Chip, manufacturing method thereof and electronic equipment

By setting up a carbon-doped isolation layer and a single crystal silicon channel layer in the fin structure of the FinFET, the leakage problem caused by metal residue in the metal-induced crystallization method is solved, and the performance and reliability of the chip are improved.

CN118943184APending Publication Date: 2024-11-12HUAWEI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310538857.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the back-end manufacturing process of a single-chip three-dimensional integrated circuit, metal residues in the recrystallization process of amorphous silicon caused by metal-induced crystallization, resulting in leakage and other problems, making it difficult to achieve a high-quality crystallized silicon process.

Method used

A carbon-doped isolation layer is provided in the fin structure of the FinFET to prevent metals and impurities from diffusion, and the single crystal silicon channel layer is epitaxially grown on the crystalline silicon layer to reduce leakage effect and improve mobility.

Benefits of technology

Effectively prevent metals and impurities from diffusion, reduce leakage effect, reduce power consumption, and improve chip performance and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943184A_ABST
    Figure CN118943184A_ABST
Patent Text Reader

Abstract

The invention provides a chip, a manufacturing method thereof and electronic equipment, relates to the technical field of chips, and can solve various problems caused by metal residues in crystalline silicon in a back-end manufacturing process. The chip comprises a first device layer, a second device layer and an intermediate dielectric layer. Wherein the intermediate dielectric layer is located between the first device layer and the second device layer. The second device layer includes a fin field effect transistor. The fin type field effect transistor comprises a fin structure, and the fin structure comprises a crystalline silicon layer and an epitaxial layer located on the crystalline silicon layer. The epitaxial layer comprises a channel part and an isolation part; the crystalline silicon layer is arranged on the intermediate dielectric layer, and metal elements are arranged in the crystalline silicon layer; the isolation part is located between the crystalline silicon layer and the channel part, and the isolation part comprises carbon elements. By arranging the isolation part, metal and impurity atoms in the crystalline silicon layer can be prevented from diffusing into the channel part, and the leakage effect at the bottom of the fin structure is weakened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of chip technology, and in particular to a chip and a manufacturing method thereof, and an electronic device. Background Art

[0002] As large-scale integrated circuit technology enters the 3-nanometer node, it is no longer sustainable to simply rely on size reduction to promote chip integration and component performance improvement. Monolithic 3D integration circuit (M3D IC) uses multi-layer device overlapping settings to greatly improve integration and interconnection density, reduce latency, and continue Moore's Law.

[0003] The difficulty of M3D IC lies in developing a low thermal budget manufacturing process that is compatible with the back-end (BEOL) of CMOS (complementary metal oxide semiconductor). The most critical part is the high-quality crystalline silicon process for back-end transistor manufacturing. Currently, metal induced crystallization (MIC) is a major source of crystalline silicon in the back-end manufacturing process, but the recrystallization of amorphous silicon through MIC has metal residues (also known as metal contamination), which leads to various problems such as leakage. Summary of the invention

[0004] The present application provides a chip and a manufacturing method thereof, and an electronic device, which can solve various problems caused by metal residues in crystalline silicon in the back-end manufacturing process.

[0005] The present application provides a chip, which includes: a first device layer, a second device layer, and an intermediate dielectric layer. The intermediate dielectric layer is located between the first device layer and the second device layer. The second device layer includes a fin field effect transistor (FinFET). The FinFET includes a fin structure (Fin), the fin structure includes a crystalline silicon layer and an epitaxial layer located on the crystalline silicon layer; the epitaxial layer includes a channel portion and an isolation portion. The crystalline silicon layer is arranged on the intermediate dielectric layer, and the crystalline silicon layer contains metal elements. The isolation portion is located between the crystalline silicon layer and the channel portion, and the isolation portion includes carbon elements.

[0006] That is to say, the chip of the present application sets an isolation part between the crystalline silicon layer and the channel part in the fin structure of the FinFET, and dopes carbon elements in the isolation part, so as to prevent the diffusion of metals and impurities, while ensuring that the isolation part itself has a low conductivity. In this way, on the one hand, the isolation part can prevent the metal and impurity atoms in the crystalline silicon layer from diffusing into the channel part; on the other hand, the low conductivity of the isolation layer can weaken the leakage effect at the bottom of the Fin; thereby reducing power consumption and improving chip performance and reliability.

[0007] In some possible implementations, the crystalline silicon layer includes single crystal silicon. In this case, the channel portion epitaxially grown on the crystalline silicon layer will replicate the crystal phase in the crystalline silicon layer, thereby enabling single crystal silicon to be used as the channel material of the FinFET (i.e., the channel portion is single crystal silicon material), thereby improving the mobility of the FinFET, reducing the subthreshold slope of the FinFET, and improving the reliability of the device.

[0008] In some possible implementations, the metal elements in the crystalline silicon layer include one or more of Ni, Co, Al, and Pt.

[0009] In some possible implementations, the intermediate dielectric layer includes one or more amorphous insulating materials with low dielectric constants such as SiO2 and SiN.

[0010] In some possible implementations, the first device layer includes fin field effect transistors.

[0011] The present application also provides a chip manufacturing method, which may include: manufacturing a first device layer, and manufacturing an intermediate dielectric layer on the first device layer. Manufacturing multiple amorphous silicon template strips on the intermediate dielectric layer, and metal-induced crystallization of the amorphous silicon template strips to form crystalline silicon template strips. Epitaxially growing an isolation layer and a channel layer on the crystalline silicon template strips, and etching the crystalline silicon template strips, the isolation layer and the channel layer as a whole to form multiple FinFET fin structures; wherein the isolation layer includes carbon elements.

[0012] The manufacturing method is used to perform metal-induced crystallization on the amorphous silicon template strip to form a crystalline silicon template strip, and the crystalline silicon template strip is used as a template for epitaxial manufacturing of an isolation layer and a channel layer. As a result, in the formed FinFET, the isolation layer can prevent the metal and impurity atoms in the crystalline silicon template strip from diffusing into the channel layer (i.e., the channel portion of the FinFET). At the same time, based on the low conductivity of the isolation layer itself, the leakage effect at the bottom of the fin structure can be weakened.

[0013] In some possible implementations, the above-mentioned method of making a plurality of amorphous silicon template strips on the intermediate dielectric layer and performing metal-induced crystallization on the amorphous silicon template strips to form crystalline silicon template strips includes: making a plurality of amorphous silicon template strips with a width less than 20 μm on the intermediate dielectric layer, and performing metal-induced lateral crystallization on the amorphous silicon template strips to form single-crystalline silicon template strips. In this case, the channel layer subsequently epitaxially grown on the single-crystalline silicon template strips can replicate the crystal phase in the single-crystalline silicon template strips, ensuring that the channel material of the FinFET is single-crystalline silicon, thereby improving the performance of the device.

[0014] In some possible implementations, the above-mentioned metal-induced crystallization of the amorphous silicon template strip to form a crystalline silicon template strip includes: forming a metal block at one end of the amorphous silicon template strip, and performing metal-induced crystallization on the amorphous silicon template strip to form a crystalline silicon template strip through an annealing process, and removing two ends of the crystalline silicon template strip. In this case, the concentration of the metal element in the amorphous silicon template strip can be reduced.

[0015] In some possible implementations, the epitaxial growth of the isolation layer and the channel layer on the crystalline silicon template strip includes: epitaxially growing the epitaxial layer on the crystalline silicon template strip, and ion implanting the epitaxial layer to form an isolation layer at the bottom and a channel layer at the top.

[0016] In some possible implementations, epitaxially growing the isolation layer and the channel layer on the crystalline silicon template strip includes: epitaxially growing the isolation layer on the crystalline silicon template strip using an in-situ growth process, and epitaxially growing the channel layer on the isolation layer using an in-situ growth process.

[0017] The present application also provides an electronic device, which may include a circuit board and a chip provided in any of the possible implementation methods described above, wherein the chip is electrically connected to the circuit board. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A schematic diagram of the structure of a chip provided in an embodiment of the present application;

[0019] Figure 2 A schematic diagram of the structure of a FinFET in a chip provided in an embodiment of the present application;

[0020] Figure 3 for Figure 2 Schematic side view of

[0021] Figure 4 A chip manufacturing flow chart provided in an embodiment of the present application;

[0022] Figure 5 A schematic diagram of a chip manufacturing process provided in an embodiment of the present application;

[0023] Figure 6 A schematic diagram of a chip manufacturing process provided in an embodiment of the present application;

[0024] Figure 7 A schematic diagram of a chip manufacturing process provided in an embodiment of the present application. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of this application clearer, the technical solutions in this application will be clearly and completely described below in conjunction with the drawings in this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0026] The terms "first", "second", etc. in the specification embodiments, claims and drawings of the present application are only used for the purpose of distinguishing descriptions, and cannot be understood as indicating or implying relative importance, nor can they be understood as indicating or implying order. "And / or" is used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, "A and / or B" can mean: only A exists, only B exists, and A and B exist at the same time, where A and B can be singular or plural. The character " / " generally indicates that the objects associated before and after are in an "or" relationship. "At least one (item)" means one or more, and "multiple" means two or more. "Installation", "connection", "connected", etc. should be understood in a broad sense, for example, it can be an electrical connection or a mechanical connection; it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or it can be indirect through an intermediate medium, or it can be the internal connection of two elements. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, including a series of steps or units. Methods, systems, products or devices are not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or devices. "Up", "down", "left", "right", etc. are only used relative to the orientation of the components in the drawings. These directional terms are relative concepts. They are used for description and clarification relative to the description, which may change accordingly according to the change of the orientation of the components in the drawings.

[0027] An embodiment of the present application provides an electronic device, which includes a printed circuit board (PCB; also referred to as a printed circuit board) and a chip electrically connected to the circuit board. The chip can be a monolithic three-dimensional integrated circuit (M3D IC), which is based on a metal induced crystallization (MIC) process to be compatible with a low thermal budget manufacturing process in the back-end. An isolation layer is provided in the fin structure (Fin) of a fin field effect transistor (FinFET) in the back-end to prevent the metal and impurity atoms at the bottom of the Fin from diffusing into the channel, and the low conductivity of the isolation layer itself can reduce the leakage effect at the bottom of the Fin.

[0028] The present application does not limit the configuration of the above electronic device. For example, the electronic device may be a mobile phone, a tablet computer, a notebook, a car computer, a smart watch, a smart bracelet, a server, or other electronic products.

[0029] The specific structure of the chip (M3D IC) provided in the embodiment of the present application is described below.

[0030] First, the overall structure of the M3D IC is briefly described.

[0031] Indicative, such as Figure 1 As shown, the M3D IC includes a substrate 100 and multiple device layers stacked on the substrate 100, such as a first device layer 201, a second device layer 202, and a third device layer 203; an intermediate dielectric layer 300 (also referred to as a passivation layer) is provided between two adjacent device layers, that is, the two adjacent device layers are isolated by the intermediate dielectric layer 300. Among them, the first device layer 201 is a front-end device layer, which can be directly manufactured on the substrate 100, and the second device layer 202 and the third device layer 203 are manufactured on the intermediate dielectric layer 300 as back-end device layers.

[0032] As shown, fin field effect transistors (FinFETs) may be provided in the plurality of device layers (201, 202, 203).

[0033] The high-quality crystalline silicon required for FinFET in the back-end device layer (202, 203) is the key point of M3D IC. In the M3D IC provided in the embodiment of the present application, at least one back-end device layer (202, 203) adopts a FinFET device with a new structure, which is compatible with the low thermal budget crystalline silicon process of the back-end. Of course, the front-end device layer (201) can adopt a FinFET device with a new structure according to actual needs, or can adopt transistors of other types of structures (such as planar transistors), and the present application does not limit this.

[0034] Taking the FinFET device in the second device layer 202 as an example, the chip provided in the embodiment of the present application is further described below.

[0035] like Figure 2 and Figure 3 ( Figure 2 As shown in the side schematic diagram of the device 200, a FinFET is provided in the second device layer 202, and the FinFET has a fin structure F (Fin), and the fin structure F includes a crystalline silicon layer 11 and an epitaxial layer E located on the crystalline silicon layer 11, that is, the epitaxial layer E is obtained by epitaxial growth on the crystalline silicon layer 11. Among them, the crystalline silicon layer 11 is provided on the intermediate dielectric layer 300, and the crystalline silicon layer 11 contains metal elements, such as one or more metal elements such as Ni, Co, Al, Pt, etc.

[0036] In some possible implementations, the crystalline silicon layer 11 may be obtained by metal induced crystallization (MIC) of amorphous silicon (a-Si), and the crystalline silicon (c-Si) in the crystalline silicon layer 11 may be polycrystalline silicon or single crystal silicon. In this case, the low thermal budget crystalline silicon process of the subsequent process is compatible.

[0037] For example, in some embodiments, the crystalline silicon layer 11 may be a single crystal silicon layer formed by a metal induced lateral crystallization (MILC) process, so that the channel material of the FinFET can be single crystal silicon, thereby improving the mobility of the FinFET, reducing the subthreshold slope of the FinFET, reducing the power consumption of the device, and improving the performance and reliability of the device. For details, please refer to the relevant instructions in the subsequent manufacturing method.

[0038] refer to Figure 3As shown, the epitaxial layer E is obtained by epitaxial growth on the crystalline silicon layer 11, that is, the silicon in the epitaxial layer E will replicate the crystalline phase in the crystalline silicon layer 11. In the case where the crystalline silicon layer 11 is single crystal silicon, the silicon in the epitaxial layer E is also single crystal silicon. The epitaxial layer E includes an isolation portion 12 and a channel portion 13 (channel), and the isolation portion 12 is located between the crystalline silicon layer 11 and the channel portion 13. Among them, the isolation portion 12 is doped with carbon elements, that is, the isolation portion 12 includes Si:C, and the carbon elements doped in the isolation portion 12 can prevent the diffusion of metals and impurities, etc., and at the same time can ensure that the isolation portion itself has a lower conductivity.

[0039] The isolation portion 12 and the channel portion 13 in the epitaxial layer E may be fabricated through a single epitaxial process or may be fabricated separately through two epitaxial processes. This application does not impose any limitation on this. For details, please refer to the relevant description in the subsequent fabrication method.

[0040] To sum up, in the chip provided in the embodiment of the present application, an isolation portion 12 doped with carbon elements is provided between the crystalline silicon layer 11 and the channel portion 13 in the fin structure F. The isolation portion 12 can prevent the metal and impurity atoms in the crystalline silicon layer 11 from diffusing into the channel portion 13. At the same time, the low conductivity of the isolation layer 12 itself can weaken the leakage effect at the bottom of the fin structure F, thereby reducing power consumption and improving the performance and reliability of the chip.

[0041] Of course, FinFET may also include other structures, such as a dielectric layer and a gate layer G covering the outside of the channel portion 13, a shallow trench isolation layer STI (shallow trench isolation) filled in the sides of the crystalline silicon layer 11 and the isolation portion 12, etc. This application does not impose too many restrictions on this, and in practice it can be set according to the needs of the chip.

[0042] The present application does not impose any limitation on the dielectric material used for the intermediate dielectric layer 300 , and it can be set as required in practice.

[0043] In some possible implementations, the intermediate dielectric layer 300 may be made of amorphous insulating materials with low dielectric constants, such as SiO2, SiN x At least one of .

[0044] It should be noted that in the chip provided in the embodiment of the present application, all device layers (including front-end and back-end) can be configured to adopt the above-mentioned novel FinFET structure, and some or all back-end device layers can be configured to adopt the above-mentioned novel FinFET structure. For example, in some possible implementations, all device layers in the back-end of the chip can adopt the above-mentioned novel FinFET structure.

[0045] The FinFET located in the second device layer 202 in the embodiment of the present application is further described below in conjunction with the chip manufacturing method.

[0046] Schematically, the present application embodiment provides a method for manufacturing a chip, such as Figure 4 As shown, the production method includes:

[0047] Step 11. Reference Figure 5 As shown, a first device layer 201 is manufactured, and an intermediate dielectric layer 300 is manufactured on the first device layer 201 .

[0048] It should be noted that the first device layer 201 manufactured in step 11 can be a front-end device layer or a back-end device layer, and this application does not impose any limitation on this.

[0049] Step 12: Reference Figure 6 As shown, a plurality of amorphous silicon template strips R are fabricated on the intermediate dielectric layer 300. a-Si , and the amorphous silicon template strip R a-Si Metal induced crystallization (MIC) was performed to form crystalline silicon template strips R c-Si .

[0050] In some possible implementations, step 12 may include: Figure 6 As shown in (a), an amorphous silicon layer 10 is deposited on the intermediate dielectric layer 300. Then, referring to Figure 6 As shown in (b), the amorphous silicon layer 10 is patterned by photolithography and etching to form a plurality of amorphous silicon template strips R a-S Next, refer to Figure 6 As shown in (c), in the amorphous silicon template strip R a-Si Then, refer to Figure 6 As shown in (d), for the amorphous silicon template strip R a-Si Metal induced crystallization (MIC) was performed to form crystalline silicon template strips R c-Si , and remove the crystalline silicon template strip R c-Si The Ni content at both ends is higher to reduce the R c-Si The concentration of Ni in MgO2O3 is 2.447 W / m2.

[0051] Of course, removing the crystalline silicon template strip R c-Si Before the two ends with higher metal content, the crystalline silicon template strip R c-Si The remaining Ni metal block M1 on the surface is cleaned.

[0052] In some possible implementations, a plurality of amorphous silicon template strips R having a width less than 20 μm can be fabricated on the intermediate dielectric layer 300 through the above step 12. a-Si, and through two annealing processes, the amorphous silicon template strip R a-Si Metal induced lateral crystallization (MILC) is performed to form a single crystal silicon template strip, thereby ensuring that the channel material of the subsequently formed FinFET is single crystal silicon material, thereby improving the mobility of the FinFET, reducing the subthreshold slope of the FinFET, and improving the reliability of the device.

[0053] As shown, in the above two annealing processes of metal induced lateral crystallization (MILC): the temperature of the first annealing process can be around 400-500°C, and Ni reacts with Si to form NiSi2; the temperature of the second annealing process can be around 450-600°C, and through the metal lateral induced crystallization, the Ni element moves from one end to the other and realizes the transformation of amorphous silicon to crystalline silicon.

[0054] Step 13. Reference Figure 7 As shown, in the crystalline silicon template strip R c-Si The isolation layer 12' and the channel layer 13' are epitaxially grown on the crystalline silicon template strip R c-Si , the isolation layer 12' and the channel layer 13' are etched as a whole to form a plurality of fin structures F of FinFETs; wherein the isolation layer 12' includes carbon elements.

[0055] The isolation layer 12' and the channel layer 13' are made of crystalline silicon template strips R c-Si As a seed layer, the silicon in the isolation layer 12' and the channel layer 13' will replicate the crystalline silicon template strip R c-Si The crystal phase in.

[0056] The isolation layer 12 ′ and the channel layer 13 ′ may be manufactured through one epitaxial process or two epitaxial processes. In practice, a suitable process may be selected according to needs.

[0057] For example, in some possible implementations, the above step 13 may include: referring to Figure 7 As shown in (b), the crystalline silicon template strip R c-Si As a template, a low-temperature vapor phase epitaxial process (such as 350°C) can be used to form a crystalline silicon template strip R c-Si Then, a high-quality epitaxial layer E is obtained by epitaxial growth. Figure 7 As shown in (c), ion implantation is performed on the epitaxial layer E to form an isolation layer 12' at the bottom and a channel layer 13' at the top. Figure 7 As shown in (d), for the crystalline silicon template strip R c-Si , the isolation layer 12 ′ and the channel layer 13 ′ are etched as a whole to form a plurality of fin structures F of FinFETs.

[0058] The low-temperature vapor phase epitaxial growth process may be inductively coupled plasma chemical vapor deposition (ICPCVD), plasma enhanced chemical vapor deposition (PECVD), etc., but is not limited thereto.

[0059] Regarding the isolation layer 12' and the channel layer 13' formed by ion implantation, in some embodiments, ion implantation can be performed on the epitaxial layer E, and a high dose of C (the dose can be 1E14-1E16 / cm 2 ) to form an isolation layer 12' made of Si:C material, and P or B is implanted on the top to form a channel layer 13'.

[0060] For example, in some other possible implementations, the above step 13 may include: c-Si In the embodiment, the isolation layer 12 is formed by firstly performing an in-situ growth process, and then the channel layer 13 is formed by performing another in-situ growth process, that is, the isolation layer 12 and the channel layer 13 are separately manufactured by performing two in-situ growth processes.

[0061] It should be understood that in the crystalline silicon template strip R c-Si In the case of single crystal silicon, the crystalline silicon template strip R c-Si The channel layer 13 ′ formed by epitaxial growth as a seed layer is also made of single crystal silicon material.

[0062] Of course, reference Figure 2 and Figure 3 As shown, after step 13, other manufacturing processes may be provided, and this application does not impose any limitation thereto.

[0063] The order of execution of each manufacturing process should be determined by the internal logic of the device and should not constitute any limitation on the implementation process of the embodiment of the present application.

[0064] In addition, for other related contents in the above-mentioned production method, you can refer to the corresponding parts in the above-mentioned structural embodiment, and will not be repeated here; for other setting structures in the above-mentioned structural embodiment, you can refer to the above-mentioned production method and related production methods for adjustment, and will not be repeated here one by one.

[0065] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A chip, characterized in that: include: A first device layer, a second device layer, and an intermediate dielectric layer; wherein the intermediate dielectric layer is located between the first device layer and the second device layer; The second device layer includes fin field effect transistors; The fin field effect transistor comprises a fin structure, wherein the fin structure comprises a crystalline silicon layer and an epitaxial layer located on the crystalline silicon layer; the epitaxial layer comprises a channel portion and an isolation portion; The crystalline silicon layer is disposed on the intermediate dielectric layer, and the crystalline silicon layer contains metal elements; The isolation portion is located between the crystalline silicon layer and the channel portion, and the isolation portion includes carbon elements.

2. The chip according to claim 1, characterized in that: The crystalline silicon layer includes single crystal silicon.

3. The chip according to claim 1 or 2, characterized in that: The metal elements in the crystalline silicon layer include one or more of Ni, Co, Al, and Pt.

4. The chip according to any one of claims 1 to 3, characterized in that: The intermediate dielectric layer includes at least one of SiO2 and SiN.

5. The chip according to any one of claims 1 to 4, characterized in that: The first device layer includes fin field effect transistors.

6. A chip manufacturing method, characterized in that: include: Manufacturing a first device layer, and manufacturing an intermediate dielectric layer on the first device layer; Fabricating a plurality of amorphous silicon template strips on the intermediate dielectric layer, and subjecting the amorphous silicon template strips to metal-induced crystallization to form crystalline silicon template strips; An isolation layer and a channel layer are epitaxially grown on the crystalline silicon template strip, and the crystalline silicon template strip, the isolation layer and the channel layer are etched as a whole to form a fin structure of a plurality of fin field effect transistors; wherein the isolation portion includes carbon elements.

7. The chip manufacturing method according to claim 6, characterized in that: The method of manufacturing a plurality of amorphous silicon template strips on the intermediate dielectric layer and performing metal-induced crystallization on the amorphous silicon template strips to form crystalline silicon template strips comprises: A plurality of amorphous silicon template strips with a width less than 20 μm are manufactured on the intermediate dielectric layer, and the amorphous silicon template strips are subjected to metal-induced lateral crystallization to form single crystal silicon template strips.

8. The chip manufacturing method according to claim 6 or 7, characterized in that: The step of subjecting the amorphous silicon template strip to metal-induced crystallization to form a crystalline silicon template strip comprises: A metal block is formed at one end of the amorphous silicon template strip, and the amorphous silicon template strip is subjected to metal-induced crystallization through an annealing process to form a crystalline silicon template strip, and two ends of the crystalline silicon template strip are removed.

9. The chip manufacturing method according to any one of claims 6 to 8, characterized in that: The epitaxial growth of the isolation layer and the channel layer on the crystalline silicon template strip comprises: epitaxially growing an epitaxial layer on the crystalline silicon template strip; Ions are implanted into the epitaxial layer to form the isolation layer at the bottom and the channel layer at the top.

10. The chip manufacturing method according to any one of claims 6 to 8, characterized in that: The epitaxial growth of the isolation layer and the channel layer on the crystalline silicon template strip comprises: epitaxially growing an isolation layer on the crystalline silicon template strip by adopting an in-situ growth process; An in-situ growth process is adopted to epitaxially grow a channel layer on the isolation layer.

11. An electronic device, characterized in that: It comprises a circuit board and a chip as claimed in any one of claims 1 to 5, wherein the chip is electrically connected to the circuit board.