Composite pipe and preparation method thereof

By using silane coupling agent-modified metal oxide filler in the outer tube of the composite tube to react with hydrogen sulfide, the problem of hydrogen sulfide permeation in oil and gas transportation is solved, and safety and reliability are improved.

CN118935105APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310532865.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the oil and gas transportation of existing composite pipes, hydrogen sulfide gas is prone to penetrate, resulting in the risk of hydrogen sulfide poisoning accidents.

Method used

A composite tube is designed, in which the outer tube is added with a metal oxide filler modified with silane coupling agent, which can react chemically with hydrogen sulfide, absorb and stabilize hydrogen sulfide gas, thereby avoiding its leakage.

Benefits of technology

It effectively avoids the penetration of hydrogen sulfide gas, reduces the risk of poisoning, and reminds maintenance personnel to carry out maintenance through color changes in the outer tube, improving safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118935105A_ABST
    Figure CN118935105A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oil and gas transmission pipelines, and discloses a composite pipe and a preparation method thereof.The composite pipe comprises a lining layer, a reinforcing layer and an outer pipe which are sequentially arranged from inside to outside; the outer tube contains medium density polyethylene, a filler, a compatilizer and an optional additive, the filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can chemically react with hydrogen sulfide. By adding the filler, when hydrogen sulfide gas permeates into the outer pipe, the filler reacts with the hydrogen sulfide gas to generate a stable harmless substance (metal sulfide), so that the hydrogen sulfide gas is absorbed, and the phenomenon of hydrogen sulfide aggregation is avoided; meanwhile, the outer surface of the composite pipe can be discolored by the generated metal sulfide, so that hydrogen sulfide in the composite pipe is prompted to permeate into the outer pipe, and safety accidents such as hydrogen sulfide poisoning are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil and gas transmission pipelines, and in particular to a composite pipe and a preparation method thereof. Background Art

[0002] With the development of oil and gas resources, fiber reinforced composite pipe (RTP) is widely used in the field of oil and gas gathering and transportation due to its advantages such as light weight, flexible coiling and corrosion resistance. RTP pipe is usually composed of three layers: an inner lining layer made of polymer material, a reinforcement layer made of continuous fiber material, and an outer pipe made of anti-aging and impact thermoplastic plastic. The main function of the inner lining layer is to seal and transport materials to prevent leakage; the main function of the reinforcement layer is to provide the required pressure bearing capacity of the pipe body; the main function of the outer pipe is to protect the entire pipe body.

[0003] The lining material of RTP pipe is generally made of high-density polyethylene (HDPE). HDPE has good anti-seepage performance against water vapor. However, oil and gas gathering and transportation are usually medium- and high-pressure oil and gas, which often contain small molecules such as oxygen, carbon dioxide, hydrogen sulfide, and methane, which are easily permeable media. In high-pressure oil and gas, HDPE has poor anti-seepage performance against oxygen, carbon dioxide, hydrogen sulfide, methane and other gases in oil and gas, which makes it easy for these small molecules to penetrate outside the composite pipe. If hydrogen sulfide penetrates from the composite pipe and gathers, it is easy to cause hydrogen sulfide poisoning accidents. Therefore, it is of great significance to develop a composite pipe that can avoid hydrogen sulfide poisoning. Summary of the invention

[0004] The purpose of the present invention is to provide a composite pipe and a preparation method thereof to overcome the problem that hydrogen sulfide gas easily permeates out of the composite pipe during oil and gas transportation in the prior art, causing hydrogen sulfide poisoning accidents.

[0005] In order to achieve the above object, the present invention provides a composite pipe on one hand, the composite pipe comprises an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside;

[0006] The outer tube contains medium density polyethylene, filler, compatibilizer and optional additives,

[0007] The filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can react chemically with hydrogen sulfide.

[0008] Preferably, based on the total weight of the outer tube, the content of the polyethylene is 85-97wt%, the content of the filler is 2-10wt%, the content of the compatibilizer is 1-4wt%, and the content of the additive is 0-1wt%.

[0009] Preferably, the metal oxide is nano zinc oxide and / or nano iron oxide;

[0010] Preferably, the nano zinc oxide is a tetrapod-shaped zinc oxide whisker.

[0011] Preferably, the filler is prepared according to the following process:

[0012] Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 4 to 5.5 and reacting to obtain a coupling agent solution;

[0013] The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.

[0014] Preferably, the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25.

[0015] Preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1.

[0016] Preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:10-100.

[0017] Preferably, the melt index of the medium density polyethylene in the outer tube is 0.5 to 0.7 g / 10 min.

[0018] Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high-density polyethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.

[0019] Preferably, the additive is selected from one or more of an anti-ultraviolet agent, a plasticizer, an antioxidant and a flame retardant.

[0020] Preferably, the inner lining layer contains high-density polyethylene a and antibacterial barrier material,

[0021] The antibacterial barrier material contains high-density polyethylene b, modified nanofiller, antibacterial agent and a first auxiliary agent, wherein the modified nanofiller is obtained by modifying the sheet-like nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.

[0022] Preferably, based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%.

[0023] Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite.

[0024] Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.

[0025] Preferably, the modified nanofiller is prepared according to the following process:

[0026] S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture;

[0027] S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.

[0028] Preferably, in step S10, the weight ratio of the flaky nanofiller to water is 1:25-50;

[0029] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20.

[0030] Preferably, the melt index of the high-density polyethylene b is 0.3-0.5 g / 10 min.

[0031] Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide.

[0032] Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.

[0033] Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.

[0034] Preferably, the antibacterial barrier material is prepared according to the following process: high-density polyethylene, modified nanofiller, antibacterial agent and first auxiliary agent are blended and extruded.

[0035] Preferably, the blending extrusion is carried out in a twin-screw extruder.

[0036] Preferably, the operating temperature of the twin-screw extruder is 160-200° C., and the operating speed is 300-350 r / min.

[0037] Preferably, based on the total weight of the inner lining layer, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%.

[0038] Preferably, the high-density polyethylene a and the high-density polyethylene b are the same.

[0039] Preferably, the inner lining layer further contains a second auxiliary agent, and the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent.

[0040] Preferably, in the inner lining layer, the content of the second auxiliary agent is 1-2 wt %.

[0041] A second aspect of the present invention provides a method for preparing the composite pipe as described above, the method comprising the following steps:

[0042] A1, blending and extruding the antibacterial barrier material and high-density polyethylene a to obtain an inner lining layer;

[0043] A2, cross-winding the continuous fiber prepreg tape at an angle of 40 to 65 degrees with the axis of the inner liner layer on the outside of the inner liner layer to obtain a reinforcement layer;

[0044] A3. Blending and extruding medium-density polyethylene, fillers, compatibilizers and optional additives through an extruder, and coating the mixture on the outside of the reinforcement layer.

[0045] Preferably, in step A1, the blending extrusion is carried out in a twin-screw extruder.

[0046] Preferably, in step A1, the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 110-130°C, the temperature of zone two is 140-160°C, and the temperature of zone three is 180-200°C.

[0047] Preferably, in step A1, the head temperature of the twin-screw extruder is 165-185°C.

[0048] Preferably, in step A3, the extruder is a twin-screw extruder, the operating speed of the twin-screw extruder is 300-350r / min, the working time is 3-6min, and the working temperature is divided into three sections along the material flow direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.

[0049] In the present invention, the outer tube is made of medium-density polyethylene, fillers, compatibilizers and optional additives as raw materials, wherein the fillers contain metal oxides modified by silane coupling agents. By adding fillers, when hydrogen sulfide gas penetrates into the outer tube, the fillers react with the hydrogen sulfide gas to generate stable harmless substances (metal sulfides), so that the hydrogen sulfide gas is absorbed, thereby preventing hydrogen sulfide from leaking out of the tube; at the same time, the generated metal sulfides can cause the outer surface of the composite tube to change color, thereby indicating that hydrogen sulfide in the composite tube has penetrated into the outer tube, thereby avoiding safety accidents such as hydrogen sulfide poisoning. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 is a schematic structural diagram of a composite tube obtained in Example 5 of the present invention;

[0051] Figure 2 Schematic diagram of the microscopic morphology of the inner lining layer prepared in Comparative Example 8 of the present invention;

[0052] Figure 3 It is a schematic diagram of the microscopic morphology of the lining layer prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0053] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0054] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0055] The present invention provides a composite pipe, which comprises an inner lining layer, a reinforcement layer and an outer pipe which are arranged in sequence from the inside to the outside; the outer pipe contains medium-density polyethylene, a filler, a compatibilizer and optional additives, wherein the filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can react chemically with hydrogen sulfide.

[0056] In a preferred embodiment, based on the total weight of the outer tube, the content of the polyethylene is 85-97wt%, the content of the filler is 2-10wt%, the content of the compatibilizer is 1-4wt%, and the content of the additive is 0-1wt%.

[0057] In order to make the outer tube absorb hydrogen sulfide gas better, in the present invention, the metal oxide is nano zinc oxide and / or nano iron oxide, wherein the nano zinc oxide is preferably tetrapod-shaped zinc oxide whisker.

[0058] In the outer tube of the present invention, the filler is prepared according to the following process:

[0059] Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 4 to 5.5 and reacting to obtain a coupling agent solution;

[0060] The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.

[0061] The filler prepared by the above process has good dispersibility in polyethylene, so it can better play its role, thereby making the outer tube absorb hydrogen sulfide gas with good effect.

[0062] Further preferably, the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25, specifically, for example, 1:15, 1:17, 1:19, 1:20, 1:22, 1:23 or 1:25.

[0063] Further preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1, specifically, for example, 2:1, 2.2:1, 2.5:1, 2.7:1, 3:1, 3.5:1 or 4:1, most preferably 3:1.

[0064] Further preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:10-100, preferably 1:20-80, specifically, for example, 1:20, 1:30, 1:35, 1:40, 1:50, 1:60, 1:70 or 1:80.

[0065] More preferably, the activation temperature is 140-160° C. and the activation time is 6-10 h.

[0066] In a preferred embodiment, the melt index of the medium density polyethylene in the outer tube is 0.5 to 0.7 g / 10 min.

[0067] In the outer tube of the present invention, the compatibilizer is selected from one or more of maleic anhydride grafted high-density polyethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.

[0068] In the outer tube of the present invention, the additive is selected from one or more of an anti-ultraviolet agent, a plasticizer, an antioxidant and a flame retardant.

[0069] In a preferred embodiment, the inner lining layer contains high-density polyethylene a and an antibacterial barrier material, wherein the antibacterial barrier material contains high-density polyethylene b, a modified nanofiller, an antibacterial agent and a first auxiliary agent, wherein the modified nanofiller is a sheet-like nanofiller modified by a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer. Preferably, the first auxiliary agent is a coupling agent and a compatibilizer.

[0070] In a preferred embodiment, based on the total weight of the inner lining material (i.e., based on the total weight of the raw materials for preparing the inner lining material), the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%. More preferably, based on the total weight of the inner lining material, the content of the high-density polyethylene a is 85-95wt%, and the content of the antibacterial barrier material is 5-15wt%.

[0071] The present invention improves the dispersibility of the flaky nanofillers in high-density polyethylene (including high-density polyethylene a and high-density polyethylene b) by modifying the flaky nanofillers, so that the flaky nanofillers can better improve the gas barrier properties of the antibacterial barrier material; by adding the first auxiliary agent, the compatibility of the high-density polyethylene and the modified nanofillers is improved, so that the high-density polyethylene can better combine with the modified nanofillers, thereby avoiding the "debonding" phenomenon of the modified nanofillers; at the same time, the addition of the first auxiliary agent can also improve the bonding between the lining layer material and the reinforcement layer material, thereby improving its resistance to interlayer delamination.

[0072] The present invention improves the dispersibility of the antibacterial agent in high-density polyethylene by adding the modified nano filler and the first auxiliary agent, so that the antibacterial agent can better exert its antibacterial performance, thereby preventing bacteria in the oil and gas production fluid from adhering to the pipe wall.

[0073] In the present invention, based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%.

[0074] In a preferred embodiment, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite, and these flaky nanofillers have an aspect ratio, which makes them more dispersible in polyethylene. Specifically, the kaolin includes hydrated kaolin and anhydrous kaolin.

[0075] If the flaky nanofiller is added directly, it is easy to agglomerate, so that the flaky nanofiller cannot be distributed in the polyethylene in a flaky manner, thereby making the gas barrier property of the liner material poor. The present invention further improves its dispersibility in the resin matrix by modifying the flaky nanofiller. In a preferred embodiment, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, more preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.

[0076] In a preferred embodiment, the modified nanofiller is prepared according to the following process:

[0077] Step S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture;

[0078] Step S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid from the solid-liquid, and then washing, drying, grinding and sieving the obtained solid.

[0079] Wherein, in step S10, the weight ratio of the flaky nanofiller to water is 1:25-50, specifically, for example, 1:25, 1:30, 1:33, 1:35, 1:40, 1:45 or 1:50.

[0080] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20, specifically, for example, 1:10, 1:12, 1:15, 1:17, 1:18 or 1:20.

[0081] In a specific embodiment, step S20 includes: adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then mixing with a cationic surfactant and adjusting the pH value to 6.8-7.5, reacting for 2-4 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3-5 times, then drying at 70-90° C. for 30-50 hours, and finally grinding and sieving.

[0082] In a preferred embodiment, the melt index of the high-density polyethylene b is 0.3 to 0.5 g / 10 min, more preferably 0.35 to 0.45 g / 10 min.

[0083] The present invention does not limit the specific type of the antibacterial agent, which can be a conventional inorganic antibacterial agent, preferably nano copper oxide and / or nano silver oxide, more preferably nano copper oxide and nano silver oxide. Further preferably, the antibacterial agent is modified with a silane coupling agent before use. Specifically, the modification method includes: mixing the silane coupling agent and an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1) in a volume ratio of 1:15 to 25, dripping a hydrochloric acid solution to adjust the pH value to 3.5 to 5, hydrolyzing at room temperature for 1 to 2 hours to obtain a mixed solution, adding the antibacterial agent to the mixed solution, and then ultrasonically dispersing in a constant temperature water bath at 40 to 60°C, while mechanically stirring, reacting for 2 to 4 hours, and then filtering the reactant, washing with deionized water until there is no chloride ion, vacuum drying, activating at 140 to 160°C for 6 to 10 hours, grinding, sieving, and obtaining a modified antibacterial agent. Wherein, the weight ratio of the silane coupling agent to the antibacterial agent is 1:10-100.

[0084] In the inner liner of the present invention, the compatibilizer is selected from one or more of maleic anhydride grafted high-density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.

[0085] In the inner lining layer of the present invention, the coupling agent is a silane coupling agent and / or a titanate coupling agent.

[0086] In order to improve the antibacterial and gas barrier properties of the lining material, in a preferred embodiment, the antibacterial barrier material is prepared according to the following process: high-density polyethylene, modified nanofiller, antibacterial agent and first auxiliary agent are co-blended and extruded.

[0087] In the present invention, by firstly co-extruding high-density polyethylene b, modified nanofiller, antibacterial agent and the first auxiliary agent to form an antibacterial barrier material, and then preparing an inner lining layer with high-density polyethylene a (matrix), the dispersibility of the nanofiller and the antibacterial agent in the high-density polyethylene can be further improved, and the modified nanofiller and the antibacterial agent can be evenly dispersed in the high-density polyethylene, thereby making the gas barrier and antibacterial properties of the inner lining layer excellent.

[0088] Further preferably, when preparing the antibacterial barrier material, the co-extrusion is carried out in a twin-screw extruder. The working temperature of the twin-screw extruder is 160-200°C, the working speed is 300-350r / min, and the working time is 3-6min. Specifically, the working temperature of the twin-screw extruder is divided into three sections along the screw extrusion direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.

[0089] In order to improve the processability, flame retardancy and service life of the inner lining material, in a preferred embodiment, the inner lining material also contains a second auxiliary agent, which is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent.

[0090] Furthermore, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.

[0091] In a preferred embodiment, in the inner lining material, the content of the high-density polyethylene a is 85-95wt%, the content of the antibacterial barrier material is 4-14wt%, and the content of the second auxiliary agent is 1-2wt%. In this way, the overall performance of the obtained inner lining material is better.

[0092] In a preferred embodiment, the high-density polyethylene a and the high-density polyethylene b may be the same or different, and are preferably the same for better compatibility and ease of operation.

[0093] In the composite pipe described in the present invention, the resin matrix of the inner lining layer is high-density polyethylene, and the resin matrix of the outer pipe is medium-density polyethylene. The permeability of the outer pipe is higher than that of the inner lining layer material. The composite pipe forms a structure with gradually decreasing gas barrier properties from the inside to the outside, making it easier for the gas that penetrates into the interior of the composite pipe to penetrate outward from the pipe, thereby avoiding the accumulation of gas that penetrates into the pipe inside the pipe and causing interlayer delamination.

[0094] The composite pipe can be used for transporting high-pressure oil and gas, and the high-pressure oil and gas contain produced fluid.

[0095] In the composite pipe of the present invention, the thickness of the inner lining layer is 2 to 10 mm.

[0096] In the composite pipe described in the present invention, the reinforcement layer is made of a continuous fiber reinforced resin prepreg tape. The continuous fiber reinforced resin prepreg tape is made of a mixed material of one or more continuous fibers selected from glass fiber, aramid fiber, and carbon fiber and a lining layer high molecular weight polyolefin (matrix) consistent material through a prepreg process. The reinforcing resin in the reinforcement layer has good bonding properties with the lining layer, and reliable bonding, so that the reinforcement layer and the lining layer are integrated, the anti-peeling performance between the reinforcement layer and the lining layer is improved, and the winding defects between the reinforcement layer and the lining layer are effectively avoided, thereby reducing the possibility of delamination of the lining layer and the reinforcement layer caused by the accumulation of oil and gas in the defective parts after the pipeline penetrates into the pipe body; at the same time, since the lining layer material and the reinforcement layer material are of the same type, the thermal shrinkage rate is almost the same, and the internal stress formed inside the pipe wall by the temperature change of the pipeline is small, the pressure-bearing capacity of the composite pipe can be greatly improved, and the probability of damage to the composite pipe is reduced.

[0097] In the composite tube of the present invention, the thickness of the outer tube is 2 to 4 mm.

[0098] When the composite pipe described in the present invention is used to transport medium and high pressure oil and gas, the hydrogen sulfide gas in the oil and gas can first be blocked by the inner lining layer with high gas barrier properties, and can also be further absorbed by the outer pipe. Through the joint action of the inner lining layer and the outer pipe, the hydrogen sulfide gas in the oil and gas is prevented from penetrating out of the composite pipe; in addition, when the hydrogen sulfide gas penetrates into the outer pipe, the hydrogen sulfide gas and the metal oxide in the outer pipe generate colored sulfides, which changes the color of the outer pipe, thereby playing a warning role, reminding the staff to inspect or replace the inner lining layer, thereby avoiding safety accidents such as hydrogen sulfide poisoning.

[0099] The present invention also provides a method for preparing a composite pipe, which comprises the following steps:

[0100] Step A1, blending and extruding the antibacterial barrier material and high-density polyethylene a to obtain an inner lining layer;

[0101] Step A2, cross-winding the continuous fiber prepreg tape on the outer side of the inner lining layer at an angle of 40 to 65 degrees with the axis of the inner lining layer to obtain a reinforcement layer;

[0102] Step A3: blending and extruding the medium-density polyethylene, filler, compatibilizer and optional additives through an extruder, and coating the mixture on the outside of the reinforcement layer.

[0103] In the method described in the present invention, the blending extrusion operation in step A1 is carried out in a twin-screw extruder; wherein the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 110-130°C, the temperature of zone two is 140-160°C, and the temperature of zone three is 180-200°C.

[0104] Furthermore, in step A1, the die head temperature of the twin-screw extruder is 165-185° C. Specifically, the die head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 175-185° C., and the die temperature is 165-175° C.

[0105] In the method of the present invention, in step A1, based on the total weight of the raw materials for preparing the inner lining material, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%. More preferably, based on the total weight of the inner lining material, the content of the high-density polyethylene a is 85-95wt%, and the content of the antibacterial barrier material is 5-15wt%.

[0106] In the inner liner prepared by the method of the present invention, the modified nano filler and the antibacterial agent are uniformly dispersed in the HDPE, and the HDPE matrix tightly wraps the modified nano filler and the antibacterial agent particles without holes. Compared with the inner liner made of pure HDPE, the gas permeability of the inner liner is reduced by about 100 times, which essentially reduces the total amount of gas infiltrating into the composite pipe. At the same time, the inner liner has excellent antibacterial properties against bacteria in oil and gas.

[0107] In the method of the present invention, in step A2, the number of winding layers of the reinforcing layer is determined according to the pressure level of the composite pipe. Specifically, the number of winding layers can be an even number of 2 to 20 layers, and the calculation method of the number of winding layers refers to SY 6662.2.

[0108] In the method described in the present invention, in step A3, the extruder is a twin-screw extruder, the operating speed of the twin-screw extruder is 300-350r / min, the working time is 3-6min, and the working temperature is divided into three sections along the material flow direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.

[0109] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0110] Example 1

[0111] This embodiment is used to illustrate the outer tube in the composite tube of the present invention and the preparation method thereof.

[0112] 1. Preparation of fillers

[0113] A silane coupling agent (vinyl triethoxysilane) and an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1) are mixed and stirred, the pH of the obtained mixed solution is adjusted to 4-5.5, and hydrolyzed at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15;

[0114] Adding metal oxide (the metal oxide includes four-needle zinc oxide whiskers and nano iron oxide in a weight ratio of 1:1) to the coupling agent solution, and then ultrasonically dispersing at 50°C while mechanically stirring, reacting for 3 hours, filtering the obtained reaction solution, and then washing the obtained solid phase with deionized water until there is no chloride ion, vacuum drying, and then activating at 150°C for 8 hours, grinding, and sieving to obtain a nano-scale filler, wherein the weight ratio of the silane coupling agent to the metal oxide is 1:20.

[0115] 2. Preparation of outer tube

[0116] A31. Weigh the raw material components according to the following weight percentages: 89.6 wt% of medium-density polyethylene, 8 wt% of filler, 2 wt% of compatibilizer, and 0.4 wt% of additives, wherein the medium-density polyethylene is of grade SP988 and has a melt index of 0.6 g / 10 min; the compatibilizer is maleic anhydride-grafted high-density polyethylene; the additive is a UV inhibitor (2-hydroxy-4-octyloxybenzophenone), a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and a flame retardant (diethylaluminum hypophosphite), which are mixed in a weight ratio of 1:1:1:1;

[0117] A32. Add the weighed medium-density polyethylene, filler, compatibilizer and additives into a twin-screw extruder, heat the screw extruder, and mix in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section and a third section. The temperature of the first section is 160° C., the temperature of the second section is 175° C., and the temperature of the third section is 185° C. The extruder speed of the twin-screw extruder is 300 r / min, and the total residence time of the liner material in the twin-screw extruder is 5 min. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an outer tube.

[0118] Example 2

[0119] This embodiment is used to illustrate the outer tube in the composite tube of the present invention and the preparation method thereof.

[0120] 1. Preparation of fillers

[0121] A silane coupling agent (vinyl triethoxysilane) and an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1) are mixed and stirred, the pH of the obtained mixed solution is adjusted to 4-5.5, and hydrolyzed at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15.

[0122] Adding metal oxide (four-needle zinc oxide whisker) to the coupling agent solution, then ultrasonically dispersing at 50° C. and mechanically stirring, reacting for 3 hours, filtering the obtained reaction solution, then washing the obtained solid phase with deionized water until there is no chloride ion, vacuum drying, then activating at 140° C. for 10 hours, grinding, and sieving to obtain a nano-scale filler, wherein the weight ratio of the silane coupling agent to the metal oxide is 1:20;

[0123] 2. Preparation of outer tube

[0124] A31. Weigh the raw material components according to the following weight percentages: 96 wt% of medium-density polyethylene, 3 wt% of filler, 1.6 wt% of compatibilizer, and 0.4 wt% of additives; wherein the medium-density polyethylene is of grade SP988 and has a melt index of 0.6 g / 10 min; the compatibilizer is maleic anhydride-grafted high-density polyethylene; the additive is a UV inhibitor (2-hydroxy-4-octyloxybenzophenone), a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and a flame retardant (diethylaluminum hypophosphite), which are mixed in a weight ratio of 1:1:1:1; the preparation method of the outer tube comprises the following steps:

[0125] A32. Add the medium-density polyethylene, filler, compatibilizer and additives weighed above into a twin-screw extruder, heat the screw extruder, and mix in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section and a third section. The temperature of the first section is 160° C., the temperature of the second section is 175° C., and the temperature of the third section is 185° C. The extruder speed of the twin-screw extruder is 300 r / min, and the total residence time of the liner material in the twin-screw extruder is 5 min. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an outer tube.

[0126] Example 3

[0127] This embodiment is used to illustrate the outer tube in the composite tube of the present invention and the preparation method thereof.

[0128] 1. Preparation of fillers

[0129] A silane coupling agent (vinyl triethoxysilane) and an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1) are mixed and stirred, the pH of the obtained mixed solution is adjusted to 4-5.5, and hydrolyzed at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:20.

[0130] Adding metal oxide (the metal oxide includes four-needle zinc oxide whiskers and nano iron oxide in a weight ratio of 2:1) to the coupling agent solution, and then ultrasonically dispersing at 50° C. and mechanically stirring, reacting for 3 hours, filtering the obtained reaction solution, and then washing the obtained solid phase with deionized water until there is no chloride ion, vacuum drying, and then activating at 150° C. for 8 hours, grinding, and sieving to obtain a nano-scale filler, wherein the weight ratio of the silane coupling agent to the metal oxide is 1:30;

[0131] 2. Preparation of outer tube

[0132] A31. Weigh the raw material components according to the following weight percentages: 87 wt% of medium-density polyethylene, 8 wt% of filler, 4 wt% of compatibilizer, and 1 wt% of additive; wherein the grade of medium-density polyethylene is SP988, and the melt index is 0.6 g / 10 min; the compatibilizer is maleic anhydride grafted high-density polyethylene; the additive is an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone), a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and a flame retardant (diethylaluminum hypophosphite), which are mixed in a weight ratio of 1:2:1;1;

[0133] A32. Add the weighed medium-density polyethylene, filler, compatibilizer and additives into a twin-screw extruder, heat the screw extruder, and mix in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section and a third section. The temperature of the first section is 160° C., the temperature of the second section is 175° C., and the temperature of the third section is 185° C. The extruder speed of the twin-screw extruder is 300 r / min, and the total residence time of the liner material in the twin-screw extruder is 5 min. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an outer tube.

[0134] Example 4

[0135] The method of Example 1 is carried out, except that the outer tube does not contain additives;

[0136] Specifically, step A31 includes:

[0137] The raw material components were weighed according to the following weight percentages: 90 wt% of medium-density polyethylene, 8 wt% of filler, and 2 wt% of compatibilizer.

[0138] Example 5

[0139] This embodiment is used to illustrate the composite tube and the preparation method thereof according to the present invention.

[0140] The composite pipe comprises an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside;

[0141] In this embodiment, high-density polyethylene a and high-density polyethylene b are the same, and the grade is YGH041, and the melt index is 0.4 g / 10 min;

[0142] A11, heating deionized water to 80° C., then adding nano-montmorillonite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-montmorillonite to water is 1:25;

[0143] A12, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 min, then adding octadecyl trimethyl ammonium chloride and stirring evenly (the weight ratio of the octadecyl trimethyl ammonium chloride to the nano-montmorillonite is 1:12), and adjusting the pH value to 7.0-7.2, reacting for 3 h, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, then drying at 80 ° C for 48 h, and finally grinding and sieving to obtain modified nano-montmorillonite, i.e., modified nano filler;

[0144] A13, weighing the raw material components according to the following weight percentages: 87wt% of high-density polyethylene b, 2wt% of modified nanofiller, 10wt% of antibacterial agent and 1wt% of the first auxiliary agent, wherein the antibacterial agent comprises nano silver oxide and nano copper oxide in a weight ratio of 2:1, and the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;

[0145] A14, adding the weighed high-density polyethylene b, modified nano filler, antibacterial agent and first auxiliary agent into a twin-screw extruder and mixing them evenly, heating the screw extruder, and mixing in the twin-screw extruder, wherein the temperature of the twin-screw extruder is divided into a first section, a second section and a third section along the extrusion direction of the screw, wherein the temperature of the first section is 160° C., the temperature of the second section is 180° C., and the temperature of the third section is 190° C., the extruder speed of the twin-screw extruder is 300 r / min, the total residence time of the liner material in the twin-screw extruder is 5 min, and the material is cooled and pelletized after being extruded from the twin-screw extruder to obtain an antibacterial barrier material;

[0146] A15. Weigh the raw material components according to the following weight percentages: 89 wt% of high-density polyethylene a, 10 wt% of antibacterial barrier material and 1 wt% of a second auxiliary agent, wherein the second auxiliary agent is a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) mixed in a weight ratio of 1:1:1;

[0147] A16. Add the weighed high-density polyethylene a, antibacterial barrier material and second auxiliary agent into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone 1 is 120° C., the temperature of zone 2 is 150° C., and the temperature of zone 3 is 190° C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180° C., and the die temperature is 170° C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm;

[0148] A21. A continuous glass fiber reinforced prepreg tape with a width of 40 mm is subjected to radiation heating, and the prepreg tape is cross-wound around the outer side of the inner liner at an angle of 55° to the axis of the inner liner, with the number of winding layers being 10; wherein the continuous fibers in the continuous fiber reinforced resin prepreg tape are glass fibers, and the resin matrix is ​​high-density polyethylene;

[0149] A30. The method described in Example 1 is carried out to obtain an outer tube coated on the outside of the reinforcement layer, and the outer tube has a wall thickness of 3 mm, a nominal diameter of 65 mm, and an inner diameter of 50 mm, thereby obtaining Figure 1 The composite pipe shown has a nominal pressure of 12 MPa. Figure 1 In the figure, 1 inner lining layer; 2 reinforcement layer; 3 outer tube.

[0150] Example 6

[0151] The method described in Example 5 is used for implementation. The difference is that the preparation method of the antibacterial barrier material is different. In this embodiment, the preparation method of the antibacterial barrier material includes:

[0152] A13, weighing the raw material components according to the following weight percentages: 88wt% of high-density polyethylene b, 3wt% of modified nanofiller, 8wt% of antibacterial agent and 1wt% of the first auxiliary agent, wherein the antibacterial agent comprises nano silver oxide and nano copper oxide in a weight ratio of 2:1, and the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;

[0153] A14. Add high-density polyethylene b, modified nanofiller, antibacterial agent and the first auxiliary agent into a twin-screw extruder and mix them evenly, heat the screw extruder, and perform mixing in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section and a third section along the extrusion direction of the screw. The temperature of the first section is 170° C., the temperature of the second section is 185° C., and the temperature of the third section is 200° C. The extruder speed of the twin-screw extruder is 300 r / min, and the total residence time of the lining layer material in the twin-screw extruder is 5 min. After being extruded from the twin-screw extruder, the material is cooled and pelletized to obtain an antibacterial barrier material.

[0154] Example 7

[0155] The method described in Example 5 is used for implementation, except that the preparation method of the inner lining layer is:

[0156] A11, heating deionized water to 85° C., then adding nano-muscovite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-muscovite to water is 1:20;

[0157] A12. Adjust the pH of the mixture to 7.0-7.2 and continue heating for 30 min, then add octadecyl dimethyl benzyl ammonium chloride and stir evenly (the weight ratio of the octadecyl dimethyl benzyl ammonium chloride to the nano muscovite is 1:10), and adjust the pH to 7.0-7.2, react for 2 h, filter the obtained reaction solution, wash the filtered solid with deionized water 3 times, then dry at 80 ° C for 48 h, and finally grind and sieve to obtain modified nano muscovite, i.e., modified nano filler.

[0158] A13, weighing the raw material components according to the following weight percentages: 88wt% of high-density polyethylene b, 5wt% of modified nanofiller, 6wt% of antibacterial agent and 1wt% of the first auxiliary agent; wherein the first auxiliary agent comprises a titanate coupling agent (dioctylphosphite acyloxy titanate) and a compatibilizer (acrylic grafted polyethylene) in a weight ratio of 1:1, and the antibacterial agent comprises nano silver oxide and nano copper oxide in a weight ratio of 2:1;

[0159] A14, adding the raw material components in step A13 into a twin-screw extruder and mixing them evenly, heating the screw extruder, and performing mixing in the twin-screw extruder, wherein the temperature of the twin-screw extruder is divided into a first section, a second section, and a third section, wherein the temperature of the first section is 160° C., the temperature of the second section is 175° C., and the temperature of the third section is 190° C. The extruder speed of the twin-screw extruder is 350 r / min, and the total residence time of the antibacterial barrier material in the twin-screw extruder is 5 min. After the material is extruded from the twin-screw extruder, it is cooled and pelletized to obtain an antibacterial barrier material;

[0160] A15. Weigh the raw material components according to the following weight percentages: 85 wt% of high-density polyethylene a, 14 wt% of antibacterial barrier material and 1 wt% of a second auxiliary agent; wherein the second auxiliary agent is a mixture of a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) in a weight ratio of 1:1:1;

[0161] A16. Add the raw material components in step A15 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.

[0162] Example 8

[0163] The method described in Example 5 is implemented, except that the outer tube is implemented according to the method described in Example 2.

[0164] Example 9

[0165] The method described in Example 5 is implemented, except that the outer tube is implemented according to the method described in Example 3.

[0166] Example 10

[0167] The method described in Example 5 is implemented, except that the outer tube is implemented according to the method described in Example 4.

[0168] Comparative Example 1

[0169] The method described in Example 1 was used for implementation, except that no filler was added to the outer tube (the filler was replaced with an equal amount of medium-density polyethylene);

[0170] Specifically, step A31 includes: weighing the raw material components according to the following weight percentages: 97.6 wt% of medium-density polyethylene, 2 wt% of compatibilizer, and 0.4 wt% of additives.

[0171] Comparative Example 2

[0172] The method described in Example 1 is used for implementation, except that the filler is a metal oxide (ie, the metal oxide is not modified).

[0173] Comparative Example 3

[0174] The method described in Example 1 is used for implementation, except that the raw material for preparing the outer tube is pure medium density polyethylene (MDPE).

[0175] Comparative Example 4

[0176] The method described in Example 5 was followed, except that the first auxiliary agent was not added when preparing the antibacterial barrier material (the first auxiliary agent was replaced by an equal amount of high-density polyethylene b);

[0177] Specifically, step A13 includes: weighing the raw material components according to the following weight percentages: 88 wt% of high-density polyethylene b, 2 wt% of modified nanofiller and 10 wt% of antibacterial agent.

[0178] Comparative Example 5

[0179] The method described in Example 5 was followed, except that the nano-montmorillonite was not modified when preparing the antibacterial barrier material;

[0180] Specifically, step A13 is: weighing the raw material components according to the following weight percentages: 87 wt% of high-density polyethylene b, 2 wt% of nano-montmorillonite, 10 wt% of the antibacterial agent and 1 wt% of the first auxiliary agent.

[0181] Comparative Example 6

[0182] The method described in Example 5 is used for implementation, except that when preparing the inner lining layer, the antibacterial barrier material is not prepared first; specifically, all raw materials are directly mixed and co-extruded using the method of step A16.

[0183] Comparative Example 7

[0184] The method described in Example 5 was followed, except that no antimicrobial barrier material was added when preparing the inner lining layer;

[0185] Specifically, step A15 is: weighing the raw material components according to the following weight percentages: 99 wt % of high-density polyethylene a and 1 wt % of the second auxiliary agent.

[0186] Comparative Example 8

[0187] The method described in Example 5 was followed, except that the inner lining layer was directly prepared using high-density polyethylene a;

[0188] Specifically, the preparation method of the lining layer includes: adding high-density polyethylene a into a twin-screw extruder and mixing evenly, in the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C, the head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C, and the material is cooled and shaped after being extruded from the twin-screw extruder to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.

[0189] Test Example 1

[0190] The outer tubes prepared in Examples 1-4 and Comparative Examples 1-3 were used to prepare GB T1040.2-2006 tensile test specimens and 50 mm×50 mm×0.2 mm gas permeable film specimens.

[0191] (1) The tensile properties of the tensile specimens prepared in Examples 1-4 and Comparative Example 3 were measured at a tensile rate of 50 mm / min. The results are shown in Table 1.

[0192] Table 1

[0193] sample Yield strength / MPa Tensile strength / MPa Elongation / % Example 1 19.35 19.56 202 Example 2 18.25 18.75 211 Example 3 18.71 19.35. 187 Example 4 19.61 19.96 208 Comparative Example 3 (pure MDPE) 18.15 18.26 205.6

[0194] It can be seen from Table 1 that compared with the outer tube made of pure medium density polyethylene (MDPE), the yield strength and tensile strength of the outer tubes prepared in Examples 1-4 of the present invention do not change much. Although the elongation decreases significantly, it still meets the requirements of the composite tube for the outer tube.

[0195] (2) The gas permeability test of the gas permeable film samples prepared in Examples 1-4 and Comparative Examples 1-3 was performed on hydrogen sulfide gas permeability. The results are shown in Table 2.

[0196] Table 2

[0197] sample <![CDATA[Permeability coefficient (cm 3 ·cm) / (cm 2 ·s·Pa)]]> Example 1 <![CDATA[2.729x10 -14 ]]> Example 2 <![CDATA[7.446x10 -14 ]]> Example 3 <![CDATA[1.018x10 -13 ]]> Example 4 <![CDATA[2.529x10 -14 ]]> Comparative Example 1 <![CDATA[7.441x10 -13 ]]> Comparative Example 2 <![CDATA[3.237×10 -13 ]]> Comparative Example 3 (MDPE) <![CDATA[8.423x10 -13 ]]>

[0198] It can be seen from Table 2 that the outer tubes prepared in Examples 1-4 of the present invention have low permeability to H2S gas, indicating that the outer tubes prepared in the present invention can effectively prevent H2S from leaking out of the tube. In addition, by comparing Example 1 with Example 4, it can be seen that although the addition of additives can improve the processing properties of the material, it will have a certain adverse effect on the hydrogen sulfide permeability.

[0199] Compared with Example 1, in Comparative Example 1, no filler was added, and the permeability coefficient of the outer tube to H2S was greatly improved, indicating that the addition of fillers can significantly reduce the permeability of the outer tube to H2S gas; in Comparative Example 2, the metal oxide was not modified, and the permeability coefficient of the outer tube to H2S was improved, which may be due to the poor dispersion of the metal oxide in the medium-density polyethylene and the insufficient absorption of H2S; Comparative Example 3 was prepared using pure medium-density polyethylene, and the permeability coefficient of the outer tube to H2S gas was also greatly increased, and the permeability was reduced.

[0200] Test Example 2

[0201] The inner lining layer prepared in Example 5 was cut into small pieces of about 5 g, put into a flat vulcanizer, and pressed at a temperature of 150°C, a pressure of 10 MPa, and a time of 3 min. After air cooling, an inner lining film sample of 50 mm × 50 mm × 0.2 mm was obtained after cutting. Then, the inner lining layers in Examples 6-7 and Comparative Examples 4-8 were also made into film samples according to the same method, and the following tests were performed respectively.

[0202] (1) Scanning electron microscopy was used to characterize the film samples obtained in Comparative Example 8 (pure HDPE) and Example 5. The results are as follows: Figure 2 and Figure 3 shown.

[0203] Depend on Figure 2 and Figure 3 It can be seen that in the inner liner prepared in Example 5, the modified nano-montmorillonite and the antibacterial agent are uniformly dispersed in the HDPE, and the HDPE matrix tightly wraps the modified nano-montmorillonite and antibacterial agent particles without holes.

[0204] (2) The helium permeability of the liner film samples prepared in Examples 5-7 and Comparative Examples 4-8 was tested by a gas permeometer (the gases contained in medium and high pressure oil and gas are usually oxygen, carbon dioxide, methane, hydrogen sulfide, etc., and the diameter and volume of helium are smaller than those of these gas molecules). The results are shown in Table 3.

[0205] Table 3

[0206] project <![CDATA[Permeability coefficient (cm 3 ·cm) / (cm 2 ·s·Pa)]]> Example 5 <![CDATA[2.94×10 -15 ]]> Example 6 <![CDATA[3.21×10 -15 ]]> Example 7 <![CDATA[4.85×10 -15 ]]> Comparative Example 4 <![CDATA[9.35×10 -14 ]]> Comparative Example 5 <![CDATA[2.27×10 -13 <!-- 13 -->]]> Comparative Example 6 Membrane rupture Comparative Example 7 <![CDATA[3.24×10 -13 ]]> Comparative Example 8 (pure HDPE) <![CDATA[2.24×10 -13 ]]>

[0207] It can be seen from Table 3 that the inner liner samples prepared in Examples 5-7 of the present invention have very low permeability coefficients and have good gas barrier properties.

[0208] It can be seen from Example 5 and Comparative Example 4 that the gas barrier property of the liner layer can be improved by adding the first auxiliary agent.

[0209] It can be seen from Example 5 and Comparative Example 5 that the gas barrier properties of the lining layer can be greatly improved by modifying the flaky nanofiller. It is speculated that this may be because the unmodified flaky nanofiller has poor dispersibility in high-density polyethylene, resulting in its gas barrier properties being very little different from the lining layer made without adding antibacterial barrier materials (i.e., Comparative Examples 7-8).

[0210] The film of Comparative Example 6 broke during the permeation test. This may be because it is difficult to evenly disperse the nanofillers, antimicrobial agents, etc. in the high-density polyethylene by direct mixing. The nanofillers and antimicrobial agents agglomerate, and holes appear in the test film, causing the permeability test to fail.

[0211] It can be seen from Example 5 and Comparative Examples 7-8 that the gas barrier property of the lining layer can be greatly improved by adding the antibacterial barrier material.

[0212] It can be seen from Comparative Examples 7 and 8 that, although the addition of the second auxiliary agent improves the processing performance and antioxidant properties of the material, it has a certain adverse effect on the permeability of the material.

[0213] (3) The inner lining film samples prepared in Example 5 and Comparative Examples 4-8 were subjected to antibacterial tests according to the antibacterial test standard QB / T2591-2003A "Antibacterial plastic antibacterial performance test method and antibacterial effect". The test bacteria: sulfate-reducing bacteria. The test results are shown in Table 4.

[0214] Table 4

[0215] project Bacterial attachment rate / % Example 5 0.93 Comparative Example 4 68.26 Comparative Example 5 7.32 Comparative Example 6 74.50 Comparative Example 7 91.03 Comparative Example 8 (pure HDPE) 89.07

[0216] It can be seen from Table 4 that the antibacterial rate of the lining layer sample prepared in Example 5 of the present invention reaches 99%, and the antibacterial performance is excellent.

[0217] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A composite pipe, characterized in that: The composite pipe comprises an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside; The outer tube contains medium density polyethylene, filler, compatibilizer and optional additives, The filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can react chemically with hydrogen sulfide.

2. The composite pipe according to claim 1, characterized in that: Based on the total weight of the outer tube, the content of the polyethylene is 85-97wt%, the content of the filler is 2-10wt%, the content of the compatibilizer is 1-4wt%, and the content of the additive is 0-1wt%.

3. The composite pipe according to claim 1 or 2, characterized in that: The metal oxide is nano zinc oxide and / or nano iron oxide; Preferably, the nano zinc oxide is a tetrapod-shaped zinc oxide whisker.

4. The composite pipe according to any one of claims 1 to 3, characterized in that: The filler is prepared according to the following steps: Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 4 to 5.5 and reacting to obtain a coupling agent solution; The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.

5. The composite pipe according to claim 4, characterized in that: The volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25; Preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1; Preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:10-100.

6. The composite pipe according to claim 1 or 2, characterized in that: The melt index of the medium density polyethylene in the outer tube is 0.5 to 0.7 g / 10 min; Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high-density polyethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer; Preferably, the additive is selected from one or more of an anti-ultraviolet agent, a plasticizer, an antioxidant and a flame retardant.

7. The composite pipe according to claim 1, characterized in that The inner lining layer contains high-density polyethylene a and antibacterial barrier material, The antibacterial barrier material contains high-density polyethylene b, modified nanofiller, antibacterial agent and a first auxiliary agent, wherein the modified nanofiller is obtained by modifying the sheet-like nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.

8. The composite pipe according to claim 7, characterized in that Based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%; Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite; Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.

9. The composite pipe according to claim 7 or 8, characterized in that: The modified nanofiller is prepared according to the following process: S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture; S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.

10. The composite pipe according to claim 9, characterized in that In step S10, the weight ratio of the flaky nanofiller to water is 1:25-50; Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20.

11. The composite pipe according to claim 7, characterized in that The melt index of the high-density polyethylene b is 0.3 to 0.5 g / min; Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide; Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high-density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer; Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.

12. The composite pipe according to claim 7, characterized in that The antibacterial barrier material is prepared according to the following process: high-density polyethylene, modified nanofiller, antibacterial agent and first auxiliary agent are blended and extruded; Preferably, the blending extrusion is carried out in a twin-screw extruder; Preferably, the operating temperature of the twin-screw extruder is 160-200° C., and the operating speed is 300-350 r / min.

13. The composite pipe according to claim 7, characterized in that Based on the total weight of the inner lining layer, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%; Preferably, the high-density polyethylene a and the high-density polyethylene b are the same; Preferably, the inner lining layer further contains a second auxiliary agent, and the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent; Preferably, in the inner lining layer, the content of the second auxiliary agent is 1-2 wt %.

14. The method for preparing a composite pipe according to any one of claims 1 to 13, characterized in that: The method comprises the following steps: A1, blending and extruding the antibacterial barrier material and high-density polyethylene a to obtain an inner lining layer; A2, cross-winding the continuous fiber prepreg tape at an angle of 40 to 65 degrees with the axis of the inner liner layer on the outside of the inner liner layer to obtain a reinforcement layer; A3. Blending and extruding medium-density polyethylene, fillers, compatibilizers and optional additives through an extruder, and coating the mixture on the outside of the reinforcement layer.

15. The method according to claim 14, characterized in that In step A1, the blending extrusion is carried out in a twin-screw extruder; Preferably, in step A1, the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone 1 is 110-130° C., the temperature of zone 2 is 140-160° C., and the temperature of zone 3 is 180-200° C.; Preferably, in step A1, the head temperature of the twin-screw extruder is 165-185°C.

16. The method according to claim 14, characterized in that In step A3, the extruder is a twin-screw extruder, the operating speed of the twin-screw extruder is 300-350r / min, the working time is 3-6min, and the working temperature is divided into three sections along the material flow direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.