Secondary battery and electric device
By designing the composite electrode structure in the positive electrode sheet of the secondary battery, the single layer is solved by using different particle sizes of iron manganese and lithium nickel cobalt manganese oxides, as well as carbon nanotubes and binders of different particle sizes. The problems of large conductive impedance and poor kinetic performance caused by thick coating improve the energy density and cycling performance of the battery.
Patent Information
- Application Number
- CN202411210704.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
The single-layer thick coating of existing secondary batteries can easily lead to cracking, the internal conductivity impedance of the electrodes is large, and the dynamic performance is insufficient, resulting in the unmet need for energy density improvement.
Design the composite electrode structure, by providing the first and second positive electrode active material layers in the positive electrode sheet, containing lithium manganese iron oxide and lithium nickel cobalt manganese oxide, respectively, and using carbon nanotubes of different particle sizes and binders , the weight ratio and particle size ratio of the material layer are controlled to improve coating quality and electrical conductivity.
It effectively improves the thick coating problem of the positive electrode sheet, reduces the impedance, and improves the dynamic performance and energy density of the secondary battery.
Smart Images

Figure BDA0005020386880000081 
Figure BDA0005020386880000091 
Figure BDA0005020386880000092
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, in particular to a secondary battery and an electrical device. Background Art
[0002] With the rapid development of secondary batteries, the market demand for secondary battery energy density is getting higher and higher, and the demand for thick coating of LFP and LMFP systems is getting higher and higher. However, single-layer thick coating is prone to cracking and difficult to process, and its thickness and pore size are large, the transmission distance of ion conduction and electronic conduction inside the electrode is long, the impedance is large, and the kinetic performance is insufficient. These two factors lead to the demand for energy density improvement far less than expected. Therefore, it is of great significance to improve the cracking problem of thick coating and reduce impedance to improve kinetic performance and energy density through fine design and regulation of composite electrode structure. Summary of the invention
[0003] The purpose of the present application is to provide a secondary battery and an electrical device to improve the electrochemical performance of existing secondary batteries.
[0004] To achieve the above object, in a first aspect of the present application, a secondary battery is provided, the secondary battery comprising a positive electrode sheet, the positive electrode sheet comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, the positive electrode active material layer comprising a first positive electrode active material layer and a second positive electrode active material layer, the first active material layer being disposed between the current collector and the second positive electrode active material layer;
[0005] The positive electrode active material layer comprises manganese iron lithium oxide and lithium nickel cobalt manganese oxide, wherein the average particle size of the lithium nickel cobalt manganese oxide is greater than the average particle size of the manganese iron lithium oxide;
[0006] wherein the weight ratio of the manganese iron lithium oxide to the lithium nickel cobalt manganese oxide present in the first positive electrode active material layer is higher than the weight ratio of the manganese iron lithium oxide to the lithium nickel cobalt manganese oxide present in the second positive electrode active material layer;
[0007] The first positive electrode active material layer includes first carbon nanotubes, and the second positive electrode active material layer includes second carbon nanotubes. The average aspect ratio of the first carbon nanotubes is smaller than the average aspect ratio of the second carbon nanotubes.
[0008] As an embodiment of the present application, the average aspect ratio of the first carbon nanotubes is 50-200.
[0009] As an embodiment of the present application, the average aspect ratio of the second carbon nanotubes is 200-1000.
[0010] As an embodiment of the present application, the first positive electrode active material layer includes a first binder, the second positive electrode active material layer includes a second binder, and the swelling rate of the first binder is smaller than the swelling rate of the second binder.
[0011] As an embodiment of the present application, the first positive electrode active material layer includes a first binder, and the swelling rate of the first binder is 5% to 100%.
[0012] As an embodiment of the present application, the second positive electrode active material layer includes a second binder, and the swelling rate of the second binder is 30% to 500%.
[0013] As an embodiment of the present application, the first binder includes polyvinylidene fluoride.
[0014] As an embodiment of the present application, the second binder includes at least one of polyacrylate, polyhydroxyethyl acrylate, polymethyl acrylate, polymethyl methacrylate, polyvinyl acetate, polyvinyl carbonate, polytert-butyl benzoate, polydiethyl carbonate, and hydrogenated nitrile rubber.
[0015] As an embodiment of the present application, a weight content ratio of lithium iron manganese oxide to lithium nickel cobalt manganese oxide present in the first positive electrode active material layer is A1, satisfying: A1>1.
[0016] As an embodiment of the present application, a weight content ratio of lithium iron manganese oxide to lithium nickel cobalt manganese oxide present in the second positive electrode active material layer is A2, satisfying: A2<1.
[0017] A second aspect of the present application provides an electrical device, wherein the electrical device comprises the secondary battery described in the first aspect of the present application.
[0018] Compared with the prior art, the beneficial effects of this application are:
[0019] The present application improves the problems of thick coating and cracking of positive electrode sheets, large impedance, and resulting poor kinetic performance, low energy density, and poor cycle performance of secondary batteries by controlling the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide in the first positive electrode active material layer to be higher than the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide in the second positive electrode active material layer, and making the average aspect ratio of the first carbon nanotubes in the first positive electrode active material layer smaller than the average aspect ratio of the second carbon nanotubes in the second positive electrode active material. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0021] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0022] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0023] The reagents or instruments used in this application without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0024] An embodiment of the present application provides a secondary battery, the secondary battery comprising a positive electrode sheet, the positive electrode sheet comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, the positive electrode active material layer comprising a first positive electrode active material layer and a second positive electrode active material layer, the first active material layer being disposed between the current collector and the second positive electrode active material layer;
[0025] The positive electrode active material layer comprises manganese iron lithium oxide and lithium nickel cobalt manganese oxide, wherein the average particle size of the lithium nickel cobalt manganese oxide is greater than the average particle size of the manganese iron lithium oxide;
[0026] wherein the weight ratio of the manganese iron lithium oxide to the lithium nickel cobalt manganese oxide present in the first positive electrode active material layer is higher than the weight ratio of the manganese iron lithium oxide to the lithium nickel cobalt manganese oxide present in the second positive electrode active material layer;
[0027] The first positive electrode active material layer includes first carbon nanotubes, and the second positive electrode active material layer includes second carbon nanotubes. The average aspect ratio of the first carbon nanotubes is smaller than the average aspect ratio of the second carbon nanotubes.
[0028] In some embodiments, the average aspect ratio of the first carbon nanotubes is 50 to 200. For example, the average aspect ratio of the first carbon nanotubes can be any one of 50, 80, 100, 120, 150, 180, and 200, or a range between any two values. When the average aspect ratio of the first carbon nanotubes is within the above range, the problem of large electronic impedance of the positive electrode sheet can be further improved, and the kinetic performance of the secondary battery can be improved.
[0029] In some embodiments, the average aspect ratio of the second carbon nanotubes is 200 to 1000. For example, the average aspect ratio of the second carbon nanotubes can be any one of 200, 300, 400, 500, 600, 700, 800, 900, 1000 or a range between any two values. When the average aspect ratio of the second carbon nanotubes is within the above range, the kinetic performance of the secondary battery can be further improved, and the problem of severe gas generation during high-temperature storage of the secondary battery can be improved.
[0030] In some embodiments, the first positive electrode active material layer includes a first binder, the second positive electrode active material layer includes a second binder, and the swelling rate of the first binder is smaller than the swelling rate of the second binder.
[0031] In some embodiments, the first positive electrode active material layer includes a first binder, and the swelling rate of the first binder is 5% to 100%. For example, the swelling rate of the first binder can be any one of 5%, 20%, 30%, 40%, 60%, 70%, 80%, 90%, 100%, or a range between any two values.
[0032] In some embodiments, the second positive electrode active material layer includes a second binder, and the swelling rate of the second binder is 30% to 500%. For example, the swelling rate of the first binder can be any one of 30%, 60%, 100%, 150%, 200%, 250%, 300%, 350%, 400%, 450%, 500%, or a range between any two values. When the swelling rate of the second binder is within the above range, it has better liquid absorption performance, shortens the ion transmission distance, thereby improving concentration polarization, reducing ionic impedance, and improving the problem of poor dynamic performance of the positive electrode sheet due to its excessive thickness.
[0033] In some embodiments, the first binder comprises polyvinylidene fluoride.
[0034] In some embodiments, the second binder comprises at least one of polyacrylate, polyhydroxyethyl acrylate, polymethyl acrylate, polymethyl methacrylate, polyvinyl acetate, polyvinyl carbonate, polytert-butyl benzoate, and polydiethyl carbonate. The above binder has good liquid absorption performance, and can be used in the second positive electrode active material layer to shorten the ion transmission distance, thereby improving concentration polarization, reducing ion impedance, and improving the problem of poor dynamic performance of the positive electrode sheet due to its excessive thickness.
[0035] In some embodiments, the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide present in the first positive electrode active material layer is A1, satisfying: A1>1. For example, the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide present in the first positive electrode active material layer can be any one of 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9 or a range between any two values. In some embodiments, A1≥1.5. In some embodiments, A1≥4.
[0036] In some embodiments, the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide present in the second positive electrode active material layer is A2, satisfying: A2<1. For example, the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide present in the second positive electrode active material layer can be any one of 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or a range between any two values. In some embodiments, A2≤0.7. In some embodiments, A2≤0.25. The second positive electrode active material layer is away from the current collector, and the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide in the second positive electrode active material layer is controlled within the above range, which can further increase the coating weight and thus increase the energy density of the secondary battery, while improving the kinetic performance of the secondary battery.
[0037] In some embodiments, the first positive electrode active material layer and the second positive electrode active material layer further include at least one of carbon black, graphite flakes, and Ketjen black.
[0038] In some embodiments, the manganese iron lithium oxide comprises a chemical formula of Li a1 Fe x1 Mn y1 M z1 A compound of PO4, wherein M comprises at least one of Mg and Ti, 0.95≤a1≤1.05, x1+y1+z1=1, 0.4≤x1<1, 0.5≤y1<1, 0≤z1≤0.05.
[0039] In some embodiments, the lithium nickel cobalt manganese oxide comprises a chemical formula of Li a2 Nix2 Co y2 Mn z2 Me p O2 compound, wherein Me contains at least one of B, Y, Nb, In, La, Zr, Ce, W, Al, Ti, Sr, Mg, Sb, V, Zn, Cu, Cr, Fe, 0.95≤a2≤1.05, 0.5≤x2<1, 0<y2≤0.2, 0<z2≤0.3, 0≤p≤0.1.
[0040] In some embodiments, the average particle size of the manganese iron lithium oxide is 0.1 to 5 μm. For example, the average particle size of the manganese iron lithium oxide can be 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm.
[0041] In some embodiments, the average particle size of the lithium nickel cobalt manganese oxide is 2 to 20 μm. For example, the average particle size of the lithium nickel cobalt manganese oxide can be any value of 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm, 18 μm, 20 μm, or a range consisting of any two of the values.
[0042] In some embodiments, the mass percentage of lithium nickel cobalt manganese oxide in the second positive electrode active material layer is 60% to 100%, based on the total mass of lithium nickel cobalt manganese oxide in the positive electrode active material layer being 100%. For example, the mass percentage of lithium nickel cobalt manganese oxide in the second positive electrode active material layer can be any value of 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, or a range consisting of any two of these values.
[0043] In some embodiments, the mass percentage of the manganese iron lithium oxide in the second positive electrode active material layer is 0% to 40%, based on the total mass of the manganese iron lithium oxide in the positive electrode active material layer being 100%. For example, the mass percentage of the manganese iron lithium oxide in the second positive electrode active material layer can be any one of 0%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, or a range consisting of any two of these values.
[0044] In some embodiments, the secondary battery further comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode material.
[0045] The type of negative electrode material is not specifically limited and can be selected according to actual needs. For example, the negative electrode material can be artificial graphite, natural graphite, silicon-carbon composite material, silicon oxide, hard carbon, lithium metal and lithium titanate.
[0046] The type of negative electrode current collector is not particularly limited and can be selected according to actual needs. Preferably, copper foil or carbon-coated copper foil can be used.
[0047] In some embodiments, the secondary battery further comprises a separator. The type of separator is not particularly limited and can be selected according to actual needs. The separator can be a polypropylene film, a polyethylene film, a polyvinylidene fluoride, a spandex film, an aramid film, or a multilayer composite film modified by a coating.
[0048] In some embodiments, the preparation of a secondary battery includes: stacking the positive electrode sheet, the separator, and the negative electrode sheet in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then winding them into a square bare cell, loading them into a battery casing, and then baking them at 65 to 95°C to remove water, injecting electrolyte, sealing, and obtaining a secondary battery after standing, hot and cold pressing, formation, clamping, capacity division and other processes.
[0049] In some embodiments, the secondary battery may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a bag-type soft package, and the material of the soft package may be plastic, such as one or more of polypropylene, polybutylene terephthalate, polybutylene succinate, etc.
[0050] In some embodiments, the shape of the secondary battery is not particularly limited, and it can be cylindrical, square, or any other shape.
[0051] The second aspect of the present application provides an electric device, which includes the secondary battery described in the first aspect of the present application. The electric device can be an application device such as a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, and an electric tool. The vehicle can be a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; the electric toy includes a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; the electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and a railway electric tool, such as an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc. The embodiments of the present application do not impose any special restrictions on the above-mentioned devices.
[0052] The following are specific embodiments of the present application, and the technical scheme of the present application is further described in conjunction with the embodiments, but the present application is not limited to these embodiments. The reagents, methods and equipment used in the present application, unless otherwise specified, are conventional reagents, methods and equipment in the art.
[0053] The average particle size of lithium iron manganese phosphate used in the following examples of the present application is 0.85 μm, and the average particle size of lithium nickel cobalt manganese oxide is 4.5 μm.
[0054] The test method for the swelling rate of the binder in the present application is: cut the binder material into 20mm*20mm specimens, place them in an electrolyte (the volume ratio of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate is 1:1:1, and the concentration of lithium hexafluorophosphate is 1 mol / L), and after standing and soaking at room temperature for 7 days, calculate the swelling rate, wherein the swelling rate = (weight after swelling - original weight) / original weight × 100%.
[0055] Example 1
[0056] Embodiment 1 provides a secondary battery, and the specific preparation process of the secondary battery includes:
[0057] (1) Preparation of positive electrode sheet
[0058] The first positive electrode active material, carbon black, the first carbon nanotube, and the first binder are mixed in a mass ratio of 96:1:1:2, and NMP is added and mixed evenly to obtain a first positive electrode slurry, wherein the lithium manganese iron phosphate (LiMn 0.6 Fe 0.4 PO4, referred to as LMFP64) and lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, referred to as NCM622) has a mass ratio of 60:40, an average aspect ratio of the first carbon nanotube is 100, the first binder is PVDF, and the swelling rate of the first binder is 30%;
[0059] The second positive electrode active material, carbon black, second carbon nanotubes, and second binder are mixed in a mass ratio of 97:1:0.5:1.5, and NMP is added and mixed evenly to obtain a second positive electrode slurry, wherein the mass ratio of lithium manganese iron phosphate (LMFP64) and lithium nickel cobalt manganese oxide (NCM622) in the second positive electrode active material is 40:60, the average aspect ratio of the second carbon nanotubes is 200, the second binder is polyacrylate, and the swelling rate of the second binder is 200%;
[0060] The first positive electrode slurry and the second positive electrode slurry are evenly coated on the aluminum foil using an extrusion double-layer coating die head. The first positive electrode slurry is the lower layer close to the current collector, and the second positive electrode slurry is the upper layer away from the current collector. The positive electrode sheets are then obtained after baking, cold pressing and cutting.
[0061] (2) Preparation of negative electrode sheet
[0062] The negative electrode materials graphite, carbon black, CMC, and SBR are mixed in a mass ratio of 94.3:1.5:1.2:3, deionized water solvent is added, and stirred under the action of a stirrer until the system is uniform to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on the negative electrode collector copper foil, placed in an oven for drying, and rolled and cut to obtain negative electrode sheets.
[0063] (3) Preparation of electrolyte
[0064] Organic solvents ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate were mixed in a volume ratio of 1:1:1. In an argon atmosphere glove box with a water content of <10 ppm, fully dried lithium hexafluorophosphate was dissolved in the above organic solvents to a content of 1 mol / L, and mixed evenly to obtain an electrolyte.
[0065] (4) Preparation of secondary batteries
[0066] The positive electrode sheet, the isolation film (polypropylene), and the negative electrode sheet are wound in order to obtain a bare cell; the bare cell is placed in an outer packaging shell, vacuum dried, injected with electrolyte, allowed to stand, formed, shaped, and capacity divided to obtain a secondary battery.
[0067] Examples 2 to 5 provide a series of secondary batteries, which differ from Example 1 in that the mass ratios of lithium manganese iron phosphate and lithium nickel cobalt manganese oxide in the first positive electrode active material and the second positive electrode active material are different, as shown in Table 1.
[0068] Embodiments 6 to 10 provide a series of secondary batteries, which differ from Embodiment 3 in that the average aspect ratios of the first carbon nanotubes and / or the second carbon nanotubes are different, as shown in Table 1 for details.
[0069] Examples 11 to 18 provide some advantageous secondary batteries, which differ from Example 7 in that the swelling rates of the first binder and / or the second binder are different, as shown in Table 1 for details.
[0070] Comparative Example 1 provides a secondary battery, which is different from Example 1 in that the mass ratios of lithium iron manganese phosphate and lithium nickel cobalt manganese oxide in the first positive electrode active material and the second positive electrode active material are different, as shown in Table 1.
[0071] Comparative Example 2 provides a secondary battery, which is different from Example 1 in that the average aspect ratio of the second carbon nanotubes is different, as shown in Table 1.
[0072] Table 1
[0073]
[0074]
[0075] The electrochemical performance of the secondary batteries prepared in the embodiments and comparative examples was tested. The specific test results are shown in Table 2.
[0076] The test method of room temperature DCR is as follows: under the test environment of 25℃, the test battery is charged to 4.4V at 0.2C constant current and constant voltage, cut off at 0.05C, then discharged to 50% SOC at 0.2C, left for 10min, and the terminal voltage V1 is recorded; then discharged at 5C (current I) for 10s, and the terminal voltage V2 is recorded. The DC impedance of the battery is calculated according to the following formula: room temperature DCR = |V1-V2| / I;
[0077] The test method of low temperature DCR is as follows: under the test environment of 25℃, the test battery is charged to 4.4V at 0.2C constant current and constant voltage, cut off at 0.05C, and then discharged to 50% SOC at 0.2C, left for 10 minutes, and the terminal voltage V1 is recorded; the battery is placed in a test environment of -20℃, left for 60 minutes, and then discharged at 0.5C (current I) for 10s, and the terminal voltage V2 is recorded. The DC impedance of the battery is calculated according to the following formula: low temperature DCR = |V1-V2| / I;
[0078] The test method for the 25℃ cycle capacity retention rate is as follows: In a 25℃ test environment, charge the test battery at 0.2C for 3 cycles to obtain the average capacity C0, then charge to 4.4V at a constant rate of 1C0, let stand for 10 minutes, discharge to 2.5V at a constant rate of 1C0, let stand for 10 minutes, repeat the charge and discharge cycle until the capacity retention rate is 80%, and record the number of cycles at this time. The battery cycle capacity retention rate is calculated according to the following formula: Cycle capacity retention rate = last cycle discharge capacity / first cycle discharge capacity × 100%;
[0079] The test method for the 70℃ storage volume expansion rate is as follows: in a 25℃ test environment, the test battery is charged at 0.2C for 3 cycles to obtain the average capacity C0 (0.2C constant rate charge to 4.4V, constant rate 0.2C discharge to 2.5V), and then fully charged at 0.2C0 and left to stand for 5 minutes, the initial volume V0 of the battery is tested by the drainage method, the fully charged cell is placed in a 70℃ high and low temperature box, and the volume V of the battery under the cabinet is tested for 60 days. The 70℃ storage volume expansion rate (%) of the battery is calculated according to the following formula: Storage volume expansion rate (%) = (V-V0) / V0*100%.
[0080] Table 2
[0081]
[0082]
[0083] From the above embodiments and comparative examples, by controlling the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide in the first positive electrode active material layer to be higher than the weight content ratio of manganese iron lithium oxide to lithium nickel cobalt manganese oxide present in the second positive electrode active material layer, and making the average aspect ratio of the first carbon nanotubes in the first positive electrode active material layer smaller than the average aspect ratio of the second carbon nanotubes in the second positive electrode active material, the problems of thick coating and cracking of the positive electrode sheet, large impedance, and resulting in poor kinetic performance of the secondary battery, low energy density, and poor cycle performance are improved.
[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A secondary battery, characterized in that: A positive electrode sheet is included, wherein the positive electrode sheet includes a current collector and a positive electrode active material layer disposed on at least one side of the current collector, wherein the positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer, and the first active material layer is disposed between the current collector and the second positive electrode active material layer; The positive electrode active material layer comprises manganese iron lithium oxide and lithium nickel cobalt manganese oxide, wherein the average particle size of the lithium nickel cobalt manganese oxide is greater than the average particle size of the manganese iron lithium oxide; wherein the weight ratio of the manganese iron lithium oxide to the lithium nickel cobalt manganese oxide present in the first positive electrode active material layer is higher than the weight ratio of the manganese iron lithium oxide to the lithium nickel cobalt manganese oxide present in the second positive electrode active material layer; The first positive electrode active material layer includes first carbon nanotubes, and the second positive electrode active material layer includes second carbon nanotubes. The average aspect ratio of the first carbon nanotubes is smaller than the average aspect ratio of the second carbon nanotubes.
2. The secondary battery according to claim 1, characterized in that: The average aspect ratio of the first carbon nanotubes is 50-200.
3. The secondary battery according to claim 1, characterized in that: The average aspect ratio of the second carbon nanotubes is 200-1000.
4. The secondary battery according to claim 1, characterized in that: The first positive electrode active material layer includes a first binder, and the second positive electrode active material layer includes a second binder. The swelling rate of the first binder is smaller than that of the second binder.
5. The secondary battery according to claim 1, characterized in that: The first positive electrode active material layer includes a first binder, and the swelling rate of the first binder is 5% to 100%.
6. The secondary battery according to claim 1, characterized in that: The second positive electrode active material layer includes a second binder, and the swelling rate of the second binder is 30% to 500%.
7. The secondary battery according to claim 4, characterized in that: The first binder comprises polyvinylidene fluoride; And / or the second binder includes at least one of polyacrylate, polyhydroxyethyl acrylate, polymethyl acrylate, polymethyl methacrylate, polyvinyl acetate, polyvinyl carbonate, polytert-butyl benzoate, polydiethyl carbonate, and hydrogenated nitrile rubber.
8. The secondary battery according to claim 1, characterized in that: The weight content ratio of the lithium iron manganese oxide to the lithium nickel cobalt manganese oxide present in the first positive electrode active material layer is A1, satisfying: A1>1.
9. The secondary battery according to claim 1, characterized in that: The weight content ratio of the lithium iron manganese oxide to the lithium nickel cobalt manganese oxide present in the second positive electrode active material layer is A2, satisfying: A2<1.
10. An electrical device, characterized in that: The electrical equipment comprises the secondary battery according to any one of claims 1 to 9.
Citation Information
Patent Citations
Lithium ion battery positive plate, preparation method thereof and lithium ion battery
CN113948673A
Positive electrode for lithium secondary battery and lithium secondary battery comprising same
CN114788042A
Battery and electric equipment
CN116130597A
Lithium ion battery and electric device
CN116613277A
Secondary battery and electric device
CN118099396A
Cited By
Battery cell, manufacturing method therefor, battery apparatus and electrical apparatus
WO2026157408A1