid melt-blown filter material.

[0009] Specifically, the present application is implemented through the following scheme:

[0010] A method for preparing a flexible and degradable melt-blown filter material comprises the following steps:

[0011] (1) Synthesis of thermoplastic polyether ester copolymer: using tetrabutyl titanate (TBT) as a catalyst, 1,4-dimethyl phthalate (DMT) and diol are melt-condensed to obtain a hard segment, polyethylene glycol (PEG) and an antioxidant are added, heated under stirring until an ester exchange reaction occurs, and the pressure is reduced to a set value and maintained for a period of time to obtain a thermoplastic polyether ester block copolymer. In the obtained thermoplastic polyether ester block copolymer, the mass fraction of the hard segment is maintained at 20 to 80% (preferably 40 to 80%), the melting point of the copolymer is 180 to 220° C., and the melt index is 20 to 50 g / min;

[0012] (2) preparing composite masterbatch: polylactic acid (PLA) chips, thermoplastic polyetherester block copolymer and hydrophobic nanoparticles are uniformly mixed, melt-extruded, and then cooled and cut to obtain composite masterbatch;

[0013] (3) preparing polylactic acid melt-blown material: melt-extruding, melt-blowing and drawing the composite masterbatch to obtain a micro-nano melt-blown filter material;

[0014] (4) Corona electret melt-blown filter material.

[0015] The above scheme synthesizes a thermoplastic polyether ester copolymer through hard segments and soft segments, and controls the rigidity and flexibility of the copolymer by controlling the type of hard segments and the molecular weight of the soft segments. At the same time, the soft segments can also serve as a compatibilizer for the hard segments, hydrophobic nanoparticles and polylactic acid. The polyether ester copolymer and the hydrophobic nanoparticles synergistically toughen and reinforce the polylactic acid melt-blown filter material, and while improving the tensile strength of the filter material, its tensile elongation at break is increased, thereby improving the flexibility of the filter material and making it have a good hand feel quality.

[0016] Further, as a preference:

[0017] The diol is any one of 1,4-butanediol (BDO), 1,3-propylene glycol (PDO), and ethylene glycol (EG), and the corresponding hard segment is polybutylene terephthalate PBT, polypropylene terephthalate PTT, and polyethylene terephthalate PTT. Correspondingly, the thermoplastic polyether ester block copolymer is PBT-PEG, PTT-PEG, and PET-PEG.

[0018] The hydrophobic nanoparticles are a mixture of any one or more of hydrophobic nano silicon dioxide (SiO2), hydrophobic nano titanium dioxide (TiO2) or hydrophobic nano calcium carbonate (CaCO3), and hydrophobic nano silicon carbide (SiC), with an average nanometer particle size of 15 to 50 nm and a density of 0.1 to 0.2 g / m 3 .

[0019] In step (2), the mass ratio of the polylactic acid slices, the thermoplastic polyether ester copolymer and the hydrophobic nanoparticles is 92-95:2-8:0.2-0.5.

[0020] In step (2), the vacuum drying temperature is 80-100° C. and the drying time is 4-6 hours.

[0021] In step (2), the melting temperature is 200-240°C.

[0022] In step (3), the temperature of the three zones of the melt extruder is 170-240°C, and the extrusion rate of the metering pump is 60-100 cc.min. -1 .

[0023] In step (3), the hot air temperature on both sides of the drafting is 240-270°C, and the drafting fan speed is 1350-1450 r.min. -1 .

[0024] In step (4), the negative electret voltage is 10 to 50 kV, and the electret distance is 2 to 8 cm.

[0025] The present application blends thermoplastic polyether ester copolymer and hydrophobic nanoparticles in polylactic acid slices to improve the brittle feel and poor flexibility of polylactic acid melt-blown filter materials, and develops thermoplastic polyether ester copolymer and hydrophobic nanoparticles synergistically toughened polylactic acid melt-blown filter materials.

[0026] Compared with the previous toughened polylactic acid melt-blown filter material, the advantages of this application are:

[0027] (1) The synthesized thermoplastic polyether ester copolymer, hydrophobic nanoparticles and polylactic acid chips are mixed and granulated, and the polylactic acid melt-blown filter material is prepared by melt-blowing process. The thermoplastic polyether ester copolymer is composed of polyether flexible segments and polyester hard segments. By synthesizing different segment lengths, different toughening effects on the polylactic acid melt-blown filter material are adjusted to solve the problem of easy brittleness of the filter material.

[0028] (2) Polyethylene glycol, as a flexible segment of thermoplastic polyether ester copolymer, has good compatibility with polylactic acid molecular chains and hydrophobic nanoparticles, which helps nanoparticles and hard segments to be effectively dispersed in polylactic acid, and can be used as a compatibilizer for hard segment molecules, nanoparticles and polylactic acid. Hydrophobic nanoparticles, as polylactic acid nucleating agents, can effectively promote the crystallization of polylactic acid and can be used as inorganic toughening and reinforcing agents. At the same time, thermoplastic polyether ester copolymer is a degradable material and does not affect the degradation performance of the matrix polylactic acid. DETAILED DESCRIPTION

[0029] The feasibility of the present application is further verified by specific embodiments below, and the embodiments listed are preferred solutions of the present application, therefore, the present application is not limited to the scope of the embodiments. Anyone who imitates or changes the technical solution and concept of the present application shall be within the protection scope of the present application.

[0030] 1. Raw materials:

[0031] Polylactic acid chips: melt-blown grade polylactic acid, melt index 75g / 10min, melting point 165℃, glass transition temperature 60℃, relative molecular mass 2.5×10 5 , density 1.25g / m 3 .

[0032] 1,4-Dimethyl phthalate: molecular weight 194.18, purity 99%, Aladdin reagent.

[0033] 1,4-Butanediol, 1,3-Propanediol, Ethylene glycol: All are analytical grade, 98%, Aladdin reagent.

[0034] Tetrabutyl titanate: purity ≥99%, condensation catalyst, Aladdin reagent.

[0035] Polyethylene glycol: flexible chain segment, number average molecular weight 400-4000, analytical grade, Aladdin reagent.

[0036] Hydrophobic nanoparticles: hydrophobic nano-silicon dioxide (SiO2), hydrophobic nano-titanium dioxide (TiO2) or hydrophobic nano-calcium carbonate (CaCO3), hydrophobic nano-silicon carbide (SiC), with an average particle size of 15-50nm and a density of 0.1-0.2g / m 3 .

[0037] Antioxidant: Hindered phenol antioxidant Irgafox 1010 or 1076, phosphite antioxidant Irgafos168, white powder, melting point <190°C, reagent from Ciba Fine Chemicals Co., Ltd., Switzerland.

[0038] 2. Test:

[0039] According to GB / T 24218.3-2010 standard, the sample is cut along the longitudinal direction (MD) and transverse direction (CD). The sample width is 50mm±0.5mm, the length clamping distance is 200mm, and the sample is stretched at a constant elongation speed of 100mm / min until it breaks. The sample breaking strength and elongation at break are recorded.

[0040] Example 1

[0041] The preparation process of the melt-blown filter material of this embodiment is as follows:

[0042] (1) DMT, 1,4-butanediol, and tetrabutyl titanate (catalyst, 0.2%wt DMT) were placed in a reaction kettle, purged with nitrogen, heated to 190°C, and stirred for 2 hours to melt-polycondense to obtain PBT.

[0043] (2) PEG (Mn = 1000) was added to the reactor system, the mass ratio of PBT to PEG was 3:2 (i.e., the mass fraction of the hard segment was 60%), and an antioxidant (0.4% relative to the mass of the PBT / PEG system) was added. The mixture was slowly heated to a certain temperature (about 235°C) under continuous stirring to undergo an ester exchange reaction. The pressure in the reactor was then reduced to below 50 Pa and maintained for 6 hours to obtain a thermoplastic polyetherester block copolymer PBT-PEG.

[0044] (3) 93.7 parts by weight of polylactic acid chips were dried at 80°C for 8 h, and 6 parts by weight of PBT-PEG block copolymer and 0.3 parts by weight of hydrophobic nano-titanium dioxide (average particle size 30 nm, density 0.15 g / m) were added. 3 ) is dried at 80°C for 3h, and then the dried polylactic acid and additives are crushed in a high-speed crusher and fully mixed in a high-speed stirring mixer at a temperature of 80°C. The mixed materials are then put into a twin-screw granulator for melt extrusion, and are cut after being cooled in a water bath to obtain polylactic acid composite masterbatch.

[0045] (4) The polylactic acid composite masterbatch was vacuum dried at 80°C for 2 h and then fed into the melt-blown equipment. The process parameters for preparing the melt-blown filter material are shown in Table 1.

[0046] (5) The modified polylactic acid melt-blown filter material was subjected to electret treatment by the method of positive and negative corona electret, the electret cathode voltage was 30 kV, and the electret distance was 4 cm. Thus, a flexible polylactic acid melt-blown filter material 1# was obtained.

[0047] The longitudinal breaking strength of filter material 1# is 24.08N / 5cm, and the transverse breaking strength is 17.97N / 5cm; the longitudinal breaking elongation is 18.61%, and the transverse breaking elongation is 13.86%.

[0048] Table 1: Meltblown filter material process parameter settings

[0049]

[0050] Example 2

[0051] This embodiment is configured the same as that of embodiment 1, except that the molecular weight Mn of the added PEG is different.

[0052] Table 2: Effect of different PEG molecular weights on filter media strength and toughness

[0053]

[0054]

[0055] It can be seen from Table 2 that as the PEG molecular weight increases, the breaking strength decreases, while the elongation increases slightly; when the PEG molecular weight is controlled in the range of 1000 to 3000, the breaking strength and breaking elongation are better.

[0056] Example 3

[0057] The configuration of this embodiment is the same as that of embodiment 1, except that the mass ratio of the hard segments is different.

[0058] Table 3: Effect of the hard segment mass ratio in thermoplastic polyetherester block copolymers on filter media

[0059]

[0060]

[0061] As can be seen from Table 3, with the increase of the amount of hard segments, the breaking strength increases significantly and the breaking elongation decreases. When no hard segments are added (serial number 3-10), the breaking strength is the lowest and the elongation is the highest. The mass ratio of the hard segments in the thermoplastic polyetherester block copolymer is preferably controlled at 40-80%.

[0062] Example 4

[0063] The configuration of this embodiment is the same as that of embodiment 1, except that: in step (1), ethylene glycol is used as the diol, and PET is obtained by melt polycondensation; in step (2), the Mn of PEG is 3000, and the mass ratio of PET to PEG is 7:3; in step (3), the raw material ratio is: 92.7 parts by mass of polylactic acid chips, 7 parts by mass of PET-PEG block copolymer, and 0.3 parts by mass of hydrophobic nano-titanium dioxide, to obtain toughened polylactic acid melt-blown filter material 2#.

[0064] The longitudinal breaking strength of filter material 2# is 28.31N / 5cm, and the transverse breaking strength is 20.90N / 5cm; the longitudinal breaking elongation is 22.40%, and the transverse breaking elongation is 18.37%.

[0065] By comparing the above-mentioned Examples 1 to 4, it can be seen that the longitudinal and transverse breaking strengths of the melt-blown filter material prepared in this case are slightly increased, and the breaking elongation is significantly increased.

[0066] Comparative Example 1

[0067] The configuration of this comparative example is the same as that of Example 1, except that in step (2), the Mn of the added PEG is 1600; in step (3), the raw material ratio is: 93 parts of polylactic acid chips and 7 parts of PBT-PEG block copolymer. The resulting filter material is recorded as comparative 1#.

[0068] In comparison, the longitudinal breaking strength of 1# is 18.92N / 5cm, and the transverse breaking strength is 13.85N / 5cm; the longitudinal breaking elongation is 16.37%, and the transverse breaking elongation is 13.63%.

[0069] Comparing Example 2 (the solution corresponding to 2-2 in Table 2) with Comparative Example 1, when no hydrophobic nanoparticles were added, the breaking strength decreased and the breaking elongation decreased slightly.

[0070] Comparative Example 2

[0071] In this comparative example, no block copolymer is added, and 99.7 parts of polylactic acid chips and 0.3 parts of hydrophobic nano-silicon carbide are directly used as raw materials to perform the same extrusion melting, melt blowing, and corona electret charging as in Example 1 to obtain polylactic acid melt-blown filter material comparison 2#.

[0072] In comparison, the longitudinal breaking strength of 2# is 14.32N / 5cm, and the transverse breaking strength is 9.41N / 5cm; the longitudinal breaking elongation is 10.64%, and the transverse breaking elongation is 8.96%.

[0073] It can be seen from Comparative Example 2 that when only hydrophobic nanoparticles are added to the raw materials of the filter material without adding the thermoplastic polyetherester block copolymer, the breaking strength and elongation of the sample are both relatively low.

[0074] Comparative Example 3

[0075] In this comparative example, no additives were added, and polylactic acid slices were directly used as raw materials. They were dried at 80°C for 2 hours and then fed into the melt-blown equipment. The process parameters for preparing the melt-blown filter material are shown in Table 1. The modified polylactic acid melt-blown filter material was subjected to electret treatment by the positive and negative corona electret method. The electret cathode voltage was 30 kV and the electret distance was 4 cm. The polylactic acid melt-blown filter material comparison 3# was obtained.

[0076] In comparison, the longitudinal breaking strength of 3# is 12.72N / 5cm, and the transverse breaking strength is 8.76N / 5cm; the longitudinal breaking elongation is 10.45%, and the transverse breaking elongation is 8.81%.

[0077] Comparing Comparative Example 3 with Comparative Example 2, when the raw materials of the filter material are not added, the breaking strength decreases and the breaking elongation does not change much, indicating that the hydrophobic nanoparticles can slightly improve the strength of the material, which also verifies the rationality of the above conclusions of Examples 1 to 4 and Comparative Examples 1 to 3.

Claims

1. A method for preparing a flexible and degradable melt-blown filter material, It is characterized in that The following steps are involved: (1) Synthesis of thermoplastic polyether ester copolymer: Using tetrabutyl titanate as a catalyst, 1,4-dimethyl phthalate and diol are melt-condensed to obtain a hard segment, and then polyethylene glycol and an antioxidant are added. The mixture is heated under stirring until an ester exchange reaction occurs, and the pressure is reduced to a set value and maintained for a period of time to obtain a thermoplastic polyether ester block copolymer. In the obtained thermoplastic polyether ester block copolymer, the mass fraction of the hard segment is maintained at 20-80%; (2) Preparation of composite masterbatch: polylactic acid chips, thermoplastic polyether ester block copolymer and hydrophobic nanoparticles are mixed evenly, vacuum dried, melt extruded, cooled and cut to obtain composite masterbatch; (3) Preparation of polylactic acid melt-blown material: melt extrusion, melt-blowing and drawing of the composite masterbatch to obtain a micro-nano melt-blown filter material; (4) Corona electret melt-blown filter material.

2. A method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: The diol is any one of 1,4-butanediol, 1,3-propylene glycol and ethylene glycol.

3. The method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: The mass fraction of the hard segment is maintained at 40~80%.

4. A method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: The hydrophobic nanoparticles are a mixture of any one or more of hydrophobic nano-silicon dioxide, hydrophobic nano-titanium dioxide, hydrophobic nano-calcium carbonate, and hydrophobic nano-silicon carbide.

5. A method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: In step (2), the mass ratio of the polylactic acid slices, the thermoplastic polyether ester copolymer and the hydrophobic nanoparticles is 92-95:2-8:0.2-0.

5.

6. The method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: In step (2), the vacuum drying temperature is 80-100 °C and the drying time is 4-6 h.

7. The method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: In step (2), the melting temperature is 200-240°C.

8. The method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: In step (3), the temperature of the melt extruder is 170-240 °C, and the extrusion rate of the metering pump is 60-100 cc.min. -1 .

9. The method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: In step (3), the hot air temperature on both sides of the drawing is 240~270℃, and the drawing fan speed is 1350~1450 r.min -1 .

10. The method for preparing a flexible and degradable melt-blown filter material according to claim 1, Features: In step (4), the negative electret voltage is 10~50 kV and the electret distance is 2~8 cm.

Citation Information

Patent Citations

  • Toughened polylactic acid and preparation method of same

    CN103194052A

  • Degradable melt-blown filter material as well as preparation method and application thereof

    CN114108127A

  • Modifier for polylactic acid resin

    JP2008163220A

  • Polyether ester block copolymer resin composition and manufacturing method thereof

    KR1019980027483A