Improved crystalline silicon solar cell preparation method and crystalline silicon solar cell
By using etching and light-induced laser-assisted electroplating technology in the manufacturing process of crystalline silicon solar cells, the problems of silicon substrate damage and electroplating solution stability caused by seed layer production are solved, the battery performance and efficiency are improved, and the application scenarios are expanded.
Patent Information
- Application Number
- CN202410995157.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the manufacturing process of existing crystalline silicon solar cells, the production of seed layer causes damage to the silicon substrate, affecting battery performance, and insufficient stability and uniformity of the plating solution, affecting the quality of the plating layer and production costs.
Etching is used to form patterned grooves, combining light-induced and laser-assisted electroplating of nickel, double-sided copper and silver layers to optimize the plating process of silicon substrates, reduce damage and improve the uniformity and adhesion of the plating layer.
It improves the open circuit voltage and photoelectric conversion efficiency of solar cells, reduces silicon substrate damage, optimizes the uniformity and adhesion of metal layers, and expands the application scenarios of crystalline silicon solar cells.
Smart Images

Figure BDA0004961457570000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cell preparation, and in particular to an improved crystalline silicon solar cell preparation method and a crystalline silicon solar cell. Background Art
[0002] Metallization is one of the key processes in the preparation of silicon solar cells. It is mainly used to make silicon solar cell electrodes, forming ohmic contacts at both ends of the PN junction to achieve current output. As a non-contact electrode preparation technology, electroplating technology usually requires plating a layer of metal on the silicon surface as a seed layer, and then depositing other metals as conductive layers and protective layers to form electroplated solar cells.
[0003] In the current manufacturing process of crystalline silicon solar cells, the preparation of the seed layer is one of the key steps, and nickel metal is usually used as the seed layer material. Before the nickel plating process, the silicon substrate needs to be pre-treated, and the laser film opening technology is used to remove part of the passivation layer on the surface of the silicon substrate to form a specific pattern. Although this step can achieve patterning, the laser treatment will damage the pyramid velvet structure of the silicon substrate, which may in turn destroy the PN junction of the silicon substrate and affect the performance of the battery, especially the open circuit voltage.
[0004] In the electroplating process, nickel sulfate system and nickel sulfamate system are two commonly used electroplating solutions. Although the nickel sulfate system can provide good coating quality, its current density range is narrow, and the internal stress of the coating is large, and the porosity is relatively high, which may affect the uniformity and adhesion of the coating. Although the nickel sulfamate system has smaller internal stress and faster deposition rate, its stability is poor and it is easy to decompose and generate organic matter during the electroplating process, thereby contaminating the electroplating solution, which not only affects the quality of the coating, but may also increase production costs and environmental risks.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the objectives of the present invention is to provide an improved method for preparing a crystalline silicon solar cell, aiming to solve at least one of the above-mentioned technical problems in the prior art.
[0007] A second object of the present invention is to provide a crystalline silicon solar cell.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] The first aspect of the present invention provides an improved method for preparing a crystalline silicon solar cell, wherein patterned grooves are etched on the front and back sides of a silicon substrate of the solar cell, and then nickel is electroplated on the back side of the silicon substrate by light-induced electroplating, and nickel is electroplated on the front side of the silicon substrate by laser-assisted electroplating, and finally, a double-sided nickel-plated silicon substrate with nickel plated on both the front and back sides is electroplated with a copper layer and a silver layer on both sides to obtain a double-sided electroplated crystalline silicon solar cell.
[0010] Furthermore, the etching is performed by screen printing a corrosion slurry and drying and sintering it.
[0011] Preferably, the solar cell silicon substrate is a TOPCon cell.
[0012] For TOPCon cells, the conventional process is to use light-induced electroplating on the back side, while direct electroplating is sufficient on the front side without light induction. On this basis, the present invention adds laser-assisted electroplating processes on both the front and back sides.
[0013] Preferably, the etching slurry comprises 10wt.% to 20wt.% of water-based acrylic resin, 0.5wt.% to 3.0wt.% of thixotropic agent, 15wt.% to 25wt.% of acid, 10wt.% to 30wt.% of filler, and the balance is solvent.
[0014] Preferably, the thixotropic agent comprises a polyamide wax thixotropic agent.
[0015] Preferably, the acid includes at least one of hydrofluoric acid, phosphoric acid, nitric acid, pyrophosphoric acid and sulfurous acid.
[0016] Preferably, the filler includes at least one of alumina, silica powder, kaolin, titanium dioxide, aluminum hydroxide and calcium carbonate.
[0017] Preferably, the solvent comprises at least one of ethanol, acetic acid, ethyl acetate, ethylene glycol and glycerol.
[0018] Preferably, the drying and sintering temperature is 300° C. to 400° C., and the time is 1 min to 3 min.
[0019] Furthermore, the specific process of the light-induced nickel electroplating is:
[0020] The back side of the silicon substrate is in contact with the electrolyte as the cathode, and the pure nickel plate is used as the anode. The anode is placed below the cathode, and the nickel plating solution is used as the electrolyte. The DC power supply and the light source are turned on for light-induced constant current electroplating. At the same time, the laser is turned on to emit a Gaussian laser beam, which is focused by the focusing lens and irradiated through the electrolyte to the back side of the silicon substrate after being expanded by the beam expander and reflected by the total reflection mirror. The grooves are scanned according to the set pattern, and the electroplating is stopped after the scanning.
[0021] Preferably, the light source of the light-induced electroplating includes a halogen lamp, an LED lamp, an incandescent lamp or a mercury lamp.
[0022] Furthermore, the specific process of laser-assisted nickel electroplating is as follows:
[0023] The front side of the silicon substrate is in contact with the electrolyte as the cathode, and the pure nickel plate is used as the anode. The anode is placed below the cathode, and the nickel plating solution is used as the electrolyte. The DC power supply is turned on for constant current electroplating. At the same time, the laser is turned on to emit a Gaussian laser beam. After being expanded by a beam expander and reflected by a total reflection mirror, it is focused by a focusing lens and irradiated to the front side of the silicon substrate through the electrolyte. The grooves are scanned according to the set pattern, and the electroplating is stopped after the scanning is completed.
[0024] Furthermore, the nickel electroplating solution includes 100 g / L to 300 g / L nickel sulfate hexahydrate, 40 g / L to 100 g / L nickel chloride hexahydrate, 30 g / L to 60 g / L boric acid, 1 g / L to 4 g / L saccharin sodium, and 0.1 g / L to 0.5 g / L wetting agent.
[0025] Preferably, the wetting agent includes at least one of sodium n-octyl sulfate, sodium 2-ethylhexyl sulfate, sodium salt of sulfosuccinate, and sodium salt of diethyl sulfosuccinate.
[0026] Preferably, the temperature of the nickel electroplating solution is 40° C. to 50° C., and the pH value is 3.5 to 4.0.
[0027] Preferably, the current density of the light-induced constant current plating or the constant current plating is independently 5A / dm 2 ~10A / dm 2 The time for each is independent and ranges from 5s to 12s.
[0028] Furthermore, the laser is a picosecond fiber laser with a wavelength of 355 nm.
[0029] Preferably, the light spot of the laser is a point-shaped light spot, the diameter of the light spot is 10 μm to 20 μm, and the distance between the light spots is -1 μm to 1 μm.
[0030] Preferably, the scanning rate of the laser is 3000 mm / s to 8000 mm / s, the frequency is 50 kHz to 500 kHz, the average power is 1 W to 3 W, and the pulse width is 10 ns to 50 ns.
[0031] Furthermore, the thickness of the nickel layer formed by light-induced nickel electroplating on the back side of the silicon substrate is 0.8 μm to 1.2 μm.
[0032] Preferably, the nickel layer formed by laser-assisted nickel electroplating on the front side of the silicon substrate has a thickness of 0.8 μm to 1.2 μm.
[0033] Furthermore, the copper layer has a thickness of 8 μm to 10 μm.
[0034] Preferably, the thickness of the silver layer is 1 μm to 2 μm.
[0035] Furthermore, the passivation layer is etched on the solar cell silicon substrate to form a patterned groove.
[0036] Preferably, the passivation layer is made of silicon nitride.
[0037] Preferably, the thickness of the passivation layer is 80 nm to 120 nm.
[0038] A second aspect of the present invention provides a crystalline silicon solar cell, which is prepared by the preparation method described in the first aspect.
[0039] Compared with the prior art, the present invention has at least the following beneficial effects:
[0040] The improved crystalline silicon solar cell preparation method provided by the present invention uses etching to open the silicon substrate, which can completely open the passivation layer, and the damage to the PN junction on the silicon substrate is also small. The silicon leaked from the opened area presents a porous structure, which is conducive to the deposition of the nickel plating layer and helps to improve the open circuit voltage of the electroplated solar cell. Laser-assisted nickel plating is used on the front and back sides. Through the precise control of the laser beam, the fine regulation of the electroplating process is achieved, and highly selective metal deposition is achieved, which reduces the damage to the silicon substrate, optimizes the uniformity and adhesion of the metal layer, and further improves the photoelectric conversion efficiency of the solar cell.
[0041] The crystalline silicon solar cell provided by the present invention, in view of the advantages brought by the above-mentioned preparation method, has a higher open circuit voltage, better performance, and higher efficiency, which expands the application scenarios of crystalline silicon solar cells and promotes the development of downstream industries. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0043] Hereinafter, the terms "including", "having" and their cognates, which may be used in various embodiments of the present invention, are intended only to indicate specific features, numbers, steps, operations, elements, components or combinations of the foregoing items, and should not be understood as first excluding the existence of one or more other features, numbers, steps, operations, elements, components or combinations of the foregoing items or adding the possibility of one or more features, numbers, steps, operations, elements, components or combinations of the foregoing items.
[0044] The first aspect of the present invention provides an improved method for preparing a crystalline silicon solar cell, wherein patterned grooves are etched on the front and back sides of a silicon substrate of the solar cell, and then nickel is electroplated on the back side of the silicon substrate by light-induced electroplating, and nickel is electroplated on the front side of the silicon substrate by laser-assisted electroplating, and finally, a double-sided nickel-plated silicon substrate with nickel plated on both the front and back sides is electroplated with a copper layer and a silver layer on both sides to obtain a double-sided electroplated crystalline silicon solar cell.
[0045] The improved crystalline silicon solar cell preparation method provided by the present invention uses etching to open the silicon substrate, which can completely open the passivation layer, and the damage to the PN junction on the silicon substrate is also small. The silicon leaked from the opened area presents a porous structure, which is conducive to the deposition of the nickel plating layer and helps to improve the open circuit voltage of the electroplated solar cell. Laser-assisted nickel plating is used on the front and back sides. Through the precise control of the laser beam, the fine regulation of the electroplating process is achieved, and highly selective metal deposition is achieved, which reduces the damage to the silicon substrate, optimizes the uniformity and adhesion of the metal layer, and further improves the photoelectric conversion efficiency of the solar cell.
[0046] Furthermore, the etching is performed by screen printing a corrosion slurry and drying and sintering it.
[0047] The use of screen printing technology can precisely control the distribution of etching slurry, ensuring the uniformity and accuracy of the etching process. Water-based acrylic resin as part of the etching slurry is more environmentally friendly than oily materials, reducing volatile organic compound (VOC) emissions during the production process. The added thixotropic agent can improve the stability and thixotropy of the slurry, reduce sedimentation and flow during the printing process, and thus improve the printing quality. The acid contained in the etching slurry enables fast and effective etching. The temperature and time of drying and sintering ensure the curing and etching effect of the etching slurry, while avoiding material damage caused by over-sintering. The drying and sintering time is short, only 1 to 3 minutes, which can significantly improve production efficiency and reduce energy consumption.
[0048] Preferably, the etching slurry comprises 10wt.% to 20wt.% of water-based acrylic resin, 0.5wt.% to 3.0wt.% of thixotropic agent, 15wt.% to 25wt.% of acid, 10wt.% to 30wt.% of filler, and the balance is solvent.
[0049] In the etching slurry, typically but not limiting, the content of the water-based acrylic resin can be 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.%, 15wt.%, 16wt.%, 17wt.%, 18wt.%, 19wt.% or 20wt.%, or any value within the range of 10wt.% to 20wt.%; the content of the thixotropic agent can be 0.5wt.%, 0.6wt.%, 0.7wt.%, 0.8wt.%, 0.9wt.%, 1.0wt.%, 1.5wt.%, 2.0wt.%, 2.5wt.%, 2.8wt.% or 3.0wt.%, or any value within the range of 0.5wt.% to 3.0wt.%; the content of the acid can be 15wt.%, %, 16wt.%, 17wt.%, 18wt.%, 19wt.%, 20wt.%, 21wt.%, 22wt.%, 23wt.% or 24wt.%, 25wt.%, or any value within the range of 15wt.% to 25wt.%; the content of the filler can be 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.%, 15wt.%, 16wt.%, 17wt.%, 18wt.%, 19wt.%, 20wt.%, 21wt.%, 22wt.%, 23wt.%, 24wt.%, 25wt.%, 26wt.%, 27wt.%, 28wt.%, 29wt.% or 30wt.%, or any value within the range of 10wt.% to 30wt.%. The amount of solvent was adjusted according to the amounts of the above substances to make up 100 wt.%.
[0050] Preferably, the thixotropic agent comprises a polyamide wax thixotropic agent.
[0051] Preferably, the acid includes at least one of hydrofluoric acid, phosphoric acid, nitric acid, pyrophosphoric acid and sulfurous acid.
[0052] Preferably, the filler includes at least one of alumina, silica powder, kaolin, titanium dioxide, aluminum hydroxide and calcium carbonate.
[0053] Preferably, the solvent comprises at least one of ethanol, acetic acid, ethyl acetate, ethylene glycol and glycerol.
[0054] Preferably, the drying and sintering temperature is 300° C. to 400° C., and the time is 1 min to 3 min.
[0055] Typically but not restrictively, the temperature during the drying and sintering process can be, for example, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, or any value in the range of 300°C to 400°C; the drying and sintering time can be, for example, 1 min, 1.5 min, 2 min or 3 min, or any value in the range of 1 min to 3 min.
[0056] Furthermore, the specific process of the light-induced nickel electroplating is:
[0057] The back side of the silicon substrate is in contact with the electrolyte as the cathode, and the pure nickel plate is used as the anode. The anode is placed below the cathode, and the nickel plating solution is used as the electrolyte. The DC power supply and the light source are turned on for light-induced constant current electroplating. At the same time, the laser is turned on to emit a Gaussian laser beam, which is focused by the focusing lens and irradiated through the electrolyte to the back side of the silicon substrate after being expanded by the beam expander and reflected by the total reflection mirror. The grooves are scanned according to the set pattern, and the electroplating is stopped after the scanning.
[0058] It should be noted that during the electroplating of the nickel layer on the back of the silicon substrate, since the silicon material itself is a semiconductor rather than a conductor, its own non-conductivity is not enough to ensure the effective flow of current during the electroplating process, hindering the flow of current. In order to overcome these problems, light-induced irradiation is required, and then the P region on both sides of the PN junction generates holes, the N region generates electrons, and the electrons in the N region are used to reduce the nickel metal to complete the deposition of the nickel layer.
[0059] By using a laser beam to scan the grooves on the back of the silicon substrate, precise control of the electroplating process can be achieved, ensuring that the nickel layer is formed only in specific areas to obtain the desired pattern and structure. Light-induced electroplating technology ensures the formation of current paths and improves the uniformity and quality of the electroplated layer by focusing and scanning the laser beam.
[0060] Preferably, the light source of the light-induced electroplating includes a halogen lamp, an LED lamp, an incandescent lamp or a mercury lamp.
[0061] Furthermore, the specific process of laser-assisted nickel electroplating is as follows:
[0062] The front side of the silicon substrate is in contact with the electrolyte as the cathode, and the pure nickel plate is used as the anode. The anode is placed below the cathode, and the nickel plating solution is used as the electrolyte. The DC power supply is turned on for constant current electroplating. At the same time, the laser is turned on to emit a Gaussian laser beam. After being expanded by a beam expander and reflected by a total reflection mirror, it is focused by a focusing lens and irradiated to the front side of the silicon substrate through the electrolyte. The grooves are scanned according to the set pattern, and the electroplating is stopped after the scanning is completed.
[0063] Laser-assisted nickel electroplating is used for nickel plating on both the front and back sides. When the laser scans the surface of the silicon substrate of the solar cell, the nickel plating solution and the silicon substrate absorb the laser energy, causing the temperature of the scanned area on the silicon substrate surface and the surrounding solution to rise rapidly, resulting in a large temperature gradient, which accelerates the deposition rate of the nickel layer. The nickel grains are small and uniform during the electroplating process, the surface is flat and dense, and the bonding strength between the nickel layer and the silicon substrate is better, thereby improving the bonding strength of the plating layer of the electroplated solar cell.
[0064] The laser beam can be precisely focused and irradiated to a specific area on the back of the silicon substrate, achieving precise control of the electroplating process and ensuring that the nickel layer is formed only in the designed groove area. Through the guidance of the laser beam, the electroplating process can only occur in the required area, avoiding unnecessary deposition in unnecessary areas and improving the selectivity of electroplating. The laser scanning speed is fast and the scanning of the groove can be completed in a short time, shortening the production cycle and improving production efficiency.
[0065] Furthermore, the nickel electroplating solution includes 100 g / L to 300 g / L nickel sulfate hexahydrate, 40 g / L to 100 g / L nickel chloride hexahydrate, 30 g / L to 60 g / L boric acid, 1 g / L to 4 g / L saccharin sodium, and 0.1 g / L to 0.5 g / L wetting agent.
[0066] By precisely controlling the concentrations of nickel sulfate hexahydrate, nickel chloride hexahydrate, boric acid, sodium saccharin and wetting agents, the stability of the plating solution and the uniformity of the electroplating process can be ensured. The concentrations of the plating solution components help to form a uniform, dense and highly adherent nickel layer, improving the quality and durability of the electroplated layer. The addition of boric acid can buffer the pH value of the solution, maintain the stability of the plating solution and extend its service life. The addition of a wetting agent can improve the wettability of the plating solution on the surface of the silicon substrate, reduce the formation of air bubbles, improve pitting and pinholes, and improve electroplating efficiency. Typically but not limiting, in the nickel electroplating solution, the concentration of the nickel sulfate hexahydrate may be, for example, 100 g / L, 150 g / L, 200 g / L or 300 g / L, or any value within the range of 100 g / L to 300 g / L; the concentration of the nickel chloride hexahydrate may be, for example, 40 g / L, 60 g / L, 80 g / L or 100 g / L, or any value within the range of 40 g / L to 100 g / L; the concentration of the boric acid may be, for example, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L or 80 g / L, or any value within the range of 40 g / L to 100 g / L. The concentration of sodium saccharin can be, for example, 1g / L, 2g / L, 3g / L or 4g / L, or any value within the range of 1g / L to 4g / L; the concentration of the wetting agent can be, for example, 0.1g / L, 0.2g / L, 0.3g / L, 0.4g / L or 0.5g / L, or any value within the range of 0.1g / L to 0.5g / L.
[0067] Preferably, the wetting agent includes at least one of sodium n-octyl sulfate, sodium 2-ethylhexyl sulfate, sodium salt of sulfosuccinate, and sodium salt of diethyl sulfosuccinate.
[0068] Preferably, the temperature of the nickel electroplating solution is 40° C. to 50° C., and the pH value is 3.5 to 4.0.
[0069] The temperature and pH range of the plating solution help optimize the kinetics of the plating reaction, improve the plating rate and coating quality. By adjusting the current density and plating time, the thickness and deposition rate of the nickel layer can be precisely controlled to meet the needs of different applications. Under the premise of ensuring the quality of the plating, by adjusting the current density and time, the plating cycle can be shortened and the production efficiency can be improved.
[0070] Typically but not limiting, the temperature of the nickel electroplating solution can be, for example, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C, or any value in the range of 40°C to 50°C; the pH value of the nickel electroplating solution can be, for example, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3 or 4.4, or any value in the range of 3.5 to 4.0.
[0071] Preferably, the current density of the light-induced constant current plating or the constant current plating is independently 5A / dm 2 ~10A / dm 2 The time for each is independent and ranges from 5s to 12s.
[0072] Typically, but not limiting, the current density may be, for example, 5 A / dm 2 、6A / dm 2 , 7A / dm 2 , 8A / dm 2 、9A / dm 2 or 10A / dm 2 , or 5A / dm 2 ~10A / dm 2 The electroplating time can be, for example, 5s, 6s, 7s, 8s, 9s, 10s, 11s or 12s, or any value within the range of 5s to 12s.
[0073] It should be noted that “independently” means that the current density of the light-induced constant current plating on the back side or the constant current plating on the front side is in the same range, but the specific values can be the same or different, and there is no correlation between the two values.
[0074] Furthermore, the laser is a picosecond fiber laser with a wavelength of 355nm. The high energy density of the picosecond fiber laser helps to achieve fast and efficient material processing, especially in the field of micro-processing. The picosecond laser with a wavelength of 355nm can provide high-precision processing capabilities and is suitable for fine micro-structure processing.
[0075] Preferably, the light spot of the laser is a point-shaped light spot, the diameter of the light spot is 10 μm to 20 μm, and the distance between the light spots is -1 μm to 1 μm.
[0076] The diameter of the spot, the rate of laser scanning, the frequency power, and the pulse width can achieve fine processing details, control the density and coverage of the processing pattern, and avoid thermal effects caused by excessive power.
[0077] Typically but not restrictively, the spot diameter can be, for example, 10μm, 12μm, 14μm, 16μm, 18μm or 20μm, or any value in the range of 10μm to 20μm; the spot spacing can be, for example, -1μm, 0μm, 1μm, or any value in the range of -1μm to 1μm.
[0078] Preferably, the scanning rate of the laser is 3000 mm / s to 8000 mm / s, the frequency is 50 kHz to 500 kHz, the average power is 1 W to 3 W, and the pulse width is 10 ns to 50 ns.
[0079] Typically but not limiting, the scanning rate of the laser can be, for example, 3000 mm / s,
[0080] 4000mm / s, 5000mm / s, 6000mm / s, 7000mm / s or 8000mm / s, or any value within the range of 3000mm / s to 8000mm / s; the frequency of the laser can be, for example, 50kHz,
[0081] 100kHz, 150kHz, 200kHz, 250kHz, 300kHz, 350kHz, 400kHz or 500kHz, or any value in the range of 50kHz to 500kHz; the average power of the laser can be, for example, 1W, 1.5W, 2W or 3W, or any value in the range of 1W to 3W; the pulse width of the laser can be, for example, 10ns, 20ns, 30ns, 40ns or 50ns, or any value in the range of 10ns to 50ns.
[0082] Furthermore, the thickness of the nickel layer formed by light-induced nickel electroplating on the back side of the silicon substrate is 0.8 μm to 1.2 μm.
[0083] Typically but not limiting, the thickness of the back nickel layer may be, for example, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm or 1.2 μm, or any value within the range of 0.8 μm to 1.2 μm.
[0084] Preferably, the nickel layer formed by laser-assisted nickel electroplating on the front side of the silicon substrate has a thickness of 0.8 μm to 1.2 μm.
[0085] The thickness of the nickel layer is between 0.8μm and 1.2μm, which can enhance the bonding strength with the base material and improve the durability and reliability of the final product. Moreover, as a conductive layer, the thickness of the nickel layer has a direct impact on the conductivity, and the appropriate thickness can ensure good conductivity. The nickel layer can be used as a shielding layer to reduce electromagnetic interference, and the appropriate thickness helps to improve the shielding effect.
[0086] Typically but not restrictively, the thickness of the front nickel layer may be, for example, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm or 1.2 μm, or any value within the range of 0.8 μm to 1.2 μm.
[0087] Furthermore, the thickness of the copper layer is 8 μm to 10 μm. Typically but not limiting, the thickness of the copper layer may be, for example, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, or any value within the range of 8 μm to 10 μm.
[0088] Preferably, the thickness of the silver layer is 1 μm to 2 μm.
[0089] Typically but not limiting, the thickness of the silver layer may be, for example, 1 μm, 1.5 μm or 2 μm, or any value within the range of 1 μm to 2 μm.
[0090] The copper layer thickness is in the range of 8μm to 10μm, which can provide high electrical and thermal conductivity and is suitable as a conductive and heat dissipation layer. The silver layer thickness is controlled at 1μm to 2μm. Although it is thin, silver has extremely high conductivity and can be used in applications that require high electrical conductivity. The moderate thickness of the copper and silver layers can improve the reliability of welding and the strength of the solder joints.
[0091] Furthermore, the passivation layer is etched on the solar cell silicon substrate to form a patterned groove.
[0092] Preferably, the passivation layer is made of silicon nitride.
[0093] Preferably, the thickness of the passivation layer is 80 nm to 120 nm.
[0094] Typically but not limiting, the thickness of the passivation layer may be, for example, 80 nm, 90 nm, 100 nm, 110 nm or 120 nm, or any value within the range of 80 nm to 120 nm.
[0095] Typically but not limiting, the width of the patterned groove may be, for example, 20 μm, 30 μm, 40 μm, 50 μm or 60 μm, or any value within the range of 20 μm to 60 μm.
[0096] By forming patterned grooves on the silicon substrate, the scattering and absorption of light can be increased, thereby improving the photoelectric conversion efficiency of solar cells. The thickness of the passivation layer is controlled within the range of 80nm to 120nm, which can ensure the passivation effect while avoiding the negative impact of an excessively thick passivation layer on the absorption and scattering of light. By accurately etching the patterned grooves, defects in the battery manufacturing process can be reduced and the overall reliability of the battery can be improved.
[0097] A second aspect of the present invention provides a crystalline silicon solar cell, which is prepared by the preparation method described in the first aspect.
[0098] The crystalline silicon solar cell provided by the present invention, in view of the advantages brought by the above-mentioned preparation method, has a higher open circuit voltage, better performance, and higher efficiency, which expands the application scenarios of crystalline silicon solar cells and promotes the development of downstream industries.
[0099] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. The raw materials used in the examples and comparative examples of the present invention, if no specific conditions are specified, are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.
[0100] Example 1
[0101] This embodiment provides a crystalline silicon solar cell, and the preparation method is as follows:
[0102] 1. Provide an N-type TOPCon solar cell silicon substrate with a size of 210 mm×210 mm. A silicon nitride passivation layer is deposited on the surface of the silicon substrate, and the thickness of the passivation layer is controlled to be 100 nm.
[0103] 2. Use screen printing technology to print the etching slurry on the front and back of the silicon substrate to remove the silicon nitride passivation layer to form a patterned groove. After printing, the silicon substrate is dried and sintered at a temperature of 350°C for 2 minutes. Subsequently, the silicon substrate is soaked in hot water for a period of time and cleaned with spray water at a temperature of 90°C for 4 minutes. The width of the patterned groove is 40μm.
[0104] The components of the etching slurry include 15wt.% of water-based acrylic resin, 1.6wt.% of polyamide wax thixotropic agent, 20wt.% of hydrofluoric acid, 20wt.% of aluminum oxide, and the balance is ethanol.
[0105] 3. The front side of the silicon substrate with the patterned grooves is sucked by a vacuum chuck, and the back side is floated on the nickel electroplating solution as the cathode, and a pure nickel plate is placed under the cathode as the anode. The temperature of the nickel electroplating solution is 45°C and the pH value is 3.7. Turn on the DC power supply, halogen lamp and picosecond fiber laser for light-induced electroplating. The current density of electroplating is 7A / dm 2 , the time is 8 seconds.
[0106] Among them, the picosecond fiber laser emits a Gaussian laser beam with a wavelength of 355nm, a point-shaped spot, a diameter of 15μm, and a spot spacing of 1μm. After the laser beam is expanded by a beam expander and reflected by a total reflector, it is focused by a focusing lens and irradiated onto the surface of the silicon substrate through the electroplating solution, and the grooves are scanned according to the set pattern. The scanning rate is 5000mm / s, the frequency is 300kHz, the average power is 2W, and the pulse width is 30ns. After the scanning is completed, the electroplating is stopped to obtain a solar cell silicon substrate with nickel plating on the back, and the thickness of the nickel plating is 1μm.
[0107] The concentration of the nickel electroplating solution is: 200 g / L nickel sulfate hexahydrate, 70 g / L nickel chloride hexahydrate, 30-60 g / L boric acid, 2.3 g / L saccharin sodium, and 0.3 g / L sodium n-octyl sulfate.
[0108] 4. The back of the silicon substrate with the patterned grooves is sucked by a vacuum chuck, and the front side is floated on the nickel plating solution as the cathode, and the pure nickel plate is placed under the cathode as the anode. The parameters and steps of the front laser-assisted nickel plating are exactly the same as those in step 3, the only difference is that the halogen lamp does not need to be turned on during the nickel plating process.
[0109] 5. Several double-sided nickel-plated solar cells were retained without copper and silver plating, and used for the test in the subsequent test example 1. The remaining double-sided nickel-plated solar cell silicon substrates were subjected to double-sided electroplating of copper and silver. The thickness of the double-sided copper plating layer was 9 μm, and the thickness of the double-sided silver plating layer was 1 μm, to obtain a crystalline silicon solar cell.
[0110] Example 2
[0111] This embodiment provides a crystalline silicon solar cell, and the preparation method is as follows:
[0112] 1. Same as the step in Example 1.
[0113] 2. Use screen printing technology to print the etching slurry on the front and back of the silicon substrate to remove the silicon nitride passivation layer to form a patterned groove. After printing, the silicon substrate is dried and sintered at a temperature of 320°C for 2.5 minutes. Subsequently, the silicon substrate is soaked in hot water for a period of time and cleaned with spray water at a temperature of 90°C for 4 minutes. The width of the patterned groove is 30μm.
[0114] The components of the etching slurry include 18wt.% of water-based acrylic resin, 1wt.% of polyamide wax thixotropic agent, 18wt.% of hydrofluoric acid, 10wt.% of aluminum oxide, 10wt.% of silicon micropowder, and the balance is ethanol.
[0115] 3. The front side of the silicon substrate with the patterned grooves is sucked by a vacuum chuck, and the back side is floated on the nickel electroplating solution as the cathode, and the pure nickel plate is placed under the cathode as the anode. The temperature of the nickel electroplating solution is 43°C and the pH value is 3.5. Turn on the DC power supply, halogen lamp and picosecond fiber laser for light-induced electroplating. The current density of electroplating is 8A / dm 2 , time is 10 seconds.
[0116] Among them, the picosecond fiber laser emits a Gaussian laser beam with a wavelength of 355nm, a point-shaped spot, a diameter of 15μm, and a spot spacing of 1μm. After the laser beam is expanded by a beam expander and reflected by a total reflector, it is focused by a focusing lens and irradiated onto the surface of the silicon substrate through the electroplating solution, and the grooves are scanned according to the set pattern. The scanning rate is 5000mm / s, the frequency is 300kHz, the average power is 2W, and the pulse width is 30ns. After the scanning is completed, the electroplating is stopped to obtain a solar cell silicon substrate with nickel plating on the back, and the thickness of the nickel plating is 1μm.
[0117] The concentration of the nickel electroplating solution is: 200 g / L nickel sulfate hexahydrate, 70 g / L nickel chloride hexahydrate, 30-60 g / L boric acid, 2.3 g / L saccharin sodium, and 0.3 g / L sodium n-octyl sulfate.
[0118] 4. Same as the step in Example 1.
[0119] 5. Same as the step in Example 1.
[0120] Example 3
[0121] This embodiment provides a crystalline silicon solar cell, which is different from the embodiment 1 in that in step 2, the temperature of drying and sintering the silicon substrate is 300° C., the time is 3 minutes, and the width of the patterned groove formed is 50 μm. The remaining steps and operating parameters are the same as those in the embodiment 1 and will not be repeated here.
[0122] Example 4
[0123] This embodiment provides a crystalline silicon solar cell, which is different from the embodiment 1 in that in step 2, the temperature of drying and sintering the silicon substrate is 400° C., the time is 1 minute, and the width of the patterned groove formed is 30 μm. The remaining steps and operating parameters are the same as those in the embodiment 1 and will not be repeated here.
[0124] Example 5
[0125] This embodiment provides a crystalline silicon solar cell, which is different from the embodiment 1 in that in step 2, the temperature of drying and sintering the silicon substrate is 200° C., the time is 3 minutes, and the width of the patterned groove formed is 15 μm. The remaining steps and operating parameters are the same as those in the embodiment 1 and will not be repeated here.
[0126] Example 6
[0127] This embodiment provides a crystalline silicon solar cell, which is different from the embodiment 1 in that in step 2, the temperature of drying and sintering the silicon substrate is 500° C., the time is 1 minute, and the width of the patterned groove formed is 50 μm. The remaining steps and operating parameters are the same as those in the embodiment 1 and will not be repeated here.
[0128] Example 7
[0129] This embodiment provides a crystalline silicon solar cell. The difference from the embodiment 1 is that in step 3 and step 4, the current density of electroplating is 5A / dm 2 , the time is 12 seconds, and the remaining steps and operating parameters are the same as those in Example 1 and will not be repeated here.
[0130] Example 8
[0131] This embodiment provides a crystalline silicon solar cell. The difference from the embodiment 1 is that in step 3 and step 4, the current density of electroplating is 10A / dm 2 , the time is 5 seconds, and the remaining steps and operating parameters are the same as those in Example 1 and will not be repeated here.
[0132] Example 9
[0133] This embodiment provides a crystalline silicon solar cell. The difference from the embodiment 1 is that in step 3 and step 4, the current density of electroplating is 15A / dm 2, the time is 3 seconds, and the remaining steps and operating parameters are the same as those in Example 1 and will not be repeated here.
[0134] Example 10
[0135] This embodiment provides a crystalline silicon solar cell. The difference from the embodiment 1 is that in step 3 and step 4, the current density of electroplating is 3A / dm 2 , the time is 15 seconds, and the remaining steps and operating parameters are the same as those in Example 1 and will not be repeated here.
[0136] Comparative Example 1
[0137] This comparative example provides a crystalline silicon solar cell, and the preparation method is as follows:
[0138] 1. Same as the step in Example 1.
[0139] 2. Use laser film opening to form patterned grooves, and the width of the patterned grooves is 40 μm.
[0140] 3. Same as the step in Example 1.
[0141] 4. Same as the step in Example 1.
[0142] 5. Same as the step in Example 1.
[0143] Comparative Example 2
[0144] This comparative example provides a crystalline silicon solar cell, and the preparation method is as follows:
[0145] 1. Same as the step in Example 1.
[0146] 2. Same as the step in Example 1.
[0147] 3. The front side of the silicon substrate with the patterned grooves is sucked by a vacuum chuck, and the back side is floated on the nickel electroplating solution as the cathode, and the pure nickel plate is placed under the cathode as the anode. The temperature of the nickel electroplating solution is 45°C and the pH value is 3.7. Turn on the DC power supply and halogen lamp for light-induced electroplating. The current density of electroplating is 7A / dm 2 , time is 8 seconds, and a solar cell silicon substrate with nickel plating on the back is obtained, and the thickness of the nickel plating layer is 1 μm.
[0148] The concentration of the nickel electroplating solution is: 200 g / L nickel sulfate hexahydrate, 70 g / L nickel chloride hexahydrate, 30-60 g / L boric acid, 2.3 g / L saccharin sodium, and 0.3 g / L sodium n-octyl sulfate.
[0149] 4. The back of the silicon substrate with the patterned grooves is sucked by a vacuum chuck, and the front side is floated on the nickel plating solution as the cathode, and the pure nickel plate is placed under the cathode as the anode. The parameters and steps of the front side nickel plating are exactly the same as those in step 3, the only difference is that the halogen lamp does not need to be turned on during the nickel plating process.
[0150] 5. Same as the step in Example 1.
[0151] Comparative Example 3
[0152] This comparative example provides a crystalline silicon solar cell, and the preparation method is as follows:
[0153] 1. Same as the step in Example 1.
[0154] 2. Use laser film opening to form patterned grooves, and the width of the patterned grooves is 40 μm.
[0155] 3. Same as the steps in Comparative Example 2.
[0156] 4. Same as the steps in Comparative Example 2.
[0157] 5. Same as the step in Example 1.
[0158] Test Example 1
[0159] The double-sided plated solar cells obtained in the examples and comparative examples were subjected to welding tensile test, and the test method was as follows:
[0160] (1) Coating bonding strength: 3M tape test
[0161] (2) Low temperature (200°C) welding tensile force: tensile tester test (double-sided electroplating involves testing the tensile force on the front and back sides. The tensile force on both sides is qualified when the average value of the 12 test points is ≥ 0.8N. The tensile force on the front side is higher than that on the back side).
[0162] The specific test results are shown in Table 1 (where “ / ” means welding cannot be completed):
[0163] Table 1
[0164]
[0165] As can be seen from Table 1, etching the silicon substrate can completely open the passivation layer, which is helpful for the deposition of the nickel plating layer. Laser-assisted nickel electroplating is used on the front and back sides. Through the precise control of the laser beam, the electroplating process can be finely controlled, highly selective metal deposition can be achieved, and the uniformity and adhesion of the metal layer are optimized.
[0166] Test Example 2
[0167] The crystalline silicon solar cells obtained in the embodiment and the comparative example were made into the same specifications and tested for electrical properties, including photoelectric conversion efficiency and open circuit voltage.
[0168] Specifically, IV testing was performed at a temperature of 25° C. and an AM of 1.5 G, and the obtained data is shown in Table 2 below.
[0169] Table 2
[0170] Eta(%) Uoc(V) Isc(A) FF(%) Rs(Ω) Example 1 26.36 0.720 18.54 87.01 0.00058 Example 2 26.34 0.721 18.50 87.08 0.00061 Example 3 26.23 0.719 18.51 86.89 0.00062 Example 4 26.26 0.720 18.53 86.59 0.00064 Example 5 24.37 0.705 18.27 83.56 0.00075 Example 6 25.85 0.714 18.53 86.02 0.00068 Example 7 26.27 0.722 18.52 86.59 0.00063 Example 8 26.16 0.721 18.50 86.55 0.00059 Example 9 26.03 0.719 18.43 86.69 0.00064 Example 10 26.07 0.721 18.38 86.74 0.00061 Comparative Example 1 25.86 0.714 18.51 86.25 0.00078 Comparative Example 2 18.17 0.706 18.47 61.47 0.00237 Comparative Example 3 13.97 0.702 18.57 47.22 0.00345
[0171] As can be seen from Table 2, the drying and sintering temperature of Example 5 is low, and the slotting effect is poor; the sintering temperature in Example 6 is high, resulting in a larger groove width and poorer accuracy of the patterned groove. In Comparative Example 2, the nickel layer is too thin, resulting in contact between copper and silicon, causing the series resistance to increase and the efficiency to deteriorate.
[0172] The silicon substrate is opened by etching, which can completely open the passivation layer and cause less damage to the PN junction on the silicon substrate, which helps to increase the open circuit voltage of the electroplated solar cell. Laser-assisted nickel plating is used on the front and back sides. Through the precise control of the laser beam, the electroplating process can be finely controlled, highly selective metal deposition can be achieved, the damage to the silicon substrate is reduced, and the photoelectric conversion efficiency of the solar cell is improved.
[0173] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. An improved method for preparing a crystalline silicon solar cell, characterized in that: Patterned grooves are etched on the front and back sides of the silicon substrate of the solar cell, and then nickel is electroplated on the back side of the silicon substrate by light-induced electroplating, and nickel is electroplated on the front side of the silicon substrate by laser-assisted electroplating. Finally, the double-sided nickel-plated silicon substrate with nickel plated on both the front and back sides is electroplated with copper and silver layers to obtain a double-sided electroplated crystalline silicon solar cell.
2. The preparation method according to claim 1, characterized in that: The etching is performed by screen printing a corrosion slurry and drying and sintering the slurry; Preferably, the etching slurry comprises 10wt.% to 20wt.% of water-based acrylic resin, 0.5wt.% to 3.0wt.% of thixotropic agent, 15wt.% to 25wt.% of acid, 10wt.% to 30wt.% of filler, and the balance is solvent; Preferably, the thixotropic agent comprises a polyamide wax thixotropic agent; Preferably, the acid comprises at least one of hydrofluoric acid, phosphoric acid, nitric acid, pyrophosphoric acid and sulfurous acid; Preferably, the filler comprises at least one of alumina, silica powder, kaolin, titanium dioxide, aluminum hydroxide and calcium carbonate; Preferably, the solvent comprises at least one of ethanol, acetic acid, ethyl acetate, ethylene glycol and glycerol; Preferably, the drying and sintering temperature is 300° C. to 400° C., and the time is 1 min to 3 min.
3. The preparation method according to claim 1, characterized in that: The specific process of the light-induced nickel electroplating is: The back of the silicon substrate is contacted with an electrolyte as a cathode, and a pure nickel plate is used as an anode. The anode is placed below the cathode, and the nickel plating solution is used as an electrolyte. A DC power supply and a light source are turned on to perform light-induced constant current electroplating. At the same time, a laser is turned on to emit a Gaussian laser beam, which is expanded by a beam expander and reflected by a total reflection mirror, and then focused by a focusing lens and irradiated to the back of the silicon substrate through the electrolyte. The grooves are scanned according to a set pattern, and electroplating is stopped after the scanning is completed. Preferably, the light source of the light-induced electroplating includes a halogen lamp, an LED lamp, an incandescent lamp or a mercury lamp.
4. The preparation method according to claim 1, characterized in that: The specific process of laser-assisted nickel electroplating is as follows: The front side of the silicon substrate is in contact with the electrolyte as the cathode, and the pure nickel plate is used as the anode. The anode is placed below the cathode, and the nickel plating solution is used as the electrolyte. The DC power supply is turned on for constant current electroplating. At the same time, the laser is turned on to emit a Gaussian laser beam. After being expanded by a beam expander and reflected by a total reflection mirror, it is focused by a focusing lens and irradiated to the front side of the silicon substrate through the electrolyte. The grooves are scanned according to the set pattern, and the electroplating is stopped after the scanning is completed.
5. The preparation method according to claim 3 or 4, characterized in that: The nickel electroplating solution comprises 100 g / L to 300 g / L nickel sulfate hexahydrate, 40 g / L to 100 g / L nickel chloride hexahydrate, 30 g / L to 60 g / L boric acid, 1 g / L to 4 g / L sodium saccharin, and 0.1 g / L to 0.5 g / L wetting agent; Preferably, the wetting agent comprises at least one of sodium n-octyl sulfate, sodium 2-ethylhexyl sulfate, sodium salt of sulfosuccinate, and sodium salt of diethyl sulfosuccinate; Preferably, the temperature of the nickel electroplating solution is 40°C to 50°C, and the pH is 3.5 to 4.0; Preferably, the current density of the light-induced constant current plating or the constant current plating is independently 5A / dm 2 ~10A / dm 2 The time for each is independent and ranges from 5s to 12s.
6. The preparation method according to claim 3 or 4, characterized in that: The laser is a picosecond fiber laser with a wavelength of 355nm; Preferably, the laser spot is a point spot with a spot diameter of 10 μm to 20 μm and a spot spacing of -1 μm to 1 μm; Preferably, the scanning rate of the laser is 3000 mm / s to 8000 mm / s, the frequency is 50 kHz to 500 kHz, the average power is 1 W to 3 W, and the pulse width is 10 ns to 50 ns.
7. The preparation method according to claim 1, characterized in that: The thickness of the nickel layer formed by light-induced nickel electroplating on the back of the silicon substrate is 0.8 μm to 1.2 μm; Preferably, the nickel layer formed by laser-assisted nickel electroplating on the front side of the silicon substrate has a thickness of 0.8 μm to 1.2 μm.
8. The preparation method according to claim 1, characterized in that: The thickness of the copper layer is 8 μm to 10 μm; Preferably, the thickness of the silver layer is 1 μm to 2 μm.
9. The preparation method according to claim 1, characterized in that: etching a passivation layer on a solar cell silicon substrate to form a patterned groove; Preferably, the material of the passivation layer is silicon nitride; Preferably, the thickness of the passivation layer is 80nm to 120nm; Preferably, the width of the patterned groove is 20 μm to 60 μm.
10. A crystalline silicon solar cell, characterized in that: The preparation method is described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method for improving electroplating quality of front electrode of solar cell
CN102222729A
Silicon solar cell front face electrode lead-free silver paste and preparing method thereof
CN104157332A
Producing method of selective emitter double-faced PERC crystalline silicon solar cell
CN106449876A
Contact hole-opening process for IBC batteries
CN106711244A
Femtosecond laser etching process method of perovskite thin film solar cell
CN112885968A