Zinc metastannate negative electrode material and preparation method and application thereof

By soaking zinc metastanate material in biphenyl-lithium-tetrahydrofuran prelithiation reagent to form SEI film, the problems of low efficiency and poor circulation stability of the first circle of zinc metastanate negative electrode material in lithium-ion batteries are solved, and the problem of low efficiency and poor circulation stability of zinc metastanate negative electrode material in lithium-ion batteries is achieved. Higher energy efficiency and improved battery performance.

CN118943306AActive Publication Date: 2024-11-12CHINA UNIV OF GEOSCIENCES (WUHAN)

Patent Information

Application Number
CN202411291897.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The first-round Coulomb efficiency of zinc metastanate negative electrode material in existing lithium-ion batteries is low, resulting in low energy efficiency and powdering and agglomeration during the cycle, affecting battery performance.

Method used

By soaking zinc metastannate material in prelithiation reagent for redox reaction, a uniform protective film is formed, and lithium ions are uniformly embedded in the anode, improving the efficiency and circulation stability of the first circle of Coulomb. The prelithiation reagent is composed of biphenyl-lithium-tetrahydrofuran to form a strong Li-Bp reducing agent to form an SEI film to protect the electrode surface.

Benefits of technology

It significantly improves the first-circle Coulomb efficiency and cycle stability of the negative electrode material, improves the energy efficiency and capacity retention rate of the battery, and improves the battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943306A_ABST
    Figure CN118943306A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, and particularly discloses a zinc metastannate negative electrode material and a preparation method and application thereof, and the preparation method comprises the following steps: S1, dissolving sodium stannate, zinc acetate and urea into a mixed solution of ethanol and deionized water, uniformly mixing, and carrying out hydrothermal treatment, centrifugal drying and calcination to obtain zinc metastannate powder; s2, dissolving a lithiation reagent and metal lithium in a tetrahydrofuran solvent to obtain a chemical pre-lithiation reagent solution, wherein the pre-lithiation reagent solution at least comprises biphenyl, lithium and tetrahydrofuran; and S3, putting the prepared zinc metastannate powder into a chemical pre-lithiation reagent solution for reaction or putting the prepared zinc metastannate powder into chemical pre-lithiation reagent steam for reaction, and collecting after vacuum drying to obtain the zinc metastannate negative electrode material. A uniform SEI film is generated on the surface of the zinc metastannate material through a pre-lithiation method, so that the surface of the material can be effectively protected, irreversible reaction is reduced, the first-circle coulombic efficiency and the cycling stability of the negative electrode material are improved, and the cycling performance can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a zinc metastannate negative electrode material and a preparation method and application thereof. Background Art

[0002] With the increasingly serious environmental problems and the growing demand for energy, various electrochemical energy storage systems (EES) have emerged and developed rapidly. Rechargeable metal ion batteries are considered to be one of the most promising electrochemical energy storage systems due to their advantages such as high energy consumption and high battery life. Lithium-ion batteries (LIBs) are the most representative rechargeable metal ion batteries due to their outstanding advantages, including high energy density, no memory effect, and low self-discharge. They are widely used in portable electronic devices, electric vehicles, grid energy storage and other fields. It should be noted that the electrochemical performance of these batteries mainly depends on the electrode materials. In order to meet market demand, it is necessary to develop batteries with higher specific capacity (>600mAh·g -1 ), a negative electrode material with stable capacity and excellent rate performance.

[0003] Zinc stannate (ZnSnO3) is a multifunctional ternary metal oxide material that has long been a popular functional material in the fields of chemistry and physics, such as lead-free ferroelectrics, transparent conductors, photocatalysts, dye-sensitized solar cells, and gas sensors. In recent years, it has attracted great attention due to its ultra-high theoretical capacity (1317 mAh g -1 ), lower working potential, it is considered to be a very promising negative electrode candidate material for lithium-ion batteries. More importantly, as a bimetallic oxide, it also has higher intrinsic advantages than single metal zinc oxide (ZnO) and tin dioxide (SnO2), especially its adjustable working potential and higher electronic conductivity.

[0004] However, there is limited research on zinc metastannate as anode material for lithium-ion batteries. The main reason is that the first-cycle coulombic efficiency of zinc metastannate is too low, which makes the energy efficiency of the battery too low. Powdering and agglomeration will also occur during the cycle, resulting in poor battery performance. Therefore, the development of a method for efficiently modifying zinc metastannate materials is of great significance for the development of negative electrode materials for lithium-ion batteries. The pre-lithiation technology is a method of adding a small amount of lithium source to the electrode material before the battery is officially charged and discharged. It compensates for the formation of the solid electrolyte interface during the first cycle reaction and the lithium loss caused by the side reaction, so as to achieve the first cycle coulombic efficiency and increase the reversible capacity. So far, predecessors have done a lot of research on pre-lithiation. The commonly used pre-lithiation method for the negative electrode is to directly supplement lithium to the negative electrode, such as lithium foil supplementation. This method seems to be easy to implement, but the lithium ions are not evenly distributed on the anode, so the effect is not good. Another alternative method is electrochemical pre-lithiation. The lithium foil as the counter electrode forms a half-cell, and pre-lithiation is achieved by discharge or short circuit. This approach allows control over the extent of pre-lithiation, but the operations involved in half-cell assembly and disassembly make it more complicated to implement. Summary of the invention

[0005] The object of the present invention is to provide a zinc metastannate negative electrode material and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art, which is achieved by immersing the negative electrode material in a pre-lithiation agent and then drying and collecting it. In this process, a redox reaction is involved, and lithium ions are uniformly embedded in the anode. The pre-lithiation agent is usually composed of a strong reducing substance (such as lithium naphthalene (Li-Naph) and lithium biphenyl) and an ether solvent (such as tetrahydrofuran and dimethoxyethane), so that a uniform protective film is generated on its surface, which can effectively protect the electrode surface and reduce the occurrence of irreversible reactions, thereby improving the first-cycle coulomb efficiency and cycle stability of the negative electrode material.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] The first object of the present invention is to provide a method for preparing a zinc metastannate negative electrode material, comprising the following steps:

[0008] S1: dissolving appropriate amounts of sodium stannate, zinc acetate and urea into a mixed solution of ethanol and deionized water, uniformly mixing, hydrothermally drying, centrifugally drying and calcining to obtain zinc metastannate powder;

[0009] S2: dissolving a lithiation reagent and metallic lithium in a tetrahydrofuran solvent to obtain a chemical pre-lithiation reagent solution, wherein the pre-lithiation reagent solution comprises at least biphenyl, lithium, and tetrahydrofuran;

[0010] S3: placing the prepared zinc metastannate powder in a chemical pre-lithiation reagent solution for reaction or placing it in a chemical pre-lithiation reagent vapor, and collecting it after vacuum drying to obtain a chemical pre-lithiation zinc metastannate negative electrode material.

[0011] Furthermore, the molar ratio of tin and zinc added to the drug in S1 is 1:1, and the volume ratio of ethanol and deionized water is 1:(1-3);

[0012] Furthermore, the mixing method in S1 is any one of stirring and ultrasound, and the mixing time is 0.1 to 3 hours;

[0013] Furthermore, the hydrothermal conditions in S1 are a temperature of 150 to 180° C. and a time of 4 to 6 hours;

[0014] Furthermore, the centrifugal conditions are a rotation speed of 7200-7800 r / min, a time of 3-5 min, a drying treatment is any one of normal pressure drying, reduced pressure drying, spray drying, microwave drying, and infrared drying, and a drying temperature is 40-120°C.

[0015] Furthermore, the calcination conditions are a temperature of 450-650° C., a heating rate of 2-10° C. / min, a calcination time of 2-6 hours, and a calcination atmosphere of dry air, nitrogen, or argon, followed by natural cooling to room temperature to obtain the product.

[0016] Further, in step S2, the pre-lithiation solvent includes at least one or more of tetrahydrofuran, ethylene glycol dimethyl ether, methyl propyl ether, methyl butyl ether, methyl amyl ether, ethyl propyl ether, ethyl butyl ether, ethyl amyl ether, propyl butyl ether, propyl amyl ether, methyltetrahydrofuran, dimethyltetrahydrofuran, ethyltetrahydrofuran, diethyltetrahydrofuran, phenyltetrahydrofuran, 1,2-dimethoxyethane and diethylene glycol dimethyl ether.

[0017] Further, in step S2, the lithiation reagent includes at least one or more of biphenyl, naphthalene, methylnaphthalene, dimethylnaphthalene, tetramethylnaphthalene, anthracene, methylanthracene, dimethylanthracene, tetramethylanthracene, phenanthrene, methylphenanthrene, dimethylphenanthrene, trimethylphenanthrene, tetramethylphenanthrene, pyrene, methylpyrene, dimethylpyrene, trimethylpyrene, tetramethylpyrene, methylpyrene, dimethylpyrene, trimethylpyrene, tetramethylpyrene, methylpyrene, dimethylpyrene, trimethylpyrene, tetramethylpyrene, methylbiphenyl, dimethylbiphenyl and tetramethylbiphenyl.

[0018] Further, in step S2, the metallic lithium includes at least one or more of lithium sheets and lithium ribbons.

[0019] Furthermore, in step S3, the reaction time in the chemical pre-lithiation reagent solution is 5 to 60 minutes.

[0020] Further, in step S3, the concentration of the pre-lithiation reagent is 1 mol / L, 1.5 mol / L, and 0.5 mol / L.

[0021] Furthermore, in step S3, pre-lithiation steam is introduced into the steam chamber, and the zinc metastannate negative electrode sheet passes through and is exposed to the steam chamber, and the exposure time in the steam chamber is 20 minutes.

[0022] Furthermore, in step S3, the liquid pre-lithiation reagent is heated and a carrier gas is introduced to form pre-lithiation steam, wherein the steam temperature is between the boiling point of the pre-lithiation reagent ±40°C.

[0023] Further, in step S3, the zinc metastannate negative electrode plate includes at least the following components: 50-99wt% of zinc metastannate negative electrode material, 0.5-40wt% of conductive agent, and 0.5-10wt% of binder.

[0024] Further, in step S3, the conductive agent includes at least one or more of acetylene black, Ketjen black, Super P, MCMB, and carbon nanotubes.

[0025] Further, in step S3, the binder includes at least one or more of polyvinylidene fluoride, polyvinyl chloride, polyvinyl butyral, polyacrylonitrile, polyacrylic acid, polyethylene glycol, polypyrrole, polyaniline, sucrose, glucose, maltose, citric acid, asphalt, furfural resin, epoxy resin, phenolic resin, sodium alginate and carboxymethyl cellulose.

[0026] The second object of the present invention is to provide a zinc metastannate negative electrode material obtained by the above preparation method.

[0027] The third object of the present invention is to provide a zinc metastannate negative electrode sheet, which is obtained by fully mixing the above-mentioned zinc metastannate material, binder, and conductive carbon in a certain proportion, then coating it on a copper foil material, and drying and cutting it.

[0028] Furthermore, the zinc metastannate negative electrode plate includes at least the following components: 50-99wt% zinc metastannate negative electrode material, 0.5-40wt% conductive agent, and 0.5-10wt% binder. The conductive agent includes at least one or more of acetylene black, Ketjen black, Super P, MCMB, and carbon nanotubes; the binder includes at least one or more of polyvinylidene fluoride, polyvinyl chloride, polyvinyl butyral, polyacrylonitrile, polyacrylic acid, polyethylene glycol, polypyrrole, polyaniline, sucrose, glucose, maltose, citric acid, asphalt, furfural resin, epoxy resin, phenolic resin, sodium alginate and carboxymethyl cellulose.

[0029] The fourth object of the present invention is to provide an electrode, comprising the above-mentioned zinc metastannate negative electrode sheet.

[0030] A fifth object of the present invention is to provide a lithium ion secondary battery comprising the above-mentioned electrode.

[0031] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0032] The present invention proposes a method for preparing a zinc metastannate negative electrode material, which utilizes the relative stability of the pre-lithiation reagent made of biphenyl-lithium-tetrahydrofuran in ambient air and the unique electrochemical behavior of biphenyl in ether and carbonate solvents. In ether solvents (e.g., tetrahydrofuran and dimethoxyethane), it can react with lithium metal and form a strong reducing agent of Li-Bp (biphenyl-lithium). In addition, the obtained pre-lithiation reagent is relatively less disturbed by air and moisture. The pre-lithiation method generates a uniform SEI film on the surface of the zinc metastannate material, which can effectively protect the surface of the material and reduce the occurrence of irreversible reactions, thereby improving the first-cycle coulomb efficiency and cycle stability of the negative electrode material and improving the cycle performance; in addition, the pre-lithiation method used allows lithium ions to be successfully embedded in the anode, which can controllably and uniformly compensate for the irreversible lithium loss to achieve a higher first-cycle coulomb efficiency, thereby effectively modifying the battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1a and Figure 1b These are pictures of zinc metastannate material at different magnifications under a scanning electron microscope (SEM);

[0034] Figure 2 This is the XRD comparison diagram of zinc stannate material and its precursor ZnSn(OH)6;

[0035] Figure 3 This is a schematic diagram of the first three cycles of charge and discharge of untreated zinc metastannate material in the voltage range of 0.01V-3V;

[0036] Figure 4 Schematic diagram of the first three charge and discharge cycles of the zinc metastannate material in the voltage range of 0.01V-3V after pre-lithiation in Example 1;

[0037] Figure 5 Schematic diagram of the first cycle coulombic efficiency of batteries assembled with zinc metastannate negative electrode materials in different embodiments;

[0038] Figure 6 The XPS spectra of Example 1 before and after pre-lithiation are compared;

[0039] Figure 7 This is a cross-sectional view of an untreated zinc metastannate negative electrode sheet;

[0040] Figure 8 This is the interface diagram of the zinc stannate negative electrode after steam pre-lithiation treatment. DETAILED DESCRIPTION

[0041] To make the present invention easier to understand, the present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. Unless otherwise defined, the professional terms used below are consistent with the meanings understood by professional and technical personnel in the field; unless otherwise specified, the raw materials and reagents involved in the present invention can be purchased from the market or prepared by known methods.

[0042] The preparation process of the zinc metastannate electrode used in the embodiment is as follows:

[0043] Material preparation: 0.425g of sodium stannate and 0.367g of anhydrous zinc acetate were dissolved in two beakers of 15ml ethanol and deionized water respectively, with the volume ratio of ethanol to deionized water being 1:1. After stirring for 5h, the two solutions were mixed, and then 3.5g of urea was added. After continuing to stir for 3h, the mixed solution was poured into a 50ml reactor for hydrothermal reaction. The hydrothermal conditions were 170℃ for 5h, and then ethanol and deionized water were used for multiple centrifugation at 7500r / min. Subsequently, the powder was vacuum dried at 90℃, and the dried powder was heated to 400℃ at 5℃ / min in a dry air atmosphere, calcined for 3h, and naturally cooled to obtain zinc metastannate powder material.

[0044] Pre-lithiation step: Under the protection of an inert atmosphere, place an appropriate amount of zinc metastannate material in a 1M chemical pre-lithiation solution for reaction for 5 to 60 minutes. After the reaction is completed, vacuum dry and collect the pre-lithiation zinc metastannate material.

[0045] Preparation of electrode: Zinc metastannate powder (or pre-lithiation zinc metastannate powder), conductive carbon black (Super P) and binder (PVDF) are weighed and mixed in a weight ratio of 7:2:1, and dimethylpyrrolidone (NMP) is added as a solvent to mix and stir into a uniform slurry. The slurry is evenly applied on the copper foil, dried at 80℃ for 12h, and the electrode sheet is cut into discs with a diameter of 12mm. The loading amount of active material on each disc is about 1-3mg / cm 2 The disc is the desired zinc metastannate negative electrode.

[0046] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), with metallic lithium as the negative electrode, a glass fiber membrane (GE Whatman) as the separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte, were assembled into CR2032 button cells in an argon glove box.

[0047] Battery electrical performance test: The assembled battery was tested using the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The anode film load density was about 1 mg cm -2 ~3mg cm -2 The specific capacity is calculated based on the amount of lithium metal oxide components in the anode film (i.e., the weight after removing the weight of conductive carbon black, binder, and carbon coating), and the test conditions are as follows: the charge and discharge voltage range is 0.01V to 3V, and constant current charge and discharge tests are performed at a current density of 0.5C or a current density of 1C.

[0048] X-ray diffraction (XRD) test: The test was conducted using a D8 Focus X-ray powder diffractometer from Bruker, Japan, Germany, using Cu-Kα as the radiation source with a wavelength of 1.5046λ; using a Ni filter, a tube current of 40mA, a tube voltage of 40KV, a scanning range of 20° to 80°, a scanning speed of 5° / min, and a step length of 0.05°. The material was placed on a glass slide and flattened, and the glass slide was embedded in the center of the instrument experimental slot for testing; the identification of the physical phase and the crystal structure information were analyzed by JADE 6.0 software.

[0049] Example 1

[0050] Preparation of pre-lithiation reagent: Prepare 1M biphenyl-lithium-tetrahydrofuran solution. First, weigh 0.77g of biphenyl and dissolve it in 5ml of tetrahydrofuran solution. Then dissolve 0.035g of lithium flakes in the mixed solution of biphenyl and tetrahydrofuran until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0051] In a glove box, the prepared zinc metastannate material (denoted as A0) was placed in a 1M pre-lithiation reagent for reaction for 20 minutes. The pre-lithiation reagent consisted of a solvent tetrahydrofuran, a solute lithium sheet, and a mixture of biphenyl. After the reaction, vacuum drying was used to collect the pre-lithiation zinc metastannate negative electrode material (denoted as A1).

[0052] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A1), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material, and dried and cut to obtain a zinc metastannate negative electrode sheet.

[0053] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), a glass fiber membrane (GE Whatman) as a separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte were assembled into CR2032 button cells in an argon glove box.

[0054] Electrochemical performance test:

[0055] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 .

[0056] The results are shown in Table 1:

[0057] Table 1. Comparison of battery performance between A0 and A1

[0058]

[0059] As can be seen from Table 1, the first cycle coulombic efficiency after pre-lithiation with biphenyl-lithium-tetrahydrofuran solution increased by 38.95%, and the capacity retention rate after 100 cycles also increased from 19.93% to 71.52%. Figure 3 and Figure 4 It can be seen that the original sample no longer provides capacity above 1.5V, resulting in a very low first-cycle efficiency, while the charge and discharge curve after pre-lithiation has a better platform, with an initial efficiency of up to 94.38%. Figure 5 This is an XPS comparison chart of the untreated zinc metastannate material and the zinc metastannate material treated with a biphenyl-lithium-tetrahydrofuran pre-lithiation solution for 20 minutes. It can be seen that no peak of lithium element is detected in the untreated zinc metastannate material, while a peak of lithium element is clearly detected after the treatment in the embodiment, which can infer the successful embedding of lithium ions.

[0060] Example 2

[0061] Preparation of pre-lithiation reagent: Prepare 1M biphenyl-lithium-ethylene glycol dimethyl ether solution. First, weigh 0.77g of biphenyl and dissolve it in 5ml of ethylene glycol dimethyl ether solution. Then dissolve 0.035g of lithium flakes in the mixed solution of biphenyl and ethylene glycol dimethyl ether until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0062] In a glove box, the prepared zinc metastannate material (denoted as A0) was placed in a 1M pre-lithiation reagent for reaction for 20 minutes. The pre-lithiation reagent consisted of a solvent of ethylene glycol dimethyl ether, a solute of lithium sheets, and a mixture of biphenyl. After the reaction, vacuum drying was used to collect the pre-lithiation zinc metastannate negative electrode material (denoted as A2).

[0063] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A2), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material, and dried and cut to obtain a zinc metastannate negative electrode sheet.

[0064] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), a glass fiber membrane (GE Whatman) as a separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte were assembled into CR2032 button cells in an argon glove box.

[0065] Electrochemical performance test:

[0066] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 .

[0067] The results are shown in Table 2:

[0068] Table 2. Comparison of battery performance between A0 and A2.

[0069]

[0070] As can be seen from Table 2, the coulombic efficiency of the first cycle after pre-lithiation using biphenyl-lithium-ethylene glycol dimethyl ether solution is increased by 29.8%, proving that the SEI film produced by pre-lithiation on the surface of the electrode reduces irreversible reactions; the capacity retention rate after 100 cycles is also increased from 19.93% to 60.65%, proving that the embedding of lithium ions improves the stability of the battery, but the modification effect is weaker than that in Example 1.

[0071] Example 3

[0072] Preparation of pre-lithiation reagent: Prepare 1M naphthalene-lithium-tetrahydrofuran solution. First, weigh 0.64 g of naphthalene and dissolve it in 5 ml of tetrahydrofuran solution. Then dissolve 0.035 g of lithium flakes in the mixed solution of naphthalene and tetrahydrofuran until the solution turns dark blue. Let it stand for 12 hours to obtain the desired solution.

[0073] In a glove box, the prepared zinc metastannate material (denoted as A0) was placed in a pre-lithiation reagent for reaction for 5 minutes. The pre-lithiation reagent consisted of a solvent tetrahydrofuran, a solute lithium sheet, and a mixture of naphthalene. After the reaction, a vacuum drying method was used to collect the pre-lithiation zinc metastannate negative electrode material (denoted as A3).

[0074] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A3), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material, and dried and cut to obtain a zinc metastannate negative electrode sheet.

[0075] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), a glass fiber membrane (GE Whatman) as a separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte were assembled into CR2032 button cells in an argon glove box.

[0076] Electrochemical performance test:

[0077] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 .

[0078] The results are shown in Table 3:

[0079] Table 3. Comparison of battery performance between A0 and A3

[0080]

[0081] As can be seen from Table 3, the coulombic efficiency of the first cycle after pre-lithiation with naphthalene-lithium-tetrahydrofuran solution is increased by 27.62%, proving that the SEI film produced by pre-lithiation on the surface of the electrode reduces the irreversible reaction; the capacity retention rate after 100 cycles is also increased from 19.93% to 61.38%, proving that the embedding of lithium ions improves the battery stability, but the modification effect is weaker than that in Example 1.

[0082] Example 4

[0083] Preparation of pre-lithiation reagent: Prepare 1M naphthalene-lithium-ethylene glycol dimethyl ether solution. First, weigh 0.64 g of naphthalene and dissolve it in 5 ml of ethylene glycol dimethyl ether solution. Then dissolve 0.035 g of lithium flakes in the mixed solution of naphthalene and ethylene glycol dimethyl ether until the solution turns dark blue. Let it stand for 12 hours to obtain the desired solution.

[0084] In a glove box, the prepared zinc metastannate material (denoted as A0) is placed in a pre-lithiation reagent for reaction for 60 minutes. The pre-lithiation reagent is composed of a solvent of ethylene glycol dimethyl ether and a mixture of solute lithium sheets and naphthalene. After the reaction is completed, the pre-lithiation zinc metastannate negative electrode material (denoted as A4) can be obtained by vacuum drying and collection.

[0085] Preparation of pole pieces: The pre-lithiation treated zinc metastannate negative electrode material (A4), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material, and after drying and cutting, a zinc metastannate negative electrode piece is obtained.

[0086] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), with metallic lithium as the negative electrode, glass fiber membrane (GE Whatman) as the separator, 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC = 1:1, vol%) as the electrolyte, was assembled into a CR2032 button cell in an argon glove box. Electrochemical performance test:

[0087] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 .

[0088] The results are shown in Table 4:

[0089] Table 4. Comparison of battery performance between A0 and A4

[0090]

[0091] It can be seen from Table 4 that the first cycle coulombic efficiency after pre-lithiation with naphthalene-lithium-ethylene glycol dimethyl ether solution is increased by 19.21%, proving that the SEI film produced by pre-lithiation on the electrode surface reduces irreversible reactions; the capacity retention rate after 100 cycles is also increased from 19.93% to 59.12%, proving that the embedding of lithium ions improves the battery stability, but the modification effect is weaker than that in Example 1.

[0092] In order to explore the effect of the ratio of the pre-lithiation reagent on the electrochemical properties of the zinc metastannate negative electrode material, the following experiment will be continued by changing the ratio of the pre-lithiation reagent in Example 1 (biphenyl / lithium sheet / tetrahydrofuran) and the pre-lithiation reagent in Example 2 (biphenyl / lithium sheet / ethylene glycol dimethyl ether).

[0093] Example 5

[0094] Preparation of pre-lithiation reagent: Prepare 1.5M biphenyl-lithium-tetrahydrofuran solution. First, weigh 1.16g of biphenyl and dissolve it in 5ml of tetrahydrofuran solution. Then dissolve 0.052g of lithium flakes in the mixed solution of biphenyl and tetrahydrofuran until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0095] In a glove box, the prepared zinc metastannate material (denoted as A0) was placed in a pre-lithiation reagent for reaction for 20 minutes. The pre-lithiation reagent consisted of a solvent tetrahydrofuran, a solute lithium sheet, and a mixture of biphenyl. After the reaction, the pre-lithiation zinc metastannate electrode (denoted as A5) was obtained by vacuum drying and collection.

[0096] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A5), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material, and dried and cut to obtain a zinc metastannate negative electrode sheet.

[0097] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), with metallic lithium as the negative electrode, glass fiber membrane (GE Whatman) as the separator, 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC = 1:1, vol%) as the electrolyte, was assembled into a CR2032 button cell in an argon glove box. Electrochemical performance test:

[0098] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 The results are shown in Table 5:

[0099] Table 5. Comparison of battery performance between A0 and A5

[0100]

[0101] It can be seen from Table 5 that the coulombic efficiency of the first cycle after pre-lithiation with biphenyl-lithium-tetrahydrofuran solution is increased by 35.24%, proving that the SEI film produced by pre-lithiation on the surface of the electrode reduces the irreversible reaction; the capacity retention rate after 100 cycles is also increased from 19.93% to 70.03%, proving that the embedding of lithium ions improves the battery stability, but the modification effect is weaker than that in Example 1.

[0102] Example 6

[0103] Preparation of pre-lithiation reagent: Prepare 0.5M biphenyl-lithium-tetrahydrofuran solution. First, weigh 0.39g of biphenyl and dissolve it in 5ml of tetrahydrofuran solution. Then dissolve 0.017g of lithium flakes in the mixed solution of biphenyl and tetrahydrofuran until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0104] In a glove box, the prepared zinc metastannate material (denoted as A0) was placed in a pre-lithiation reagent for reaction for 20 minutes. The pre-lithiation reagent consisted of a solvent tetrahydrofuran, a solute lithium sheet, and a mixture of biphenyl. After the reaction, the pre-lithiation zinc metastannate negative electrode material (denoted as A6) was obtained by vacuum drying and collection.

[0105] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A6), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material. After drying and cutting, the zinc metastannate negative electrode sheet is obtained.

[0106] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), with metallic lithium as the negative electrode, glass fiber membrane (GE Whatman) as the separator, 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC = 1:1, vol%) as the electrolyte, was assembled into a CR2032 button cell in an argon glove box. Electrochemical performance test:

[0107] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 The results are shown in Table 6:

[0108] Table 6. Comparison of battery performance between A0 and A6

[0109]

[0110] It can be seen from Table 6 that the coulombic efficiency of the first cycle after pre-lithiation with biphenyl-lithium-tetrahydrofuran solution is increased by 32.37%, proving that the SEI film produced by pre-lithiation on the surface of the electrode reduces the irreversible reaction; the capacity retention rate after 100 cycles is also increased from 19.93% to 66.5%, proving that the embedding of lithium ions improves the battery stability, but the modification effect is weaker than that in Example 1.

[0111] Example 7

[0112] Preparation of pre-lithiation reagent: Prepare 1.5M biphenyl-lithium-ethylene glycol dimethyl ether solution. First, weigh 1.16g of biphenyl and dissolve it in 5ml of ethylene glycol dimethyl ether solution. Then dissolve 0.052g of lithium flakes in the mixed solution of biphenyl and ethylene glycol dimethyl ether until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0113] In a glove box, the prepared zinc metastannate material (denoted as A0) was placed in a pre-lithiation reagent for reaction for 20 minutes. The pre-lithiation reagent consisted of a solvent of ethylene glycol dimethyl ether, a solute of lithium sheets, and a mixture of biphenyl. After the reaction, the pre-lithiation zinc metastannate negative electrode material (denoted as A7) was obtained by vacuum drying and collection.

[0114] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A7), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material, and dried and cut to obtain a zinc metastannate negative electrode sheet.

[0115] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), with metallic lithium as the negative electrode, glass fiber membrane (GE Whatman) as the separator, 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC = 1:1, vol%) as the electrolyte, was assembled into a CR2032 button cell in an argon glove box. Electrochemical performance test:

[0116] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 The results are shown in Table 7:

[0117] Table 7. Comparison of battery performance between A0 and A7

[0118]

[0119] It can be seen from Table 7 that the coulombic efficiency of the first cycle after pre-lithiation with biphenyl-lithium-tetrahydrofuran solution is increased by 24.16%, proving that the SEI film produced by pre-lithiation on the surface of zinc metastannate material reduces irreversible reactions; the capacity retention rate after 100 cycles is also increased from 19.93% to 58.59%, proving that the embedding of lithium ions improves the stability of the battery, but the modification effect is weaker than that of Example 2 and Example 1.

[0120] Example 8

[0121] Preparation of pre-lithiation reagent: Prepare 0.5M biphenyl-lithium-ethylene glycol dimethyl ether solution. First, weigh 0.39g of biphenyl and dissolve it in 5ml of ethylene glycol dimethyl ether solution. Then dissolve 0.017g of lithium flakes in the mixed solution of biphenyl and ethylene glycol dimethyl ether until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0122] In a glove box, the prepared zinc metastannate material (denoted as A0) is placed in a pre-lithiation reagent for reaction for 20 minutes. The pre-lithiation reagent is composed of a solvent of ethylene glycol dimethyl ether, a solute of lithium sheets, and a mixture of biphenyl. After the reaction is completed, the pre-lithiation zinc metastannate negative electrode material (denoted as A8) can be obtained by vacuum drying and collection.

[0123] Pole sheet preparation: The pre-lithiation treated zinc metastannate negative electrode material (A8), binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material. After drying and cutting, the zinc metastannate negative electrode sheet is obtained.

[0124] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), with metallic lithium as the negative electrode, glass fiber membrane (GE Whatman) as the separator, 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC = 1:1, vol%) as the electrolyte, was assembled into a CR2032 button cell in an argon glove box. Electrochemical performance test:

[0125] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 The results are shown in Table 8:

[0126] Table 8. Comparison of battery performance between A0 and A8

[0127]

[0128] It can be seen from Table 8 that the first cycle coulombic efficiency after pre-lithiation using 0.5M biphenyl-lithium-ethylene glycol dimethyl ether solution is increased by 5.3%, proving that the SEI film produced by pre-lithiation on the surface of zinc stannate material reduces irreversible reactions; the capacity retention rate after 100 cycles is also increased from 19.93% to 39.22%, proving that the embedding of lithium ions improves the battery stability, but the modification effect is weaker than that of Example 2 and Example 1.

[0129] Depend on Figure 5It can be seen that, based on the above embodiments, different pre-lithiation agents all have a modification effect on the zinc metastannate negative electrode material, among which the pre-lithiation agent of lithium-biphenyl-tetrahydrofuran with a 1M ratio has the best effect.

[0130] In order to further study the pre-lithiation effect of chemical pre-lithiation reagents on zinc metastannate materials, different concentrations of pre-lithiation reagents were used in gaseous form to form pre-lithiation steam, and then the original zinc metastannate material negative electrode was placed in the steam, so that the pre-lithiation steam diffused to the negative electrode to obtain steam pre-lithiation zinc metastannate electrode

[0131] Example 9

[0132] Preparation of pre-lithiation reagent: Prepare 1M biphenyl-lithium-tetrahydrofuran solution. First, weigh 0.77g of biphenyl and dissolve it in 5ml of tetrahydrofuran solution. Then dissolve 0.035g of lithium flakes in the mixed solution of biphenyl and tetrahydrofuran until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0133] Preparation of pole pieces: The untreated zinc metastannate negative electrode material, binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material. After drying and cutting, the zinc metastannate negative electrode piece is obtained.

[0134] The nitrogen is heated to 80°C and passed into the acetonitrile tank, and the nitrogen and acetonitrile mixed gas is introduced into the steam chamber through the air inlet, and the gas flow rate is controlled to be 80 mL / min. The gas is recycled through the air outlet. The prepared zinc metastannate negative electrode sheet (denoted as A0) is placed in a pre-lithiation reagent steam filled with 1M for 20 minutes. The pre-lithiation reagent is composed of a solvent tetrahydrofuran, a solute lithium sheet, and a biphenyl mixture. After the reaction is completed, it is naturally dried to obtain a steam pre-lithiation zinc metastannate negative electrode material (denoted as A9).

[0135] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), a glass fiber membrane (GE Whatman) as a separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte were assembled into CR2032 button cells in an argon glove box.

[0136] Electrochemical performance test:

[0137] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm-2 The results are shown in Table 9:

[0138] Table 9. Comparison of battery performance between A0 and A9

[0139]

[0140] As can be seen from Table 9, the coulombic efficiency of the first cycle after pre-lithiation with 1M biphenyl-lithium-tetrahydrofuran solution steam increased by 36.92%, proving that the SEI film produced by pre-lithiation on the surface of zinc metastannate material reduced the irreversible reaction; the capacity retention rate after 100 cycles also increased from 19.93% to 70.51%, proving that the embedding of lithium ions improved the battery stability. Figure 7 and Figure 8 The electron microscope cross-sectional images of the zinc metastannate electrode before and after steam pre-lithiation are shown in Figure 1. By comparison, it can be seen that the electrode load after steam pre-lithiation has a significantly increased thickness, which can once again verify that the embedding of lithium ions causes the load to expand. However, its modification effect is weaker than that of Example 1.

[0141] Example 10

[0142] Preparation of pre-lithiation reagent: Prepare 1.5M biphenyl-lithium-ethylene glycol dimethyl ether solution. First, weigh 1.16g of biphenyl and dissolve it in 5ml of ethylene glycol dimethyl ether solution. Then dissolve 0.052g of lithium flakes in the mixed solution of biphenyl and ethylene glycol dimethyl ether until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0143] Preparation of pole pieces: The untreated zinc metastannate negative electrode material, binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material. After drying and cutting, the zinc metastannate negative electrode piece is obtained.

[0144] The nitrogen is heated to 80°C and passed into the acetonitrile tank, and the nitrogen and acetonitrile mixed gas is introduced into the steam chamber through the air inlet, and the gas flow rate is controlled to be 80 mL / min. The gas is recycled through the air outlet. The prepared zinc metastannate negative electrode sheet (denoted as A0) is placed in a pre-lithiation reagent steam filled with 1.5M for 20 minutes. The pre-lithiation reagent is composed of a solvent tetrahydrofuran, a solute lithium sheet, and a biphenyl mixture. After the reaction is completed, it is naturally dried to obtain a steam pre-lithiation zinc metastannate negative electrode material (denoted as A10).

[0145] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), a glass fiber membrane (GE Whatman) as a separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte were assembled into CR2032 button cells in an argon glove box.

[0146] Electrochemical performance test:

[0147] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 The results are shown in Table 10:

[0148] Table 10. Comparison of battery performance between A0 and A10

[0149]

[0150] It can be seen from Table 10 that the first cycle coulombic efficiency after pre-lithiation using 1.5M biphenyl-lithium-tetrahydrofuran solution steam is increased by 32.48%, proving that the SEI film produced by pre-lithiation on the surface of zinc metastannate material reduces irreversible reactions; the capacity retention rate after 100 cycles is also increased from 19.93% to 49.23%, proving that the embedding of lithium ions improves the battery stability, but the modification effect is weaker than that of Example 1 and Example 9.

[0151] Embodiment 11

[0152] Preparation of pre-lithiation reagent: Prepare 0.5M biphenyl-lithium-ethylene glycol dimethyl ether solution. First, weigh 0.39g of biphenyl and dissolve it in 5ml of ethylene glycol dimethyl ether solution. Then dissolve 0.017g of lithium flakes in the mixed solution of biphenyl and ethylene glycol dimethyl ether until the solution turns dark blue. Let it stand for 12h to obtain the desired solution.

[0153] Preparation of pole pieces: The untreated zinc metastannate negative electrode material, binder and conductive carbon are fully mixed in a ratio of 7:2:1, and then coated on a copper foil material. After drying and cutting, the zinc metastannate negative electrode piece is obtained.

[0154] The nitrogen is heated to 80°C and passed into the acetonitrile tank, and the nitrogen and acetonitrile mixed gas is introduced into the steam chamber through the air inlet, and the gas flow rate is controlled to be 80 mL / min. The gas is recycled through the air outlet. The prepared zinc metastannate negative electrode sheet (denoted as A0) is placed in a pre-lithiation reagent steam filled with 0.5M for 20 minutes. The pre-lithiation reagent is composed of a solvent tetrahydrofuran, a solute lithium sheet, and a biphenyl mixture. After the reaction is completed, it is naturally dried to obtain a steam pre-lithiation zinc metastannate negative electrode material (denoted as A11).

[0155] Battery assembly: LiPF6 added to ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (volume ratio of 1:1), a glass fiber membrane (GE Whatman) as a separator, and 1.0 mol / L LiPF6 / ethylene carbonate (EC) + diethyl carbonate (DEC) solution (EC:DEC=1:1, vol%) as the electrolyte were assembled into CR2032 button cells in an argon glove box.

[0156] Electrochemical performance test:

[0157] The electrochemical performance of the battery was tested on the LAND battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage range was 0.01V~3V, and the current density was 1C (866.6mA g -1 ) The loading density of the anode film is about 1.5 mg cm -2 The results are shown in Table 11:

[0158] Table 11. Comparison of battery performance between A0 and A11

[0159]

[0160]

[0161] It can be seen from Table 11 that the coulombic efficiency of the first cycle after pre-lithiation with 0.5M biphenyl-lithium-tetrahydrofuran solution steam is only increased by 4.31%, proving that the SEI film produced by pre-lithiation on the surface of zinc metastannate material reduces irreversible reactions, but the effect is poor due to the low concentration; the capacity retention rate after 100 cycles is also increased from 19.93% to 50.64%, proving that the embedding of lithium ions improves the stability of the battery, but the modification effect is weaker than that of Example 1 and Example 9.

[0162] Based on the analysis of all the above examples, it can be concluded that the best reagent formula for pre-lithiation effect is biphenyl-lithium-tetrahydrofuran solution, and the optimal concentration is 1 M, and the optimal reaction time is 20 minutes. After analysis, it is believed that too high a concentration or too long a time will lead to excessive reaction and reach saturation, while too low a concentration or too short a time will lead to insufficient reaction and failure to supplement enough lithium ions to make up for the lithium deficiency.

[0163] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.

[0164] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a zinc metastannate negative electrode material, characterized in that: The following steps are involved: S1. Dissolve appropriate amounts of sodium stannate, zinc acetate and urea in a mixed solution of ethanol and deionized water, mix evenly, and then perform hydrothermal treatment, centrifugal drying and calcination to obtain zinc metastannate powder; S2, dissolving a lithiation reagent and metallic lithium in a tetrahydrofuran solvent to obtain a chemical pre-lithiation reagent solution, wherein the pre-lithiation reagent solution comprises at least biphenyl, lithium, and tetrahydrofuran; S3, placing the prepared zinc metastannate powder in a chemical pre-lithiation reagent solution for reaction or placing it in a chemical pre-lithiation reagent vapor for reaction, and collecting it after vacuum drying to obtain a chemical pre-lithiation zinc metastannate negative electrode material.

2. The preparation method according to claim 1, characterized in that In step S1, tin and zinc are added in a molar ratio of 1:1, and the volume ratio of ethanol and deionized water is 1:(1-3); the mixing method is any one of stirring and ultrasound, and the mixing time is 0.1-3h; the hydrothermal temperature is 150-180°C, and the time is 4-6h; the centrifugal speed is 7200-7800r / min, and the time is 3-5min. The drying treatment is any one of normal pressure drying, reduced pressure drying, spray drying, microwave drying, and infrared drying, and the drying temperature is 40-120°C. The calcination conditions are a temperature of 450-650°C, a heating rate of 2-10°C / min, a calcination time of 2-6h, and a calcination atmosphere of dry air, nitrogen, and argon. Then, the product is naturally cooled to room temperature to obtain the product.

3. The preparation method according to claim 1, characterized in that: In step S2, the chemical pre-lithiation solvent includes at least one or more of tetrahydrofuran, ethylene glycol dimethyl ether, methyl propyl ether, methyl butyl ether, methyl amyl ether, ethyl propyl ether, ethyl butyl ether, ethyl amyl ether, propyl butyl ether, propyl amyl ether, methyltetrahydrofuran, dimethyltetrahydrofuran, ethyltetrahydrofuran, diethyltetrahydrofuran, phenyltetrahydrofuran, 1,2-dimethoxyethane and diethylene glycol dimethyl ether.

4. The preparation method according to claim 3, characterized in that: In step S2, the lithiation reagent includes at least one or more of biphenyl, naphthalene, methylnaphthalene, dimethylnaphthalene, tetramethylnaphthalene, anthracene, methylanthracene, dimethylanthracene, tetramethylanthracene, phenanthrene, methylphenanthrene, dimethylphenanthrene, trimethylphenanthrene, tetramethylphenanthrene, pyrene, methylpyrene, dimethylpyrene, trimethylpyrene, tetramethylpyrene, methylpyrene, dimethylpyrene, trimethylpyrene, tetramethylpyrene, methylbiphenyl, dimethylbiphenyl and tetramethylbiphenyl; in step S2, the metallic lithium includes at least one or more of lithium sheets and lithium strips.

5. The preparation method according to claim 1, characterized in that: In step S3, the reaction time in the chemical pre-lithiation reagent solution is 5 to 60 minutes.

6. A zinc metastannate negative electrode material prepared by the preparation method according to any one of claims 1 to 5.

7. A zinc metastannate negative electrode sheet, characterized in that: The zinc metastannate material, binder and conductive carbon described in claim 6 are fully mixed in a certain proportion, then coated on a copper foil material, and dried and cut to obtain the product.

8. The zinc metastannate negative electrode sheet according to claim 7, characterized in that: The zinc metastannate negative electrode plate includes at least the following components: 50-99wt% zinc metastannate negative electrode material, 0.5-40wt% conductive agent, and 0.5-10wt% binder; the conductive agent includes at least one or more of acetylene black, Ketjen black, Super P, MCMB, and carbon nanotubes; the binder includes at least one or more of polyvinylidene fluoride, polyvinyl chloride, polyvinyl butyral, polyacrylonitrile, polyacrylic acid, polyethylene glycol, polypyrrole, polyaniline, sucrose, glucose, maltose, citric acid, asphalt, furfural resin, epoxy resin, phenolic resin, sodium alginate, and carboxymethyl cellulose.

9. An electrode, characterized in that: It comprises the zinc metastannate negative electrode sheet as described in claim 7 or 8.

10. A lithium ion secondary battery, characterized in that: Comprising the electrode as claimed in claim 9.

Citation Information

Patent Citations

  • Ternary metal oxide based on zinc ion doping, and preparation method and application thereof

    CN109390564A

  • Chemical pre-lithiation method for preparing organic negative electrode material with high initial coulombic efficiency

    CN117393705A

  • High-performance anode material for lithium secondary battery having oxide protective layer

    KR1020140137792A

  • Rotary Honey Extractor for Improvement Honey Comb of Natura Bee

    KR102376549B1

  • Prelithiated and methods for prelithiating an energy storage device

    US20190181440A1

Cited By

  • Lithium supplement reagent for negative electrode of lithium ion battery and application of lithium supplement reagent

    CN119812525A