Metallographic specimen for fine detection of inclusion precipitates, preparation method of metallographic specimen and multi-index characterization method
Metallographic samples were prepared through Sterl metallographic sample preparation and grinding and polishing process, combined with the Glabbs inspection method, the problem of detecting small and medium-sized inclusions in high-quality steel was solved, and the fine detection of inclusions below 2μm was achieved. and multi-index characterization to meet complex detection needs and provide flexible and concise evaluation results representation.
Patent Information
- Application Number
- CN202411078729.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
The existing technology cannot effectively detect and evaluate small and medium-sized inclusions of high-quality steel (≤2μm), and the commonly used sample preparation standards and rating methods are single, which cannot meet complex testing needs, such as the cleanliness of ultra-clean pipes and the inclusions of bearing steel. brittle plasticity detection of substances.
By constructing the Sterl metallographic sample diagram, the grinding and polishing areas are divided according to the hardness, ductility and brittleness of the material, high-quality steel samples are prepared, and metallographic samples are prepared by grinding and polishing processes, combined with Glabbs inspection The method was used to perform multi-index characterization to achieve refined detection and evaluation of inclusions below 2μm.
The fine detection of inclusions below 2μm is realized, which makes up for the gap in the prior art, and provides a flexible and concise multiple evaluation results representation methods, which can simultaneously or selectively represent more than ten evaluation results, satisfying high Complex testing requirements in quality steel.
Smart Images

Figure CN118937377A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing high-quality steel, and in particular to a metallographic sample for refined detection of inclusion precipitates and a preparation method thereof, and a multi-index characterization method. Background Art
[0002] The test results of small-sized (≤2μm) inclusions (precipitates) in high-quality steel play an important role in material quality control. For example, aircraft turbine blades and bearing steels need to detect inclusions below 2μm. The various standards applicable to semiconductor ultra-clean tubes have included inclusions below 2μm in the cleanliness test. However, the commonly used ASTME768 sample preparation standard does not specify the preparation method of test specimens for inclusions below 2μm. In addition, the rating expression methods in GB / T10561 and GB / T30834 are single and cannot meet the complex detection and evaluation needs of inclusions (precipitates) in high-quality steel, such as the cleanliness of ultra-clean tubes, the brittle plasticity of inclusions in bearing steels, and defects in additively manufactured products.
[0003] Therefore, it is necessary to provide a sample preparation method that can meet the detection requirements of inclusions below 2 μm and is convenient for sample preparation, as well as a method for characterizing samples by multiple indicators. Summary of the invention
[0004] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide a metallographic specimen for refined detection of inclusions and precipitates and a preparation method and a multi-index characterization method, which are used to solve the problem that the existing sample preparation standards lack the detection of small-sized inclusions (precipitates) in high-quality steel, the representation method is single, and it cannot meet the complex detection and evaluation needs of inclusions (precipitates) in high-quality steel.
[0005] To achieve the above-mentioned object and other related objects, the present invention proposes a method for preparing a metallographic sample for refined detection of inclusion precipitates, which is characterized by comprising the following steps:
[0006] Based on the physical properties of the material, construct Struers metallographic sample drawings under different physical properties, wherein the physical properties of the material include hardness, ductility and brittleness of the material;
[0007] Divide the Struers metallographic sample into multiple grinding and polishing areas, and construct a grinding and polishing method corresponding to each grinding and polishing area according to the differences in the physical properties of the materials in each grinding and polishing area;
[0008] Select a high-quality steel sample, and determine the grinding and polishing process for the high-quality steel sample according to the grinding and polishing area to which the material of the high-quality steel sample belongs and the corresponding grinding and polishing method;
[0009] Cut high-quality steel samples into test blocks of certain sizes;
[0010] Clamp the test block on the grinding and polishing machine, grind and polish the test block according to the set grinding and polishing process, and process the longitudinal inspection surface parallel to the longitudinal axis of the steel and / or the transverse inspection surface perpendicular to the longitudinal axis of the steel on the test block;
[0011] The test block after grinding and polishing is polished and ultrasonically cleaned to clean the excess polishing agent and stains on the surface of the ground and polished test block. After air drying, a metallographic sample based on the refined detection of small-sized inclusion precipitates is obtained.
[0012] Preferably, the size of the inclusions and precipitates is 2 μm or less.
[0013] Preferably, the high-quality steel sample is clamped on the workbench of the Struers precision cutting machine, the cutting process conditions are set, and the sample is cut into a test block. The test block is a cylinder with a diameter of 30 mm. If the grinding and polishing surface area of the sample is different from this value, the required grinding and polishing pressure can be calculated based on the same grinding and polishing pressure.
[0014] Preferably, the Struers metallographic sample drawing is divided into seven grinding and polishing areas, namely A', B', C', D', E', F' and G', according to the hardness, ductility and brittleness of the material. The B' area is adjacent to the A' area, and the C' area is adjacent to the D' area; the C' area is adjacent to the A' area, the B' area, the D' area and the E' area; the D' area is adjacent to the B' area, the C' area and the F' area, and the E' area is adjacent to the C' area, the D' area, the F' area and the G' area; the hardness of the material corresponding to the A' area is less than the hardness of the material corresponding to the D' area to the G' area, and the hardness of the materials corresponding to the B' area and the C' area are both less than the hardness of the materials corresponding to the F' area and the G' area separated by each other.
[0015] Preferably, the grinding and polishing process includes coarse grinding, fine grinding, primary polishing, secondary polishing and / or tertiary polishing.
[0016] More preferably, the specific process conditions of the rough grinding step are: use a silicon carbide sandpaper pre-grinding disc with a grit size of 320 to grind and polish the A' area and the B' area, use a silicon carbide sandpaper pre-grinding disc with a grit size of 220 to grind and polish the C area, use a resin bond diamond fine grinding disc with a grit size of 220 to grind and polish the D' area to the G' area, the lubricant is water, the loading pressure in the A' area is 25N, the loading pressure in the B' area, the C' area and the G' area is 30N, the loading pressure in the D' area to the F' area is 40N, the grinding and polishing disc speed is 300rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0017] More preferably, the specific process conditions of the fine grinding step are: use a resin bond diamond fine grinding disc with a particle size of 1200 to grind and polish the A'~C' area, use a resin bond diamond fine grinding disc with a particle size of 500 to grind and polish the D'~G' area, the suspension particle size is 9μm, the lubricant is water, the loading pressure of the A'~C' area and the E'~F' area is 40N, the loading pressure of the D' area is 30N, the loading pressure of the G' area is 35N, the grinding time for processing the A'~C' area is 4min, the grinding time for processing the D'~E' area is 3min, the grinding time for processing the F' area is 5min, and the grinding time for processing the G' area is 10min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0018] Preferably, the specific process conditions for one polishing are: use hard flannel cloth to process the A'~G' area, the suspension particle size is 3μm, the loading pressure of the A' and B' areas is 25N, the loading pressure of the C'~G' area is 30N, the polishing time for processing the A' area is 4min, the polishing time for processing the B' area is 2min, and the polishing time for processing the C'~G' area is 3min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0019] Preferably, the specific process conditions for the secondary polishing are: using soft flannel cloth to process the A'~G' area, the suspension particle size is 1μm, the loading pressure of the A'~G' area is 20N, and the polishing time for processing the A'~G' area is 3min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0020] Preferably, the specific process conditions for the three polishings are: using soft flannel cloth to process the A'~G' area, the suspension particle size is 0.1μm, the loading pressure of the A'~G' area is 10N, and the polishing time for processing the A'~G' area is 3min; the lubricant is Struers lubricant; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0021] Preferably, when the grinding and polishing disc is replaced during the grinding and polishing process, the test block and the fixture of the grinding and polishing machine are cleaned to remove the suspension and abrasive left over from the previous process.
[0022] Preferably, the polished sample should be ultrasonically cleaned for 2 to 5 minutes to remove polishing agents and stains. After processing, the test block should be placed under an optical microscope at 1000 times and observed. There should be no obvious scratches, tails, and contaminants. When transferring the processed test block, use the smooth surface of the clean paper to protect it to avoid interference factors such as human pollution or air dust.
[0023] Preferably, the polishing area of the longitudinal inspection surface and the transverse inspection surface of the test block is not less than 160mm 2 .
[0024] The present invention also provides a metallographic sample prepared by the method for preparing the metallographic sample for refined detection of inclusion precipitates.
[0025] The present invention also provides a multi-index characterization method for metallographic samples for refined detection of inclusion precipitates, characterized in that it comprises the following steps:
[0026] Based on actual needs and the automated detection function of the scanning electron microscope, high-quality steel samples are subjected to refined detection; the refined detection includes classification detection and / or grade detection, the classification detection includes size, type performance detection; the grade detection includes cleanliness, content, aspect ratio, spacing and cluster performance detection;
[0027] After the test is completed, the test results are classified and rated according to the product technical specifications or relevant technical standards, and the classification symbols and level symbols are filled in expression (1):
[0028]
[0029] In formula (1), a and b are classification symbols of inclusions and / or precipitates; c, d, e, f, g, h, j, and k are level symbols; e and g represent the average values of the test results; f and h represent the m% values of the test results corresponding to e and g, respectively; the value of m is determined according to actual needs; unrated items are omitted, but e and f must be given at the same time, and g and h must be given at the same time.
[0030] Specifically, a is the classification symbol for the size range of inclusions and / or precipitates; b is the classification symbol for the type of inclusions and / or precipitates; c represents the cleanliness level symbol for inclusions and / or precipitates; d represents the content level symbol for inclusions and / or precipitates; e represents the average spacing level symbol for inclusions and / or precipitates; g represents the average aspect ratio level symbol for inclusions and / or precipitates; f represents the m% spacing level symbol for inclusions and / or precipitates; h represents the m% aspect ratio level symbol for inclusions and / or precipitates; j represents the worst size cluster level symbol for inclusions and / or precipitates; k represents the worst number cluster level symbol for inclusions and / or precipitates.
[0031] Table 1 Description of positions and symbols in evaluation expressions
[0032]
[0033] Preferably, the m% value in the inclusions and / or precipitates is calculated according to the following steps:
[0034] After arranging the results of inclusion or precipitate level detection from small to large, a level database of inclusion or precipitate is established. The training sample set M of the inclusion level database is {(x i )|i=1,2,…,n},where x i represents the i-th inclusion level data in the inclusion level database, and n represents the number of collected training samples; wherein the inclusion or precipitate level detection is the spacing level detection or the aspect ratio level detection;
[0035] Take the values of the first m% or last m% items in the training sample set M, and determine the confidence interval P of the training sample set M;
[0036] Calculate the mean x and standard deviation S of the first m% or the last m%;
[0037]
[0038]
[0039] According to the Grubbs method, outliers in the training sample set M' are removed, normal values in the training sample set M' are retained, and a characterization level database is re-established, wherein the training sample set N' of the characterization level database is {(x p )|p=q,q+1,…,(nr)},where x p represents the pth inclusion level data in the inclusion level database; q is the number of outliers in the first m% of the eliminated training sample set M'; r is the number of outliers in the last m% of the eliminated training sample set M'; nr represents the number of items corresponding to the maximum value in the training sample set N' representing the level database;
[0040] Calculate the average value of the training sample set N' of the representation level database That is the m% value:
[0041]
[0042] Preferably, m is 1.
[0043] More preferably, the step of removing outliers in the training sample set M according to the Grubbs method is performed as follows:
[0044] a) Obtain the critical value G of the Grubbs test P (n):
[0045] When n≤30, just look up Table 3;
[0046] When n>30, calculate the critical value T of the Grubbs test according to formula (5): α,n :
[0047] T α,n=A+B 1 lg(n)+B 2 lg(n) 2 +B 3 lg(n) 3 +B 4 lg(n) 4 +B 5 lg(n) 5 +B 6 lg(n) 6 +B 7 lg(n) 7 +B 8 lg(n) 8 (5);
[0048] In formula (5), α represents the confidence interval, n represents the number of values, that is, the number of training samples collected; A, B 1 …B 8 The values of are shown in Table 2;
[0049] Table 2 Grubbs test critical value T α,n Parameter table in calculation formula
[0050]
[0051] Table 3 Grubbs table - critical value G P (n)
[0052]
[0053] b) Obtain the actual Grubbs value G i :
[0054]
[0055] In the formula, x i represents the grade data of the ith inclusion or precipitate in the inclusion grade database, x is the average value of the interval of the first 1% items, and S is the sample standard deviation;
[0056] c) Compare Gi with G P (n) if Gi is greater than G P (n), xi is an outlier and needs to be removed; if Gi is less than G P (n), x i This is a normal value and needs to be retained.
[0057] The beneficial effects of the present invention are:
[0058] (1) The present invention combines the Struers metallographic phase diagram to perform a refined sample preparation method for the detection of inclusions or precipitates below 2 μm, which fills the gap in the existing sample preparation for the detection of inclusions or precipitates below 2 μm;
[0059] (2) Compared with the evaluation result expression method in the traditional standard, the present invention combines the Grubbs test method to propose a new expression method, which can simplify the expression of up to ten evaluation results at the same time or selectively. In addition, due to the differences in the position and symbol of each indicator symbol, according to actual needs, the unevaluated items can be omitted without causing ambiguity, making the evaluation result display flexible and concise. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 It is a flow chart of the preparation of metallographic samples for refined detection of inclusion precipitates of the present invention.
[0061] Figure 2 It is the Struers metallographic sample preparation diagram of the present invention.
[0062] Figure 3 This is an optical microscopic demonstration image (×1000 times) of the test surface of a test block prepared according to an embodiment of the present invention (the circled portion in the image is a small amount of micron-sized inclusions).
[0063] Figure 4 It is a format diagram of the expression of the present invention. The square box represents the filling position; the dotted box 1 represents the filling position of the classification symbol; the dotted box 2 represents the filling position of the level symbol).
[0064] Figure 5 It is a schematic diagram of the expression of a metallographic sample prepared in one embodiment of the present invention. DETAILED DESCRIPTION
[0065] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0066] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0067] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0068] The present application is further described below in conjunction with specific embodiments, but the protection scope of the present application is not limited thereto.
[0069] The method for preparing a metallographic sample for refined detection of inclusion precipitates described in the present invention comprises the following steps:
[0070] S1 constructs Struers metallographic sample drawings under different physical properties based on the physical properties of high-quality steel samples, including hardness, ductility and brittleness of the material;
[0071] S2 divides the Struers metallographic sample into multiple grinding and polishing areas, and constructs a grinding and polishing method corresponding to each grinding and polishing area according to the differences in the physical properties of the materials in each grinding and polishing area;
[0072] S3 selects a high-quality steel sample, and determines a grinding and polishing process for the high-quality steel sample according to the grinding and polishing area to which the material of the high-quality steel sample belongs and the corresponding grinding and polishing method;
[0073] S4 cuts high-quality steel samples into test blocks of certain sizes;
[0074] S5: clamping the test block on the grinding and polishing machine, grinding and polishing the test block according to the grinding and polishing process set for the grinding and polishing process, and processing the longitudinal inspection surface parallel to the longitudinal axis of the steel material and / or the transverse inspection surface perpendicular to the longitudinal axis of the steel material on the test block;
[0075] S6 polishes the test block after grinding and polishing, ultrasonically cleans it, removes excess polishing agent and stains on the surface of the ground and polished test block, and after air drying, obtains a metallographic sample based on the refined detection of small-sized inclusion precipitates.
[0076] In some embodiments of the present invention, the size of the inclusions and precipitates is less than 2 μm.
[0077] In some embodiments of the present invention, a high-quality steel sample is mounted on a workbench of a Struers precision cutting machine, and the cutting process conditions are set to cut the sample into a test block, which is a cylinder with a diameter of 30 mm. If the area of the longitudinal inspection surface and the transverse inspection surface of the test block serving as the grinding and polishing surface is different from this value, the required grinding and polishing pressure needs to be calculated based on the same grinding and polishing pressure.
[0078] like Figure 2 As shown, the Struers metallographic sample drawing is divided into seven grinding and polishing areas, namely A', B', C', D', E', F' and G', according to the hardness, ductility and brittleness of the material. The B' area is adjacent to the A' area, and the C' area is adjacent to the D' area; the C' area is adjacent to the A' area, the B' area, the D' area and the E' area; the D' area is adjacent to the B' area, the C' area and the F' area, and the E' area is adjacent to the C' area, the D' area, the F' area and the G' area; the hardness of the material corresponding to the A' area is less than the hardness of the material corresponding to the D' area to the G' area, and the hardness of the materials corresponding to the B' area and the C' area are both less than the hardness of the materials corresponding to the F' area and the G' area separated from each other. Seven samples with different hardness, brittleness and ductility were selected for grinding and polishing tests (including pure copper (A'), T22 carbon steel (B'), iron horse steel (C'), 1-xAlx high entropy alloys with different Al contents (FeCrCoNi) (D', E'), martensitic steel (F', G') and other metal materials), and finally the grinding and polishing parameters suitable for each area were obtained.
[0079] In some embodiments of the present invention, the grinding and polishing method includes coarse grinding, fine grinding, primary polishing, secondary polishing and / or tertiary polishing.
[0080] In some embodiments of the present invention, the specific process conditions of the rough grinding process are: use a silicon carbide sandpaper pre-grinding disc with a grit size of 320 to grind and polish the A' area and the B' area, use a silicon carbide sandpaper pre-grinding disc with a grit size of 220 to grind and polish the C area, use a resin bond diamond fine grinding disc with a grit size of 220 to grind and polish the D' area to the G' area, the lubricant is water, the loading pressure in the A' area is 25N, the loading pressure in the B' area, the C' area and the G' area is 30N, the loading pressure in the D' area to the F' area is 40N, the grinding and polishing disc speed is 300rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0081] In some embodiments of the present invention, the specific process conditions of the fine grinding process are: using a resin bond diamond fine grinding disc with a particle size of 1200 to grind and polish the A'~C' area, using a resin bond diamond fine grinding disc with a particle size of 500 to grind and polish the D'~G' area, the suspension particle size is 9μm, the lubricant is water, the loading pressure of the A'~C' area and the E'~F' area is 40N, the loading pressure of the D' area is 30N, and the loading pressure of the G' area is 35N. The grinding time for processing the A'~C' area is 4min, the grinding time for processing the D'~E' area is 3min, the grinding time for processing the F' area is 5min, and the grinding time for processing the G' area is 10min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0082] In some embodiments of the present invention, the specific process conditions for one polishing are: use hard velvet cloth to process the A'~G' area, the suspension particle size is 3μm, the loading pressure of the A' and B' areas is 25N, the loading pressure of the C'~G' area is 30N, the polishing time for processing the A' area is 4min, the polishing time for processing the B' area is 2min, and the polishing time for processing the C'~G' area is 3min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0083] In some embodiments of the present invention, the specific process conditions of the secondary polishing are: using soft velvet cloth to process the A'~G' area, the suspension particle size is 1μm, the loading pressure of the A'~G' area is 20N, and the polishing time for processing the A'~G' area is 3min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0084] In some embodiments of the present invention, the specific process conditions for the three polishings are: using soft flannel cloth to process the A'~G' area, the suspension particle size is 0.1μm, the loading pressure of the A'~G' area is 10N, and the polishing time for processing the A'~G' area is 3min; the lubricant is Struers lubricant; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
[0085] In some embodiments of the present invention, when the grinding and polishing disc is replaced during the grinding and polishing process, the test block and the fixture of the grinding and polishing machine are cleaned to remove the suspension and abrasive left over from the previous process.
[0086] In some embodiments of the present invention, the polished sample should be ultrasonically cleaned for 2 to 5 minutes to remove polishing agents and stains. After processing, the test block is placed under an optical microscope at 1000 times and observed. There should be no obvious scratches, tails, and contaminants. When transferring the processed test block, use the smooth surface of the cleaning paper to protect it to avoid interference factors such as human pollution or air dust.
[0087] In some embodiments of the present invention, the polishing area of the longitudinal inspection surface and the transverse inspection surface of the test block is not less than 160 mm 2 .
[0088] Specifically, the grinding and polishing method in S2 is shown in Table 4:
[0089] Table 4 Parameters of sample grinding and polishing method
[0090]
[0091]
[0092] The present invention also provides a multi-index characterization method for a metallographic sample for refined detection of inclusion precipitates, comprising the following steps:
[0093] S11 performs refined testing on high-quality steel samples based on actual needs and the automated testing function of the scanning electron microscope. The refined testing includes classification testing and / or grade testing. Classification testing includes size and type performance testing. Grade testing includes cleanliness, content, aspect ratio, spacing and cluster performance testing.
[0094] After the S12 test is completed, the test results are classified and rated according to the product technical specifications or relevant technical standards, and the classification symbols and level symbols are filled in expression (1):
[0095]
[0096] In formula (1), a and b are classification symbols of inclusions and / or precipitates; c, d, e, f, g, h, j, and k are level symbols; e and g represent the average values of the test results; f and h represent the m% values of the test results corresponding to e and g, respectively; the value of m is determined according to actual needs; unrated items are omitted, but e and f must be given at the same time, and g and h must be given at the same time.
[0097] Specifically, a is the classification symbol for the size range of inclusions and / or precipitates; b is the classification symbol for the type of inclusions and / or precipitates; c represents the cleanliness level symbol for inclusions and / or precipitates; d represents the content level symbol for inclusions and / or precipitates; e represents the average spacing level symbol for inclusions and / or precipitates; g represents the average aspect ratio level symbol for inclusions and / or precipitates; f represents the m% spacing level symbol for inclusions and / or precipitates; h represents the m% aspect ratio level symbol for inclusions and / or precipitates; j represents the worst size cluster level symbol for inclusions and / or precipitates; k represents the worst number cluster level symbol for inclusions and / or precipitates.
[0098] Specifically, the classification of inclusion size and type, and the representation of cleanliness, content, aspect ratio and cluster rating are given as examples. Figure 5 For a complete expression of multi-index test results, due to the differences in the position and symbol of each indicator, according to actual needs, the unrated items can be omitted without causing ambiguity, making the evaluation results flexible and concise, such as 6, IIC-6N 26 , CN.
[0099] The present invention uses the Grubbs method of removing outliers to illustrate the inclusion spacing, where m is 1.
[0100] In this embodiment, the 1% value of inclusions and / or precipitates is calculated according to the following steps:
[0101] After arranging the results of 1000 inclusion or precipitate level detection from small to large, a level database of inclusions or precipitates is established. The training sample set M' of the inclusion level database is i )|i=1,2,…,n},where x i represents the i-th inclusion level data in the inclusion level database, and n represents the number of collected training samples; the inclusion or precipitate level detection is the spacing level detection;
[0102] Take the values of the first 1% items in the training sample set M', which are: 4.7, 5.4, 6, 6.5, 7.3, 7.7, 8.2, 9, 10.1, 20; determine the confidence interval P' of the training sample set M', and the confidence interval P' is 0.95;
[0103] Calculate the mean x and standard deviation S of the top 1%;
[0104]
[0105]
[0106] According to the Grubbs method, whether the maximum value 20 and the minimum value 4.7 in the training sample set M' are outliers is determined as follows:
[0107] a) Substitute P' into G with n=10 and 0.95. p' (n), obtain the critical value G of the Grubbs test 0.95 (10):
[0108] Because when n=10≤30, we can get G by looking up Table 3 0.95 (10) = 2.176;
[0109] b) Obtain the actual Grubbs value G i :
[0110]
[0111] In the formula, x i represents the i-th inclusion level data in the inclusion level database, x is the average value of the interval of the first 1% items, and S is the sample standard deviation;
[0112] c) Compare Gi with G P' (n) if Gi is greater than G P (n), xi is an outlier and needs to be removed; if Gi is less than G P (n), x i Normal value, need to be retained:
[0113] Determine whether the maximum value 20 is an abnormal value, after calculation: Therefore, the maximum value 20 in the training sample set M' is an outlier and should be removed;
[0114] To determine whether the minimum value of 4.7 is an abnormal value, we calculate: Therefore, the minimum value of 4.7 in the training sample set M' is a normal value and should be retained;
[0115] Determine whether the second largest value 10.1 is an abnormal value, after calculation: Therefore, the minimum value 10.1 in the training sample set M' is a normal value and should be retained;
[0116] Therefore, the remaining 7 values are also normal values and should be retained.
[0117] Establish a characterization level database, the training sample set N' of the characterization level database is p )|p=q,q+1,…,(nr)},where x prepresents the pth inclusion level data in the inclusion level database; q is the number of outliers in the first 1% of the eliminated training sample set M', and it can be calculated that q = 1; r is the number of outliers in the last 1% of the eliminated training sample set M', and it can be calculated that r = 1; nr represents the number of items corresponding to the maximum value in the characterization level database, and it can be calculated that nr = 9;
[0118] Calculate the mean value X of the training sample set N' of the representation level database, that is, the 1% value:
[0119]
[0120] The various grades can be divided according to enterprise production standards or according to national standards.
[0121] The present invention also provides a metallographic sample prepared by the method for preparing a metallographic sample for refined detection of inclusion precipitates. The metallographic sample prepared by the sample preparation method of the present invention and the conventional sample preparation method were subjected to data detection comparison test, as shown in Table 5. "Unidentified particles" refer to particles that cannot be classified into inclusion types according to composition conditions, which may be introduced foreign interferences, and their size distribution is in the range of 0.5 to 2 μm. The use of this method significantly reduces interferences within this range.
[0122] Table 5 Comparison of test data of ultra-clean tubes using different sample preparation methods
[0123]
[0124] This embodiment is a rating comparison test of Alloy 1 and Alloy 2 in 316L ultra-clean pipes in different rating standards. The test results are shown in Tables 6 and 7.
[0125] Table 6 Rating comparison of alloy 1 and alloy 2 prepared by this method in 316L ultra-clean pipe
[0126]
[0127] Table 7 Rating comparison of alloy 1 and alloy 2 prepared by GB / T 10561 method in 316L ultra-clean pipe
[0128]
[0129] As can be seen from Tables 6 and 7, the numbers in this method represent the cleanliness rating. The larger the number, the worse the cleanliness. Compared with the external product, the cleanliness of the large-sized brittle inclusions inside is worse. Based on this difference, smelting improvements were made and significant results were achieved. However, there is no difference between the external and internal ratings in GB / T 10561.
[0130] This embodiment is a rating comparison test of high temperature alloy 1 and high temperature alloy 2 in different rating standards. The test results are shown in Tables 8 and 9.
[0131] Table 8 Rating comparison of high temperature alloy 1 and high temperature alloy 2 prepared by this method in 316L ultra-clean tube
[0132]
[0133] Table 9 Rating comparison of high temperature alloy 1 and high temperature alloy 2 prepared by GB / T 10561 method in 316L ultra-clean tube
[0134]
[0135] It can be seen from Tables 8 and 9 that the rating results of this method show that the aspect ratio of inclusions in the external alloy 1 is low and there are no large-sized inclusions, which is consistent with its excellent fatigue performance. In addition, the rating of GB / T 10561 does not show any difference in aspect ratio and large-sized inclusions.
[0136] This embodiment is a rating test of duplex stainless steel alloy 1 and alloy 2 in different rating standards. The test results are shown in Tables 10 and 11.
[0137] Table 10 Rating comparison of alloy 1 and alloy 2 prepared by this method in 316L ultra-clean pipe
[0138]
[0139] Table 11 Rating comparison of alloy 1 and alloy 2 prepared by GB / T 10561 method in 316L ultra-clean pipe
[0140]
[0141] It can be seen from Tables 10 and 11 that the rating results of the method of the present invention show that alloys 1 and 2 contain a large amount of brittle inclusions and have poor low-temperature impact properties. The low-temperature impact properties are successfully improved by optimizing the inclusion types through subsequent smelting. In addition, the rating of GB / T 10561 does not show the amount of brittle inclusions.
[0142] The above examples are for the purpose of illustrating the embodiments disclosed by the present invention and are not to be construed as limitations of the present invention. In addition, the various modifications listed herein and the variations of methods and compositions in the invention are obvious to those skilled in the art without departing from the scope and spirit of the present invention. Although the present invention has been specifically described in conjunction with various specific preferred embodiments of the present invention, it should be understood that the present invention should not be limited to these specific embodiments. In fact, various modifications obvious to those skilled in the art as described above to obtain the invention should be included within the scope of the present invention.
Claims
1. A method for preparing a metallographic sample for fine detection of inclusion precipitates, It is characterized in that The following steps are involved: Based on the physical properties of the material, construct Struers metallographic sample drawings under different physical properties, wherein the physical properties of the material include hardness, ductility and brittleness of the material; Divide the Struers metallographic sample into multiple grinding and polishing areas, and construct a grinding and polishing method corresponding to each grinding and polishing area according to the differences in the physical properties of the materials in each grinding and polishing area; Select a high-quality steel sample, and determine the grinding and polishing process for the high-quality steel sample according to the grinding and polishing area to which the material of the high-quality steel sample belongs and the corresponding grinding and polishing method; Cut high-quality steel samples into test blocks of certain sizes; Clamp the test block on the grinding and polishing machine, grind and polish the test block according to the set grinding and polishing process, and process the longitudinal inspection surface parallel to the longitudinal axis of the steel and / or the transverse inspection surface perpendicular to the longitudinal axis of the steel on the test block; The test block after grinding and polishing is polished and ultrasonically cleaned to clean the excess polishing agent and stains on the surface of the ground and polished test block. After air drying, a metallographic sample based on the refined detection of small-sized inclusion precipitates is obtained.
2. A method for preparing a metallographic sample for fine detection of inclusion precipitates according to claim 1, Features: Struers metallographic sample drawing is divided into seven grinding and polishing areas, namely A', B', C', D', E', F' and G', according to the hardness, ductility and brittleness of the material. The B' area is adjacent to the A' area, and the C' area is adjacent to the D' area; the C' area is adjacent to the A' area, the B' area, the D' area and the E' area; the D' area is adjacent to the B' area, the C' area and the F' area, and the E' area is adjacent to the C' area, the D' area, the F' area and the G' area; the hardness of the material corresponding to the A' area is less than the hardness of the material corresponding to the D' area to the G' area, and the hardness of the materials corresponding to the B' area and the C' area are both less than the hardness of the materials corresponding to the F' area and the G' area.
3. A method for preparing a metallographic sample for fine detection of inclusion precipitates according to claim 2, It is characterized in that The grinding and polishing method includes coarse grinding, fine grinding, primary polishing, secondary polishing and tertiary polishing.
4. A method for preparing a metallographic sample for refined detection of inclusion precipitates according to claim 3, It is characterized in that The specific process conditions of the rough grinding process are as follows: use a silicon carbide sandpaper pre-grinding disc with a grit size of 320 to grind and polish the A' area and the B' area, use a silicon carbide sandpaper pre-grinding disc with a grit size of 220 to grind and polish the C area, use a resin bond diamond fine grinding disc with a grit size of 220 to grind and polish the D' area to the G' area, the lubricant is water, the loading pressure in the A' area is 25N, the loading pressure in the B' area, the C' area and the G' area is 30N, the loading pressure in the D' area to the F' area is 40N, the grinding and polishing disc speed is 300rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
5. A method for preparing a metallographic sample for fine detection of inclusion precipitates according to claim 3, It is characterized in that The specific process conditions of the fine grinding process are: use a resin bond diamond fine grinding disc with a grit size of 1200 to grind and polish the A'~C' area, use a resin bond diamond fine grinding disc with a grit size of 500 to grind and polish the D'~G' area, the suspension particle size is 9μm, the lubricant is water, the loading pressure of the A'~C' area and the E'~F' area is 40N, the loading pressure of the D' area is 30N, and the loading pressure of the G' area is 35N. The grinding time for processing the A'~C' area is 4min, the grinding time for processing the D'~E' area is 3min, the grinding time for processing the F' area is 5min, and the grinding time for processing the G' area is 10min; the grinding and polishing disc speed is 150rpm, the fixture speed is 150rpm, and the grinding and polishing disc and the fixture rotate in the same direction.
6. A method for preparing a metallographic sample for fine detection of inclusion precipitates according to claim 3, Features: When the grinding and polishing disc is replaced during the grinding and polishing process, the test block and the fixture of the grinding and polishing machine are cleaned to remove the suspension and abrasive left over from the previous pass.
7. A method for preparing a metallographic sample for fine detection of inclusion precipitates according to claim 1, Features: The polishing area of the longitudinal inspection surface and the transverse inspection surface of the test block shall not be less than 160mm 2 .
8. A metallographic sample prepared according to the method for preparing a metallographic sample for fine detection of inclusion precipitates according to any one of claims 1 to 7.
9. A multi-index characterization method for metallographic samples for refined detection of inclusion precipitates as claimed in claim 8, It is characterized in that The following steps are involved: Based on actual needs and the automated detection function of the scanning electron microscope, high-quality steel samples are subjected to refined detection; the refined detection includes classification detection and / or grade detection, the classification detection includes size, type performance detection; the grade detection includes cleanliness, content, aspect ratio, spacing and cluster performance detection; After the test is completed, the test results are classified and rated according to the product technical specifications or technical standards, and the classification symbols and level symbols are filled in expression (1): In formula (1), a and b are classification symbols of inclusions and / or precipitates; c, d, e, f, g, h, j, and k are all level symbols; among them, e and f represent the average values of the test results; g and h represent the m% values of the test results corresponding to e and f, respectively; the value of m is determined according to actual needs; unrated items are omitted, but e and f must be given at the same time, and g and h must be given at the same time.
10. The multi-index characterization method according to claim 9, It is characterized in that The m% value in inclusions and / or precipitates is calculated as follows: After arranging the results of inclusion or precipitate level detection from small to large, a database of inclusion or precipitate levels is established. The training sample set M' of the inclusion level database is i )|i=1,2,…,n},where x i represents the i-th inclusion level data in the inclusion level database, and n represents the number of collected training samples; wherein the inclusion or precipitate level detection is the spacing level detection or the aspect ratio level detection; Take the values of the first m% or last m% items in the training sample set M' to determine the confidence interval P' of the training sample set M'; Calculates the average of the first m% or last m% of the items and standard deviation S; According to the Grubbs method, outliers in the training sample set M' are eliminated, and normal values in the training sample set M' are retained; Establish a characterization level database, the training sample set N' of the characterization level database is p )|p=q,q+1,…,(nqr)},where x p represents the pth inclusion level data in the inclusion level database; q is the number of outliers in the first m% of the eliminated training sample set M'; r is the number of outliers in the last m% of the eliminated training sample set M'; nqr represents the number of training samples in the representation level database, that is, the number of normal values in the training sample set M'; Calculate the average value of the training sample set N' of the representation level database That is the m% value: