Silicon inclusion compound electrode active material, negative electrode mixture, negative electrode active material layer, and solid lithium ion battery

By controlling the content and structure of oxygen atoms in the silicon inclusion electrode active substance, combined with oxidation treatment, a silicon inclusion electrode active substance with an appropriate amount of oxygen atoms was prepared, which was used in solid lithium-ion batteries, solving the problem of expansion during charging and realizing the More even charging reaction and reduced expansion.

CN118943314APending Publication Date: 2024-11-12TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410552989.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-05-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing silicon inclusion electrode active material has an expansion problem when charging, and the prior art is difficult to further suppress this expansion.

Method used

By controlling the content of oxygen atoms in the silicon inclusion electrode active material, ensuring that it is between 0-19.4 mass%, and partially having a type II inclusion structure, combining oxidation treatment and oxygen removal treatment, an appropriate amount of oxygen is prepared to be prepared. The silicon inclusion electrode active material of atoms is used to prepare a negative electrode mixture and an anode active material layer, and is used in solid lithium-ion batteries.

Benefits of technology

It effectively suppresses the expansion of the silicon inclusion electrode active material during charging, improves ion conductivity, ensures uniformity of the charging reaction, and thus reduces the expansion during charging of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943314A_ABST
    Figure CN118943314A_ABST
Patent Text Reader

Abstract

The present disclosure provides a silicon clathrate electrode active material having small expansion during charging, and a solid lithium ion battery having such a silicon clathrate electrode active material. The silicon inclusion compound electrode active material of the present disclosure contains more than 0% by mass and less than 19.4% by mass of oxygen atoms. The solid lithium ion battery of the present disclosure has the negative electrode active material layer of the present disclosure. The negative electrode active material layer of the present disclosure contains the negative electrode mixture of the present disclosure. The negative electrode mixture according to the present disclosure contains the silicon inclusion compound electrode active material according to the present disclosure and a solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a silicon clathrate electrode active material, a negative electrode binder, a negative electrode active material layer, and a solid-state lithium ion battery. Background Art

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automotive industry, the development of batteries for electric vehicles or hybrid vehicles is being promoted. In addition, silicon is known as an electrode active material used in batteries, particularly lithium ion batteries.

[0003] The theoretical capacity of a silicon electrode active material is large, which is effective for increasing the energy density of a battery. On the other hand, however, the silicon electrode active material has a problem of large expansion during charging. In response to this, it is known to suppress the expansion during charging by using a silicon clathrate electrode active material as the silicon electrode active material.

[0004] For example, Patent Document 1 discloses a silicon clathrate electrode active material having a crystal phase of type II silicon clathrate and having a composition of Na x Si 136 (1.98 < x < 2.54). Patent Document 2 discloses a silicon clathrate electrode active material having a crystal phase of type II silicon clathrate, having voids inside primary particles, and having a void volume of voids with a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less.

[0005] Prior Art Documents

[0006] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2021-158003

[0007] Patent Document 2: Japanese Unexamined Patent Application Publication No. 2021-158004 Summary of the Invention

[0008] Although the silicon clathrate electrode active material can suppress the expansion during charging as compared with a normal silicon electrode active material, further suppression of the expansion of the silicon clathrate electrode active material during charging is required.

[0009] An object of the present disclosure is to provide a silicon clathrate electrode active material with small expansion during charging, and a solid-state lithium ion battery having such a silicon clathrate electrode active material.

[0010] The present inventors have found that the above problems can be solved by the following means.

[0011] <Mode 1>

[0012] A silicon clathrate electrode active material containing more than 0% by mass and less than 19.4% by mass of oxygen atoms.

[0013] <Method 2>

[0014] The silicon clathrate electrode active material according to Embodiment 1 contains 2.0 mass % or more of oxygen atoms.

[0015] <Method 3>

[0016] The silicon clathrate electrode active material according to Embodiment 2 contains 3.3 mass % or more and 7.0 mass % or less of oxygen atoms.

[0017] <Method 4>

[0018] The silicon inclusion compound electrode active material according to Embodiment 1 at least partially has a type II inclusion compound structure.

[0019] <Method 5>

[0020] A negative electrode mixture comprises the silicon inclusion compound electrode active material described in method 1 and a solid electrolyte.

[0021] <Method 6>

[0022] In the negative electrode mixture according to aspect 5, the solid electrolyte is a sulfide solid electrolyte.

[0023] <Method 7>

[0024] A negative electrode active material layer contains the negative electrode mixture described in embodiment 5.

[0025] <Method 8>

[0026] A solid lithium ion battery having the negative electrode active material layer described in method 7.

[0027] According to the present disclosure, it is possible to provide a silicon clathrate electrode active material that has little expansion during charge, and a solid lithium ion battery having the silicon clathrate electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a graph showing the relationship between the oxygen atomic weight and the expansion amount of the silicon clathrate electrode active materials of Examples 1 to 5 and Comparative Example 1. DETAILED DESCRIPTION

[0029] Hereinafter, the embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and can be implemented with various modifications within the scope of the disclosed gist.

[0030] 《Silicon inclusion compound electrode active material》

[0031] The silicon clathrate electrode active material disclosed herein contains more than 0 mass % and less than 19.4 mass % of oxygen atoms.

[0032] The present inventors have unexpectedly found that a silicon clathrate electrode active material containing a predetermined amount of oxygen atoms expands less during charge.

[0033] As the reason, it is not intended to be bound by any theory, but it is speculated as follows. That is, it is believed that although the lithium ion conductivity of the silicon inclusion compound electrode active material is low, if there is an appropriate amount of oxygen atoms in the silicon inclusion compound electrode active material, silicon oxide reacts with lithium to form an ion conductor such as lithium silicate, and the ion conductivity of the silicon inclusion compound electrode active material increases, thereby the charging reaction proceeds uniformly, and the expansion during charging is suppressed. In addition, it is believed that by not having excessive oxygen atoms in the silicon inclusion compound electrode active material, the conductivity is not hindered, the charging reaction proceeds uniformly, and the expansion during charging is suppressed.

[0034] Furthermore, in the present disclosure, the “electrode active material” can be used as both a “positive electrode active material” and a “negative electrode active material”, and in particular, can be used as a “negative electrode active material”.

[0035] The silicon clathrate electrode active material disclosed herein contains more than 0 mass % and less than 19.4 mass % of oxygen atoms. If the amount of oxygen atoms is within the above range, expansion during charging is sufficiently suppressed, which is preferred.

[0036] The silicon inclusion compound electrode active material may also contain more than 1.0 mass %, more than 2.0 mass %, more than 2.5 mass %, more than 2.7 mass %, more than 2.9 mass %, more than 3.0 mass %, more than 3.1 mass %, more than 3.2 mass % or more than 3.3 mass % of oxygen atoms, and may also contain less than 15.0 mass %, less than 10.0 mass %, less than 9.0 mass %, less than 8.0 mass % or less than 7.0 mass % of oxygen atoms. That is, the silicon inclusion compound electrode active material particularly preferably contains more than 3.3 mass % and less than 7.0 mass % of oxygen atoms. If the amount of oxygen atoms is within the above range, the expansion during charging can be further reduced.

[0037] The method for measuring the oxygen atomic weight is not particularly limited, and examples thereof include elemental analysis using an oxygen-nitrogen-hydrogen analyzer or a method for calculating the analytical value of EDX, XPS, etc. Specifically, in order to perform the measurement, EMGA-930 from Horiba, Ltd. can be used as an oxygen-nitrogen-hydrogen analyzer.

[0038] The silicon inclusion compound electrode active material disclosed herein may at least partially have a type II inclusion compound structure. In this case, expansion during charging can be further reduced.

[0039] In order to adjust the ratio of oxygen atoms in the silicon clathrate electrode active material, the silicon clathrate electrode active material may be subjected to oxidation treatment and oxygen removal treatment.

[0040] As a specific oxidation treatment, the silicon clathrate-type electrode active material may be placed in an oxidizing atmosphere and optionally heated.

[0041] In addition, as oxygen removal treatment, reduction treatment and silicon oxide removal treatment can be cited. Silicon oxide removal treatment can be carried out by immersing the silicon inclusion compound electrode active material in a solution capable of dissolving and removing silicon oxide, such as an aqueous solution of hydrogen fluoride. In addition, in the case where the silicon inclusion compound electrode active material has lithium silicate (Li2SiO3), using an aqueous solution of hydrogen chloride (hydrochloric acid) to convert lithium silicate into soluble silicic acid (H2SiO3), and removing the silicic acid can also reduce oxygen atoms in the silicon inclusion compound electrode active material (Li2SiO3+2HCl→2LiCl(dissolved)+H2SiO3(dissolved)).

[0042] Furthermore, by performing an oxidation treatment in advance before the silicon oxide removal treatment using a solution capable of dissolving and removing silicon oxide, oxygen removal in the subsequent oxygen removal treatment can be promoted.

[0043] Negative Electrode Mixture

[0044] The negative electrode mixture disclosed in the present invention contains a silicon inclusion compound electrode active material and a solid electrolyte. In addition, the negative electrode mixture disclosed in the present invention optionally contains a conductive auxiliary agent and a binder.

[0045] Furthermore, in the present disclosure, "negative electrode mixture" refers to a composition that can form a negative electrode active material layer directly or by further containing other components. In addition, in the present disclosure, "negative electrode mixture slurry" refers to a slurry that contains a dispersion medium in addition to the "negative electrode mixture" and can form a negative electrode active material layer by coating and drying.

[0046] <Silicon inclusion compound electrode active material>

[0047] Regarding the silicon inclusion compound electrode active material, reference can be made to the above description regarding the silicon inclusion compound electrode active material in the present disclosure.

[0048] <Solid Electrolyte>

[0049] The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for lithium ion batteries can be used. For example, the solid electrolyte can be a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer electrolyte, and a sulfide solid electrolyte is preferred.

[0050] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5 (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 (Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x PS 6-x Cl x etc.; or combinations thereof, but not limited thereto.

[0051] As an example of oxide solid electrolyte, Li7La3Zr2O 12 , Li 7-x Ln3Z 1-x Nb x O 12 , Li 7- 3x La3Zr2Al x O 12 , Li 3x La 2 / 3-x TiO3、Li 1+x Al x Ti 2-x (PO4)3、Li 1+x Al x Ge 2-x (PO4)3, Li3PO4 or Li 3+x PO 4-x N x (LiPON), etc., but not limited to these.

[0052] The sulfide solid electrolyte and the oxide solid electrolyte may be glass or crystallized glass (glass ceramic).

[0053] Examples of the polymer electrolyte include polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof, but the polymer electrolyte is not limited thereto.

[0054] The mass ratio of the silicon inclusion compound electrode active material to the solid electrolyte in the negative electrode mixture (mass of the silicon inclusion compound electrode active material:mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0055] <Conductive additive>

[0056] The conductive additive is not particularly limited and may be, for example, a carbon material such as VGCF (Vapor Grown Carbon Fiber) or carbon nanofiber, or a metal material, but is not limited thereto.

[0057] <Adhesive>

[0058] The binder is not particularly limited, and may be, for example, polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0059] 《Negative electrode active material layer》

[0060] The negative electrode active material layer of the present disclosure contains the negative electrode mixture of the present disclosure. With regard to the negative electrode mixture, the above description of the negative electrode mixture of the present disclosure can be referred to.

[0061] The thickness of the negative electrode active material layer can be, for example, 0.1 to 1000 μm.

[0062] 《Solid Lithium-ion Battery》

[0063] The solid lithium ion battery of the present disclosure has the negative electrode active material layer of the present disclosure. In addition, the solid lithium ion battery of the present disclosure may also have a negative electrode collector layer, a negative electrode active material layer of the present disclosure, a solid electrolyte layer, a positive electrode active material layer and a positive electrode collector layer in sequence. In addition, the lithium ion battery of the present disclosure may be constrained by constraining members such as end plates from both sides of the stacking direction of the above-mentioned layers.

[0064] Furthermore, in the present disclosure, "solid battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore, a solid battery may also use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. In addition, the solid battery of the present disclosure may also be an all-solid battery, that is, a battery that uses only a solid electrolyte as an electrolyte.

[0065] Since the negative electrode active material layer of the lithium ion battery of the present disclosure contains the silicon clathrate electrode active material of the present disclosure, the expansion accompanying charging is reduced, thereby suppressing the increase in the restraint pressure accompanying charging.

[0066] <Negative Electrode Collector Layer>

[0067] The material used for the negative electrode collector layer is not particularly limited, and any material that can be used as a negative electrode collector for a battery may be appropriately used, such as stainless steel (SUS), aluminum, copper, nickel, iron, titanium or carbon, a resin collector, etc., but is not limited thereto.

[0068] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among them, a foil shape is preferred.

[0069] <Negative Electrode Active Material Layer>

[0070] Regarding the negative electrode active material layer, reference can be made to the above description regarding the negative electrode active material layer in the present disclosure.

[0071] <Solid Electrolyte Layer>

[0072] The solid electrolyte layer contains at least a solid electrolyte. In addition, the solid electrolyte layer may contain a binder and the like as needed in addition to the solid electrolyte. For the solid electrolyte and the binder, reference may be made to the above description of the negative electrode active material layer in the present disclosure.

[0073] Furthermore, the solid electrolyte layer may be impregnated with an electrolyte solution having lithium ion conductivity.

[0074] The electrolyte preferably contains an electrolyte supporting salt and a solvent. As a supporting salt (lithium salt) of an electrolyte with lithium ion conductivity, for example, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3 can be cited. As a solvent used in the electrolyte, for example, cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC) can be cited. The electrolyte preferably contains two or more solvents.

[0075] The thickness of the solid electrolyte layer is, for example, 0.1 to 1000 μm. The thickness of the solid electrolyte layer is preferably 0.1 to 300 μm, and particularly preferably 0.1 to 100 μm.

[0076] <Positive Electrode Active Material Layer>

[0077] The positive electrode active material layer is a layer containing a positive electrode active material and, optionally, a solid electrolyte, a conductive auxiliary agent, a binder, and the like.

[0078] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material can be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo1 / 3 Ni 1 / 3 Mn 1 / 3 O2, by Li 1+x Mn 2-x-y A heterogeneous element-substituted Li-Mn spinel having a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni and Zn) is used, but is not limited to this.

[0079] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, has low reactivity with the positive electrode active material and the solid electrolyte, and does not flow even when in contact with the active material and the solid electrolyte, and can maintain the coating layer morphology. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but not limited to these.

[0080] The shape of the positive electrode active material may be, for example, a granular shape. The average particle size (D50) of the positive electrode active material is not particularly limited, and may be, for example, 10 nm or more, or 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material may be, for example, 50 μm or less, or 20 μm or less. The average particle size (D50) may be calculated, for example, based on the measurement of a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0081] Regarding the solid electrolyte, the conductive auxiliary agent, and the binder, reference can be made to the above description regarding the negative electrode active material layer in the present disclosure.

[0082] Furthermore, when the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material:mass of solid electrolyte) is preferably 85:15 to 30:70, more preferably 80:20 to 40:60.

[0083] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0084] <Positive Electrode Collector Layer>

[0085] The material and shape of the positive electrode current collector layer are not particularly limited, and the above description of the negative electrode active material layer disclosed in the present disclosure can be referred to. Among them, the material of the positive electrode current collector layer is preferably aluminum. In addition, the shape is preferably foil-shaped.

[0086] [Example]

[0087] 《Synthesis of Silicon Inclusion Compound Electrode Active Materials》

[0088] <Alloying>

[0089] (Example 1)

[0090] As a silicon (Si) source, Si powder (High Purity Science, SIEPB32) was prepared. The Si powder and metallic lithium (Li) were weighed at a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar under an argon atmosphere to obtain a lithium silicon alloy. The obtained lithium silicon alloy was reacted with ethanol in an argon atmosphere to obtain a powder having voids inside the primary particles, that is, a Si powder having a porous structure.

[0091] A sodium silicon (NaSi) alloy is manufactured using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. Furthermore, as NaH, NaH pre-washed with hexane is used. NaH and Si powder having a porous structure are weighed so that the molar ratio becomes 1.05:1, and the weighed NaH and Si powder having a porous structure are mixed with a cutting grinder. The obtained mixture is heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0092] <Inclusion>

[0093] The obtained NaSi alloy and aluminum fluoride (AlF3) were weighed so that the molar ratio was 1:0.35, and the weighed NaSi alloy and AlF3 were mixed with a cutting grinder to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction container, and heated in an argon atmosphere at 310°C for 60 hours in a heating furnace to obtain a reaction product containing a silicon inclusion compound. The obtained reaction product was placed in a device capable of reducing pressure and replacing gas, and after reducing pressure in the device at room temperature, it was introduced into the atmosphere for oxidation. The oxidized reaction product was acid-washed using a mixed solvent of HNO3 and H2O mixed in a volume ratio of 10:90 to remove by-products in the reaction product. After washing, the solid component separated by filtration was dried at 120°C for more than 3 hours to obtain a powdered silicon inclusion compound electrode active material. Furthermore, the obtained silicon inclusion compound electrode active material was treated with a 3 wt% HF solution at 25°C for 3 hours, filtered, and dried at 120°C for more than 3 hours, thereby obtaining the silicon inclusion compound electrode active material of Example 1.

[0094] (Example 2)

[0095] The silicon inclusion compound electrode active material of Example 2 was obtained in the same manner as in Example 1 except that oxidation during inclusion compound formation was not performed.

[0096] (Example 3)

[0097] During the clathrate formation, the silicon clathrate electrode active material of Example 3 was obtained in the same manner as in Example 1 except that the atmosphere was introduced for oxidation so that the amount of atmosphere inflow became 1 / 100 of that in Example 1.

[0098] (Example 4)

[0099] The silicon inclusion compound electrode active material of Example 4 was obtained in the same manner as in Example 2 except that the silicon inclusion compound electrode active material was treated with a hydrogen chloride (HCl) solution.

[0100] (Example 5)

[0101] The silicon inclusion compound electrode active material of Example 5 was obtained in the same manner as in Example 2 except that the silicon inclusion compound electrode active material was treated with an HF solution at 0°C.

[0102] (Comparative Example 1)

[0103] The silicon inclusion compound electrode active material of Comparative Example 1 was obtained in the same manner as in Example 2 except that the silicon inclusion compound electrode active material was not treated with the HF solution.

[0104] The silicon clathrate electrode active material of each example has a crystal phase of type II clathrate.

[0105] The production of lithium-ion batteries

[0106] Using the silicon inclusion compound electrode active material of each example, a lithium ion battery of each example was produced as follows.

[0107] <Preparation of Negative Electrode Mixture>

[0108] In a polypropylene container, butyl butyrate, 5% by weight of butyl butyrate of a polyvinylidene fluoride (PVDF)-based binder, vapor-grown carbon fiber (VGCF) as a conductive aid, a synthesized silicon inclusion compound electrode active material, and Li2S-P2S5-based glass ceramics as a sulfide solid electrolyte were added, and stirred for 30 seconds using an ultrasonic dispersion device (UH-50 manufactured by SMT). Then, the container was vibrated for 30 minutes using an oscillator (TTM-1 manufactured by Shibata Science Co., Ltd.) to obtain a slurry-like negative electrode mixture (negative electrode mixture slurry).

[0109] <Formation of Negative Electrode Active Material Layer>

[0110] The obtained negative electrode mixture slurry was applied onto a copper (Cu) foil as a negative electrode current collector layer using an applicator by a doctor blade method, and dried on a hot plate heated to 100° C. for 30 minutes to form a negative electrode active material layer on the negative electrode current collector layer.

[0111] <Formation of Solid Electrolyte Layer>

[0112] Heptane, a 5 wt% heptane solution of a butyl rubber (BR)-based binder, and Li2S-P2S5-based glass ceramics as a sulfide solid electrolyte were added to a polypropylene container and stirred for 30 seconds using an ultrasonic dispersing device (UH-50 manufactured by SMT). Then, the container was vibrated for 30 minutes using an oscillator (TTM-1 manufactured by Shibata Science Co., Ltd.) to obtain a solid electrolyte slurry.

[0113] The obtained solid electrolyte slurry was applied onto an aluminum (Al) foil as a release sheet by a doctor blade method using an applicator, and dried on a hot plate heated to 100° C. for 30 minutes to form a solid electrolyte layer. Three solid electrolyte layers were prepared.

[0114] <Preparation of positive electrode mixture>

[0115] In a polypropylene container, butyl butyrate, a 5 wt % butyl butyrate solution of a PVDF-based binder, and LiNi 2000 with an average particle size of 6 μm as a positive electrode active material were placed. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li2S-P2S5 glass ceramics as a sulfide solid electrolyte, and VGCF as a conductive additive were stirred for 30 seconds using an ultrasonic dispersing device (UH-50 manufactured by SMT).

[0116] Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.), stirred for 30 seconds with an ultrasonic disperser, and shaken for 3 minutes with the shaker to obtain a slurry-like positive electrode mixture (positive electrode mixture slurry).

[0117] <Formation of Positive Electrode Active Material Layer>

[0118] The obtained positive electrode mixture slurry was applied onto an Al foil serving as a positive electrode collector layer using a doctor blade method using an applicator, and dried on a hot plate heated to 100° C. for 30 minutes to form a positive electrode active material layer on the positive electrode collector layer.

[0119] <Battery Assembly>

[0120] The positive electrode current collector layer, the positive electrode active material layer and the first solid electrolyte layer were stacked in this order. The stack was placed on a roll press and pressed at a pressing pressure of 100 kN / cm and a pressing temperature of 165° C. to obtain a positive electrode stack.

[0121] The negative electrode current collector layer, the negative electrode active material layer and the second solid electrolyte layer were stacked in this order. The stack was placed on a roll press and pressed at a pressing pressure of 60 kN / cm and a pressing temperature of 25° C. to obtain a negative electrode stack.

[0122] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode stack and the negative electrode stack. Next, the Al foil as a release sheet was peeled off from the third solid electrolyte layer.

[0123] The positive electrode stack and the negative electrode stack were stacked one on top of the other with the solid electrolyte layer of each facing the third solid electrolyte layer, and the stack was placed on a flat uniaxial press and temporarily pressed at 100 MPa and 25° C. for 10 seconds, and finally, the stack was placed on a flat uniaxial press and pressed at a pressing pressure of 200 MPa and a pressing temperature of 120° C. for 1 minute. Thus, an all-solid battery was obtained.

[0124] "evaluate"

[0125] <Atomic Weight of Oxygen>

[0126] The oxygen atomic weight was calculated from an analysis value obtained by elemental analysis using an oxygen-nitrogen-hydrogen analyzer (EMGA-930, manufactured by Horiba, Ltd.).

[0127] <Expansion>

[0128] The all-solid battery of each example was constrained with a predetermined constraining pressure using a constraining fixture, and the change in the constraining pressure when charged to 4.55V at a constant current-constant voltage at a 10-hour rate (1 / 10C) was measured. The change in the constraining pressure is used as the expansion amount in the present disclosure. Furthermore, the change in the constraining pressure is the difference between the highest and lowest values ​​of the constraining pressure, and the value of the embodiment represents a relative value when the value of Comparative Example 1 is 100.

[0129] "result"

[0130] The oxygen atomic weight in the silicon inclusion compound electrode active material and the expansion amount of the silicon inclusion compound electrode active material in each example are shown in Tables 1 and Figure 1 .

[0131] Table 1

[0132]

[0133] As shown in Table 1 and Figure 1 As shown, the expansion amount of the batteries of Examples 1 to 5 in which the amount of oxygen atoms in the silicon inclusion compound electrode active material is within the range of the present disclosure is smaller than that of the battery of Comparative Example 1.

Claims

1. A silicon inclusion compound electrode active material containing more than 0 mass % and less than 19.4 mass % of oxygen atoms. 2 . The silicon inclusion compound electrode active material according to claim 1 , comprising 2.0 mass % or more of oxygen atoms. 3 . The silicon inclusion compound electrode active material according to claim 2 , comprising 3.3 mass % or more and 7.0 mass % or less of oxygen atoms. The silicon inclusion compound electrode active material according to claim 1 , at least partially having a type II inclusion compound structure.

5. A negative electrode mixture comprising the silicon inclusion compound electrode active material according to claim 1 and a solid electrolyte. The negative electrode mixture according to claim 5 , wherein the solid electrolyte is a sulfide solid electrolyte. 7 . A negative electrode active material layer comprising the negative electrode mixture according to claim 5 . 8 . A solid lithium ion battery comprising the negative electrode active material layer according to claim 7 .