Battery and preparation method of battery

By introducing a second metal organic frame material layer into the lithium iron phosphate battery and using carboxylic acid groups to capture iron ions, the problems of iron ion dissolution and redox reaction of lithium iron phosphate battery during high-temperature cycle/storage process are solved, and the battery is improved stability and lifespan.

CN118943466APending Publication Date: 2024-11-12ZHEJIANG JINKO ENERGY STORAGE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411215995.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There is iron ion dissolution and redox reactions during high-temperature cycle/storage and large-scale charging and discharging of lithium iron phosphate batteries, resulting in reduced stability, SEI membrane damage and separator puncture, affecting battery life and safety.

Method used

Using a battery design including a lithium iron phosphate positive electrode material layer and a second metal organic frame material layer. The second metal organic frame material is composed of zirconium metal and tetracarboxylic acid-based ligand, with high acid and alkali resistance and stability, and is not matched. The carboxylic acid group at the position can capture and chelate dissolved iron ions, preventing them from redox reactions on the negative electrode surface.

Benefits of technology

It effectively improves the high-temperature working life and stability of lithium iron phosphate batteries, reduces the risk of iron ion dissolution and SEI film destruction, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943466A_ABST
    Figure CN118943466A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the technical field of batteries, and provides a battery and a preparation method of the battery, the battery comprises a positive pole piece and a negative pole piece, the material of the positive pole piece comprises lithium iron phosphate, and the negative pole piece comprises a negative current collector; the first negative electrode material layer covers the surface of the negative electrode current collector, and the material of the first negative electrode material layer comprises a first carbon material; the second negative electrode material layer covers the surface of the first negative electrode material layer, the material of the second negative electrode material layer comprises a second metal organic framework material, the metal of the second metal organic framework material is zirconium metal, the organic ligand of the second metal organic framework material is tetracarboxylic acid ligand, and the organic ligand of the second metal organic framework material is zirconium metal. And the tetracarboxylic ligand is connected with zirconium metal through a coordinate bond. The battery and the preparation method of the battery provided by the embodiment of the invention are at least beneficial to improving the stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the field of battery technology, and in particular to a battery and a method for preparing the battery. Background Art

[0002] With the development of lithium-ion battery research, the requirements for energy density, working voltage and cycle life are getting higher and higher. At present, the positive electrode materials of lithium-ion batteries mainly include lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, ternary materials, etc. Among them, lithium iron phosphate (LiFePO4) is widely used due to its advantages such as high capacity, environmental friendliness, high safety and long cycle life.

[0003] However, the stability of lithium iron phosphate batteries needs to be improved. Summary of the invention

[0004] The embodiments of the present application provide a battery and a method for preparing the battery, which are at least beneficial to improving the stability of the battery.

[0005] According to some embodiments of the present application, on the one hand, the embodiments of the present application provide a battery, including: a positive electrode plate and a negative electrode plate, the material of the positive electrode plate includes lithium iron phosphate, and the negative electrode plate includes: a negative electrode collector; a first negative electrode material layer, the first negative electrode material layer covers the surface of the negative electrode collector, and the material of the first negative electrode material layer includes a first carbon material; a second negative electrode material layer, the second negative electrode material layer covers the surface of the first negative electrode material layer, and the material of the second negative electrode material layer includes a second metal-organic framework material, the metal of the second metal-organic framework material is zirconium metal, and the organic ligand of the second metal-organic framework material is a tetracarboxylic acid-based ligand, and the tetracarboxylic acid-based ligand is connected to the zirconium metal through a coordination bond.

[0006] In some embodiments, the ratio of the average particle size of the first carbon material to the average particle size of the second metal organic framework material is 40-200.

[0007] In some embodiments, the particle size of the second metal organic framework material is 100 nm to 500 nm; and the particle size of the first carbon material is 5 μm to 20 μm.

[0008] In some embodiments, the second negative electrode material layer includes multiple sub-negative electrode material layers stacked in sequence along a direction away from the first negative electrode material layer, the material of each sub-negative electrode material layer includes a second carbon material and a second metal-organic framework material, and in the direction away from the first negative electrode material layer, the ratio of the mass of the second metal-organic framework material to the total mass of the second carbon material and the second metal-organic framework material in the corresponding sub-negative electrode material layer increases successively.

[0009] In some embodiments, the material of the first negative electrode material layer also includes a first metal-organic framework material; the material of the second negative electrode material layer also includes a second carbon material; wherein, in the first negative electrode material layer, the ratio of the mass of the first metal-organic framework material to the total mass of the first carbon material and the first metal-organic framework material is a first ratio; in the second negative electrode material layer, the ratio of the second metal-organic framework material to the total mass of the second carbon material and the second metal-organic framework material is a second ratio, and the second ratio is greater than the first ratio.

[0010] In some embodiments, the first ratio is 0.15-0.35; the second ratio is 0.5-0.9.

[0011] According to some embodiments of the present application, on the other hand, the embodiments of the present application also provide a method for preparing a battery, including: preparing a positive electrode sheet and a negative electrode sheet, the process steps for preparing the negative electrode sheet include: preparing a second metal organic framework material, the preparation steps include: dispersing a zirconium source in an organic solvent, adding a tetracarboxylic acid-based ligand and then performing ultrasonic treatment, then adding an acid and then performing a thermal reaction to obtain a reaction liquid, cooling, filtering and washing the reaction liquid to obtain the second metal organic framework material; blending the second metal organic framework material with a second adhesive to obtain a second negative electrode coating; blending the first carbon material with the first adhesive to obtain a first negative electrode coating; applying the first negative electrode coating to the surface of the negative electrode collector and drying to form a first negative electrode material layer on the surface of the negative electrode collector; applying the second negative electrode coating to the surface of the first negative electrode material layer and drying to form a second negative electrode material layer on the surface of the first negative electrode material layer; assembling the positive electrode sheet and the negative electrode sheet.

[0012] In some embodiments, the tetracarboxylic acid-based ligand is selected from one or more of [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid, 3,3',5,5'-biphenyltetracarboxylic acid, pyromellitic acid, 9,10-di(3',5'-dicarboxyphenyl)anthracene, 2',5'-difluoro-[1,1':4',1"-terphenyl]-3,3",5,5"-tetracarboxylic acid or pyrene-1,3,6,8-tetracarboxylic acid.

[0013] In some embodiments, the zirconium source is selected from one or more of zirconium nitrate, zirconium sulfate, zirconium phosphate, zirconium chloride, or zirconium citrate.

[0014] In some embodiments, in the step of preparing the second metal organic framework material, the molar ratio of the zirconium source to the tetracarboxylic acid-based ligand is 1:1 to 4:1, the mass ratio of the solvent to the acid is 2:1 to 5:1, the temperature of the thermal reaction is 60°C to 100°C, and the time of the thermal reaction is 12h to 48h.

[0015] The technical solution provided by the embodiments of the present application has at least the following advantages:

[0016] The battery provided by the implementation of the present application includes a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive electrode collector and a positive electrode material layer covering the surface of the positive electrode collector, and the material of the positive electrode material layer is lithium iron phosphate; the negative electrode plate includes a negative electrode collector, a first negative electrode material layer and a second negative electrode material layer, the material of the first negative electrode material layer includes a first carbon material, and the material of the second negative electrode material layer includes a second metal organic framework material, and the second metal organic framework material is a zirconium-based metal organic framework material composed of zirconium metal and tetracarboxylic acid-based ligands, thereby forming a lithium iron phosphate battery. Among them, the second metal organic framework material has good acid and alkali resistance and high stability, and there are uncoordinated, exposed carboxylic acid groups in the second metal organic framework material, and the carboxylic acid groups can capture and chelate metal ions. In this way, the second metal organic framework material, as the outermost layer of the negative electrode plate, can use the carboxylic acid groups to capture the iron ions dissolved from the positive electrode to avoid the iron ions from undergoing redox reactions and depositing on the surface of the negative electrode plate, thereby avoiding the SEI film on the surface of the negative electrode plate from being damaged or piercing the diaphragm, thereby improving the high temperature operating life of the lithium iron phosphate battery and improving the stability of the lithium iron phosphate battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] One or more embodiments are exemplarily illustrated by the pictures in the corresponding drawings. These exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the pictures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present application or the technical solutions in the traditional technology, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A schematic diagram of the electrochemical structure of a battery provided in an embodiment of the present application;

[0019] Figures 2 to 4 A schematic diagram of the cross-sectional structure of various negative electrode sheets provided in the embodiments of the present application;

[0020] Figure 5a to Figure 5f The chemical formulas of various tetracarboxylic acid-based ligands provided in the examples of the present application;

[0021] Figure 6 The cycle performance test diagram of two batteries provided in the embodiments of the present application;

[0022] Figure 7 A test chart of the capacity retention rate of two batteries provided in the embodiments of the present application;

[0023] Figure 8 A test chart of the capacity recovery rate of two batteries provided in an embodiment of the present application. DETAILED DESCRIPTION

[0024] As known from the background technology, lithium iron phosphate batteries have stability problems.

[0025] Lithium iron phosphate (LiFePO4), as a positive electrode material for lithium-ion batteries, has attracted much attention due to its stable olivine structure and excellent cycle performance. The iron in lithium iron phosphate positive electrode materials is prone to dissolution under normal working conditions, and this phenomenon is more obvious during high-temperature cycling / storage and high-rate charge and discharge. This is mainly because at high temperatures, the lithium salt in the electrolyte will accelerate the dissolution of iron in the lithium iron phosphate positive electrode material. The dissolved iron ions precipitate on the surface of the negative electrode material and form elemental iron, which accelerates the thickening of the solid electrolyte interface (SEI) and affects the battery capacity attenuation. In addition, elemental iron may pierce the diaphragm, resulting in reduced stability of the lithium iron phosphate battery.

[0026] At present, the main methods to reduce the iron dissolution problem of lithium iron phosphate positive electrode materials include surface modification, bulk doping or optimization of electrolyte. Surface modification is to coat lithium iron phosphate with materials such as graphene or amorphous carbon, but graphene is a two-dimensional material, and it often cannot wrap lithium iron phosphate well to form an ideal core-shell structure; different carbon contents in amorphous carbon have different coating effects on lithium iron phosphate, resulting in different particle sizes and morphologies formed after calcination, and carbon does not participate in electrochemical reactions in positive electrode materials. Excessive carbon coating will reduce the content of active substances, resulting in a decrease in the specific capacity and energy density of the positive electrode material. Too low carbon content does not significantly improve the electrochemical performance of the positive electrode material. Bulk doping is to improve the stability of lithium iron phosphate positive electrode materials by cation doping, anion doping or composite doping, but this method introduces other impurity elements, which will have a certain impact on battery capacity and other aspects. Optimizing the electrolyte is to improve the cycle performance of the electrolyte by changing the conductive salt and using additives. For example, the use of lithium bis(oxalatoborate) (LiBOB) lithium salt can reduce the generation of hydrofluoric acid (HF), reduce the dissolution of metallic iron ions, and improve the high-temperature cycle performance of lithium iron phosphate batteries.

[0027] Although the above methods can reduce the dissolution of metallic iron, the dissolution of iron ions will be accelerated under conditions of high-temperature cycling / storage and increased charge and discharge rates. Therefore, some iron ions will still be dissolved and deposited on the surface of the negative electrode material, causing battery capacity decay. The precipitated elemental iron may also pierce the diaphragm and cause safety hazards.

[0028] The present application provides a battery and a method for preparing the battery. The positive electrode plate of the battery includes a positive electrode collector and a positive electrode material layer covering the surface of the positive electrode collector, and the material of the positive electrode material layer is lithium iron phosphate; the negative electrode plate of the battery includes a negative electrode collector, a first negative electrode material layer and a second negative electrode material layer, and the material of the first negative electrode material layer includes a first carbon material, and the material of the second negative electrode material layer includes a second metal organic framework material, and the second metal organic framework material is a zirconium-based metal organic framework material composed of zirconium metal and tetracarboxylic acid-based ligands, so as to form a lithium iron phosphate battery. Among them, the second metal organic framework material has good acid and alkali resistance and high stability, and there are uncoordinated, exposed carboxylic acid groups in the second metal organic framework material, and the carboxylic acid groups can capture and chelate metal ions. In this way, the second metal organic framework material, as the outermost layer of the negative electrode plate, can use the carboxylic acid groups to capture the iron ions dissolved from the positive electrode to avoid the iron ions from undergoing redox reactions and depositing on the surface of the negative electrode plate, thereby avoiding the SEI film on the surface of the negative electrode plate from being damaged or piercing the diaphragm, thereby improving the high temperature operating life of the lithium iron phosphate battery and improving the stability of the lithium iron phosphate battery.

[0029] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0030] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0031] In the accompanying drawings corresponding to the embodiments of the present application, the thickness and area of ​​the layer are magnified for better understanding and ease of description. When describing a component on another component or on the surface of another component, the component may be "directly" located on the surface of the other component, or a third component may be present between the two components. On the contrary, when describing a component on the surface of another component or when another component is formed or provided on the surface of a component, it means that there is no third component between the two components. In addition, when describing a component as "substantially" formed on another component, it means that the component is not formed on the entire surface (or front surface) of the other component, nor is it formed on a partial edge of the entire surface.

[0032] In the description of the embodiments of the present application, when a certain component “includes” another component, unless otherwise stated, other components are not excluded and other components may be further included.

[0033] The terms used in the description of the various described embodiments herein are used only to describe specific embodiments and are not intended to be limiting. As used in the description of the various described embodiments and the appended claims, "components" are also intended to include plural forms unless the context clearly indicates otherwise.

[0034] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0035] Figure 1 This is a schematic diagram of the electrochemical structure of the battery provided in the embodiment of the present application. To facilitate the explanation of the working principle of the battery, Figure 1 What is shown in the figure is the electrochemical principle diagram of the battery, not the structural diagram of the actual battery product.

[0036] refer to Figure 1 The battery provided in the embodiment of the present application includes: a positive electrode plate 100 and a negative electrode plate 200, the material of the positive electrode plate 100 includes lithium iron phosphate, specifically, the positive electrode plate 100 includes a positive electrode collector 110 and a positive electrode material layer 120 covering the surface of the positive electrode collector 110, the material of the positive electrode material layer 120 is lithium iron phosphate; the negative electrode plate 200 includes a negative electrode collector 210, a first negative electrode material layer 220 and a second negative electrode material layer 230, the first negative electrode material layer 220 covers the surface of the negative electrode collector 210, the material of the first negative electrode material layer 220 includes a first carbon material; the second negative electrode material layer 230 covers the surface of the first negative electrode material layer 220, the material of the second negative electrode material layer 230 includes a second metal organic framework material, the metal of the second metal organic framework material is zirconium metal, the organic ligand of the second metal organic framework material is a tetracarboxylic acid-based ligand, and the tetracarboxylic acid-based ligand is connected to the zirconium metal through a coordination bond.

[0037] In the battery provided in the embodiment of the present application, the positive electrode plate 100 includes a positive electrode current collector 110 and a positive electrode material layer 120 covering the surface of the positive electrode current collector 110, and the material of the positive electrode material layer 120 is lithium iron phosphate; the negative electrode plate 200 includes a negative electrode current collector 210, a first negative electrode material layer 220 and a second negative electrode material layer 230, and the material of the first negative electrode material layer 220 includes a first carbon material, and the material of the second negative electrode material layer 230 includes a second metal organic framework material, and the second metal organic framework material is a zirconium-based metal organic framework material (Zr-MOF-(COOH)) composed of zirconium metal and tetracarboxylic acid-based ligands. n ), thus forming a lithium iron phosphate battery. Among them, the second metal organic framework material has good acid and alkali resistance and high stability, and there are uncoordinated, exposed carboxylic acid groups in the second metal organic framework material, and the carboxylic acid groups can capture and chelate metal ions. In this way, the second metal organic framework material, as the outermost layer of the negative electrode plate 200, can use the carboxylic acid groups to capture the iron ions dissolved from the positive electrode to avoid the iron ions from undergoing redox reactions and depositing on the surface of the negative electrode plate 200, thereby avoiding the SEI film on the surface of the negative electrode plate 200 from being destroyed or piercing the diaphragm 400, so as to improve the high temperature working life of the lithium iron phosphate battery and improve the stability of the lithium iron phosphate battery.

[0038] In some embodiments, there may be some impure metal ions in the positive electrode material layer 120 , and these impure metal ions may also be dissolved out. The second metal organic framework material may also capture and chelate the impure metal ions dissolved out of the positive electrode material layer 120 .

[0039] The material of the positive electrode current collector 110 may include aluminum, nickel, stainless steel, a composite material, a conductive polymer, or a conductive resin.

[0040] The material of the negative electrode current collector 210 may include copper, aluminum, nickel, stainless steel, a composite material, a conductive polymer, or a conductive resin.

[0041] In a specific example, the material of the positive electrode current collector 110 may be aluminum foil, and the material of the negative electrode current collector 210 may be copper foil.

[0042] In the drawings provided in this embodiment, the electrolyte between the positive electrode sheet 100 and the negative electrode sheet 200 is an electrolyte 300 as an example, the positive electrode sheet 100 and the negative electrode sheet 200 are immersed in the electrolyte 300, and a separator 400 is provided between the positive electrode sheet 100 and the negative electrode sheet 200. In other embodiments, a solid electrolyte or a solid-liquid mixed electrolyte may be provided between the positive electrode sheet and the negative electrode sheet, and a separator is provided between the positive electrode sheet and the negative electrode sheet.

[0043] The following describes the charging and discharging process of the battery using the electrolyte 300 as an electrolyte:

[0044] During the charging of the battery, after the lithium ions of the lithium iron phosphate in the positive electrode material layer 120 are deintercalated, the lithium iron phosphate is converted into iron phosphate, and the deintercalated lithium ions enter the electrolyte 300 from the surface of the positive electrode material layer 120 under the action of the electric field force, and migrate to the surface of the negative electrode plate 200 after passing through the diaphragm 400, and then embed into the lattice of the first carbon material in the first negative electrode material layer 220. During the discharge of the battery, the lithium ions in the lattice of the first carbon material in the first negative electrode material layer 220 are deintercalated, enter the electrolyte 300, and migrate to the surface of the positive electrode material layer 120 after passing through the diaphragm 400, and then re-embed into the lattice of iron phosphate, and the iron phosphate is converted into lithium iron phosphate.

[0045] In some embodiments, the material of the separator 400 may be a polyolefin separator, a modified polyolefin separator, a non-woven separator, and a ceramic composite separator.

[0046] In some embodiments, the electrolyte 300 includes main components such as a solvent, a lithium salt, and an additive. The solvent is the main component of the electrolyte 300 and is used to dissolve other components to form an ion-conductive medium. The solvent can be selected from organic carbonates, such as acrylate, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC).

[0047] Figures 2 to 4 Schematic diagram of various cross-sectional structures of negative electrode sheets provided in the embodiments of the present application. Figures 2 to 4 Only the first negative electrode material layer and the second negative electrode material layer on one surface of the negative electrode current collector are shown.

[0048] refer to Figure 2 In one example, the first negative electrode material layer 220 includes a first adhesive 222 and particles 221 of a first carbon material dispersed in the first adhesive 222 ; the second negative electrode material layer 230 includes a second adhesive layer 232 and particles 231 of a second metal organic framework material dispersed in the second adhesive layer 232 .

[0049] like Figure 2 As shown, when the surface of the negative electrode collector 210 is coated with a first negative electrode material layer 220 including a first carbon material, and the surface of the first negative electrode material layer 220 is coated with a second negative electrode material layer 230 including a second metal organic framework material, the ratio of the average particle size of the particles 221 of the first carbon material to the average particle size of the particles 231 of the second metal organic framework material can be 40 to 200, for example, 40 to 80, 80 to 100, 100 to 150 or 150 to 200, specifically 40, 60, 80, 100, 130, 160, 180 or 200.

[0050] The average particle size refers to the equivalent diameter of the largest particle when the cumulative distribution in the particle size distribution curve is 50%.

[0051] In some embodiments, the particle size of the second metal organic framework material particle 231 is 100nm to 500nm, for example, 100nm to 200nm, 200nm to 300nm, 300nm to 400nm or 400nm to 500nm, and specifically can be 100nm, 130nm, 160nm, 190nm, 200nm, 210nm, 240nm, 270nm, 300nm, 320nm, 350nm, 380nm, 400nm, 440nm or 500nm. It is understandable that the particle size of different single second metal organic framework material particles 231 may be different, and therefore, the particle size of the second metal organic framework material particles 231 fluctuates within a certain range.

[0052] In some embodiments, the particle size of the first carbon material particle 221 is 5 μm to 20 μm, for example, 5 μm to 8 μm, 8 μm to 10 μm, 10 μm to 13 μm, 13 μm to 16 μm, 16 μm to 18 μm or 18 μm to 20 μm, and specifically can be 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 17 μm, 18 μm or 20 μm. It is understandable that the particle size of different single first carbon material particles 221 may be different, and therefore, the particle size of the first carbon material particles 221 fluctuates within a certain range.

[0053] refer to Figure 3 In another example, the material of the first negative electrode material layer 220 includes a first carbon material and a first metal organic framework material; the material of the second negative electrode material layer 230 includes a second metal organic framework material and a second carbon material. Specifically, the first negative electrode material layer 220 includes a first bonding layer 222 and particles 223 of the first metal organic framework material and particles 221 of the first carbon material dispersed in the first bonding layer 222, and the second negative electrode material layer 230 includes a second bonding layer 232 and particles 231 of the second metal organic framework material and particles 233 of the second carbon material dispersed in the second bonding layer 232.

[0054] In some embodiments, the first carbon material and the second carbon material are of the same type, and the first metal organic framework material and the second metal organic framework material are the same. For example, in one example, after a first negative electrode material layer 220 including a first carbon material is formed on the surface of the negative electrode current collector 210, a second negative electrode material layer 230 including a second metal organic framework material is formed on the surface of the first negative electrode material layer 220. The first carbon material in the first negative electrode material layer 220 may penetrate into the second negative electrode material layer 230, and the second metal organic framework material in the second negative electrode material layer 230 may penetrate into the first negative electrode material layer 220, thereby forming a Figure 3 In another example, when making the first negative electrode material layer 220 and the second negative electrode material layer 230, the first carbon material and the second carbon material can be directly selected to be of the same type, and the first metal organic framework material and the metal organic framework material can be of the same type, thereby forming Figure 3 The structure shown.

[0055] In some embodiments, reference Figure 3 When manufacturing the first negative electrode material layer 220 and the second negative electrode material layer 230 , the first carbon material and the second carbon material may be of different types, and the first metal organic framework material and the second metal organic framework material may be of different types.

[0056] The ratio of the average particle size of the particles 221 of the first carbon material to the average particle size of the particles 223 of the first metal organic framework material can be 40 to 200, for example, 40 to 80, 80 to 100, 100 to 150 or 150 to 200, specifically 40, 60, 80, 100, 130, 160, 180 or 200, wherein the average particle size refers to the equivalent diameter of the largest particle when the cumulative distribution in the particle size distribution curve is 50%.

[0057] In some embodiments, the particle size of the particles 223 of the first metal organic framework material can be 100nm to 500nm, for example, 100nm to 200nm, 200nm to 350nm, 350nm to 440nm or 440nm to 500nm, and can be specifically 100nm, 130nm, 160nm, 190nm, 200nm, 210nm, 240nm, 270nm, 300nm, 320nm, 350nm, 380nm, 400nm, 440nm or 500nm. It is understandable that the particle size of the particles 223 of different first metal organic framework materials may be different, and therefore, the particle size of the particles 223 of the first metal organic framework material fluctuates within a certain range.

[0058] The ratio of the average particle size of the particles 233 of the second carbon material to the average particle size of the particles 231 of the second metal organic framework material can be 40 to 200, for example, 40 to 80, 80 to 100, 100 to 150 or 150 to 200, specifically 40, 60, 80, 100, 130, 160, 180 or 200, wherein the average particle size refers to the equivalent diameter of the largest particle when the cumulative distribution in the particle size distribution curve is 50%.

[0059] In some embodiments, the particle size of the second carbon material particles 233 may be 5 μm to 20 μm, for example, 5 μm to 8 μm, 8 μm to 10 μm, 10 μm to 13 μm, 13 μm to 16 μm, 16 μm to 18 μm or 18 μm to 20 μm, and specifically may be 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 17 μm, 18 μm or 20 μm. It is understood that the particle sizes of the particles 233 of different second carbon materials may be different, and therefore, the particle size of the particles 233 of the second carbon material fluctuates within a certain range.

[0060] In some embodiments, continue to refer to Figure 3 , when the material of the first negative electrode material layer 220 includes the first carbon material and the first metal organic framework material, and the material of the second negative electrode material layer 230 includes the second metal organic framework material and the second carbon material, in the first negative electrode material layer 220, the ratio of the mass of the first metal organic framework material to the total mass of the first carbon material and the first metal organic framework material is a first ratio; in the second negative electrode material layer 230, the ratio of the second metal organic framework material to the total mass of the second carbon material and the second metal organic framework material is a second ratio, and the second ratio is greater than the first ratio. It can be understood that the second negative electrode material layer 230, as the outermost layer of the negative electrode plate 200, needs to be in contact with the electrolyte. In the second negative electrode material layer 230, the mass of the second metal organic framework material in the second negative electrode material layer 230 accounts for a large proportion, and can absorb more electrolyte and capture or chelate iron ions at the same time, so as to avoid the formation of iron element after the redox reaction of the iron ions, thereby avoiding iron from destroying the SEI film on the surface of the negative electrode plate 200, and improving the performance and stability of the battery.

[0061] The first ratio may be 0.15 to 0.35, for example, 0.15 to 0.18, 0.18 to 0.3 or 0.3 to 0.35, and specifically may be 0.15, 0.16, 0.18, 0.2, 0.23, 0.26, 0.29, 0.3, 0.33 or 0.35.

[0062] The second ratio can be 0.5-0.9, for example 0.5-0.6, 0.6-0.8 or 0.8-0.9, and specifically can be 0.5, 0.56, 0.58, 0.6, 0.61, 0.64, 0.69, 0.7, 0.73, 0.75, 0.77, 0.8, 0.82, 0.85, 0.85 or 0.9.

[0063] refer to Figure 4 In another example, the second negative electrode material layer 230 includes a plurality of sub-negative electrode material layers 240 stacked in sequence along a direction away from the first negative electrode material layer 220, and the material of each sub-negative electrode material layer 240 includes a second carbon material and a second metal-organic framework material. Specifically, each sub-negative electrode material layer 240 includes a second bonding layer 232 and particles 233 of the second carbon material and particles 231 of the second metal-organic framework material dispersed in the second bonding layer 232, and in the direction away from the first negative electrode material layer 220, the ratio of the mass of the second metal-organic framework material to the total mass of the second carbon material and the second metal-organic framework material in the corresponding sub-negative electrode material layer 240 increases successively. In this way, the mass proportion of the second metal-organic framework material in the outermost sub-negative electrode material layer 240 is relatively large, and there are more uncoordinated, exposed carboxylic acid groups that can be used to capture and chelate iron ions. In the direction close to the surface of the negative electrode current collector 210, the possibility of iron ions penetrating multiple sub-negative electrode material layers 240 layer by layer gradually decreases. Therefore, the mass proportion of the second metal-organic framework material in the sub-negative electrode material layer 240 in the corresponding sub-negative electrode material layer 240 can be reduced, while the mass proportion of the second carbon material in the corresponding sub-negative electrode material layer 240 gradually increases, so that a good conductive channel can be formed to give full play to the electrochemical properties of the second carbon material and the first carbon material.

[0064] exist Figure 4 In the example, the number of sub-negative electrode material layers 240 is 3, which does not limit the number of sub-negative electrode material layers 240. In other embodiments, the number of sub-negative electrode material layers in the second negative electrode material layer can be 2, 4 or 5.

[0065] The first carbon material may be selected from one or more of natural graphite, artificial graphite, soft carbon and hard carbon.

[0066] The second carbon material may be selected from one or more of natural graphite, artificial graphite, soft carbon and hard carbon.

[0067] Figure 5a is the chemical formula of [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid; Figure 5b is the chemical formula of 3,3',5,5'-biphenyltetracarboxylic acid; Figure 5c is the chemical formula of pyromellitic acid; Figure 5dis the chemical formula of 9,10-di(3',5'-dicarboxyphenyl)anthracene; Figure 5e is the chemical formula of 2',5'-difluoro-[1,1':4',1"-terphenyl]-3,3",5,5"-tetracarboxylic acid; Figure 5f It is the chemical formula of pyrene-1,3,6,8-tetracarboxylic acid.

[0068] In some embodiments, reference Figure 5a to Figure 5f The tetracarboxylic acid-based ligand of the second metal organic framework material can be one or more of [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid, 3,3',5,5'-biphenyltetracarboxylic acid, pyromellitic acid, 9,10-di(3',5'-dicarboxyphenyl)anthracene, 2',5'-difluoro-[1,1':4',1"-terphenyl]-3,3",5,5"-tetracarboxylic acid or pyrene-1,3,6,8-tetracarboxylic acid.

[0069] In some embodiments, the metal of the first metal organic framework material can be selected from one or more of zirconium, hafnium, cerium, copper, zinc, titanium, iron, vanadium, molybdenum, niobium or chromium, and the organic ligand can be not narrowly limited and can be selected from any organic ligand conventionally used in the production of metal organic framework materials. Suitable organic ligands generally include at least two functional groups selected from carboxylic acid, boric acid, amine, nitro, anhydride, hydroxyl and combinations thereof.

[0070] The material of the first adhesive layer 222 can be selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), sodium alginate, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate or polyhexafluoropropylene.

[0071] The material of the second adhesive layer 232 can be selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), sodium alginate, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate or polyhexafluoropropylene.

[0072] In some embodiments, the material of the first adhesive layer 222 and the material of the second adhesive layer 232 may be the same or different.

[0073] In some embodiments, the porosity of the particles 231 of the second metal organic framework material can be 80%-95%, for example, 80%-83%, 83%-86%, 86%-89%, 89%-91% or 91%-95%, specifically 80%, 82%, 86%, 88%, 90%, 92%, 94% or 95%. The particles 231 of the second metal organic framework material have a large porosity, which can increase the amount of electrolyte 300 absorbed by the negative electrode plate 200, thereby improving battery performance.

[0074] In the battery provided in the embodiment of the present application, the positive electrode plate 100 includes a positive electrode collector 110 and a positive electrode material layer 120 covering the surface of the positive electrode collector 110, and the material of the positive electrode material layer 120 is lithium iron phosphate; the negative electrode plate 200 includes a negative electrode collector 210, a first negative electrode material layer 220 and a second negative electrode material layer 230, and the material of the first negative electrode material layer 220 includes a first carbon material, and the material of the second negative electrode material layer 230 includes a second metal organic framework material, and the second metal organic framework material is a zirconium-based metal organic framework material composed of zirconium metal and tetracarboxylic acid-based ligands, thereby forming a lithium iron phosphate battery. Among them, the second metal organic framework material has good acid and alkali resistance and high stability, and there are uncoordinated, exposed carboxylic acid groups in the second metal organic framework material, and the carboxylic acid groups can capture and chelate metal ions. In this way, the second metal organic framework material, as the outermost layer of the negative electrode plate 200, can use the carboxylic acid groups to capture the iron ions dissolved from the positive electrode to avoid the iron ions from undergoing redox reactions and depositing on the surface of the negative electrode plate 200, thereby avoiding the SEI film on the surface of the negative electrode plate 200 from being damaged or piercing the diaphragm 400, so as to improve the high temperature operating life of the lithium iron phosphate battery and improve the stability of the lithium iron phosphate battery.

[0075] Correspondingly, another embodiment of the present application also provides a method for preparing a battery, which can be used to manufacture the battery provided in the above embodiment. The method for preparing a battery provided in another embodiment of the present application will be described in detail below. For the parts that are the same or corresponding to the previous embodiment, please refer to the corresponding description of the previous embodiment, and will not be described in detail below.

[0076] The method for preparing a battery provided in the embodiment of the present application comprises:

[0077] Prepare positive electrode sheets and negative electrode sheets, and assemble the positive electrode sheets and negative electrode sheets.

[0078] The process for preparing the negative electrode sheet includes steps S101 to S105:

[0079] S101: preparing a second metal organic framework material, the preparation steps comprising: dispersing a zirconium source in an organic solvent, adding a tetracarboxylic acid-based ligand and then performing ultrasonic treatment, adding an acid and then performing a thermal reaction to obtain a reaction solution, and cooling, filtering and washing the reaction solution to obtain the second metal organic framework material.

[0080] In some embodiments, the zirconium source may be selected from one or more of zirconium nitrate, zirconium sulfate, zirconium phosphate, zirconium chloride, or zirconium citrate.

[0081] In some embodiments, the organic solvent can be selected from one or more of N,N-dimethylformamide (DMF), N,N-diethylformamide (DEF), dimethylacetamide (DMA), water, ethanol, methanol, ethanol, propanol, and acetone.

[0082] In some embodiments, the tetracarboxylic acid-based ligand is selected from one or more of [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid, 3,3',5,5'-biphenyltetracarboxylic acid, pyromellitic acid, 9,10-di(3',5'-dicarboxyphenyl)anthracene, 2',5'-difluoro-[1,1':4',1"-terphenyl]-3,3",5,5"-tetracarboxylic acid or pyrene-1,3,6,8-tetracarboxylic acid.

[0083] In some embodiments, the acid can be selected from one or more of sulfuric acid, nitric acid, hydrochloric acid, acetic acid, formic acid, or trifluoroacetic acid.

[0084] In some embodiments, in the step of preparing the second metal organic framework material, the molar ratio of the zirconium source to the tetracarboxylic acid-based ligand is 1:1 to 4:1, for example, 1:1 to 2:1, 2:1 to 3:1 or 3:1 to 4:1, specifically 1:1, 1.2:1, 1.5:1, 1.8:1, 2:1, 2.3:1, 2.6:1, 2.8:1, 3:1, 3.5:1 or 4:1; the mass ratio of the solvent to the acid is 2:1 to 5:1, specifically 2:1, 2.3:1, 2.5:1, 2.8:1, :1, 3:1, 3.3:1, 3.6:1, 3.9:1, 4:1, 4.4:1, 4.8:1 or 5:1; the temperature of the thermal reaction is 60℃~100℃, specifically 60℃, 66℃, 70℃, 75℃, 80℃, 84℃, 90℃, 95℃ or 100℃; the time of the thermal reaction is 12h~48h, specifically 12h, 14h, 16h, 18h, 20h, 23h, 26h, 29h, 32h, 34h, 38h, 40h, 44h, 48h.

[0085] S102: Blending a second metal organic framework material with a second adhesive to obtain a second negative electrode coating.

[0086] In some embodiments, the second adhesive can be selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), sodium alginate, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate or polyhexafluoropropylene.

[0087] In some embodiments, a conductive agent may be added when the second metal organic framework material is blended with the second adhesive, and the conductive agent includes one or more of conductive carbon black, acetylene black, carbon black (Super-P), Ketjen black (KT-Black), conductive carbon balls, conductive graphite, carbon nanotubes, conductive carbon fibers, graphene and reduced graphene oxide.

[0088] In some embodiments, the method for blending the second metal organic framework material with the second adhesive can adopt a slurry method, and the stirring speed can be 20rpm / min~100rpm / min, for example, 20rpm / min~40rpm / min, 40rpm / min~70rpm / min, 70rpm / min~90rpm / min or 90rpm / min~100rpm / min, specifically 20rpm / min, 30rpm / min, 40rpm / min, 50rpm / min, 60rpm / min, 70rpm / min, 80rpm / min, 90rpm / min or 100rpm / min; the stirring time can be 0.5h~1h, for example, 0.5h~0.7h, 0.7h~0.9h or 0.9h~1h, specifically 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h.

[0089] S103: Blending the first carbon material with the first adhesive to obtain a first negative electrode coating.

[0090] In some embodiments, the first carbon material is selected from one or more of natural graphite, artificial graphite, soft carbon, and hard carbon.

[0091] In some embodiments, a conductive agent can also be added when the first carbon material is blended with the first adhesive, and the conductive agent includes one or more of conductive carbon black, acetylene black, carbon black (Super-P), Ketjen black (KT-Black), conductive carbon balls, conductive graphite, carbon nanotubes, conductive carbon fibers, graphene and reduced graphene oxide.

[0092] In some embodiments, the first adhesive can be selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), sodium alginate, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate or polyhexafluoropropylene.

[0093] In some embodiments, the method for blending the first carbon material and the first adhesive can adopt a slurry method, and the stirring speed can be 20rpm / min~100rpm / min, for example, 20rpm / min~50rpm / min, 50rpm / min~80rpm / min or 80rpm / min~100rpm / min, specifically 20rpm / min, 30rpm / min, 40rpm / min, 50rpm / min, 60rpm / min, 70rpm / min, 80rpm / min, 90rpm / min or 100rpm / min; the stirring time can be 0.5h~1h, for example, 0.5h~0.8h or 0.8h~1h, specifically 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h.

[0094] S104: applying a first negative electrode coating to the surface of the negative electrode current collector and drying the coating to form a first negative electrode material layer on the surface of the negative electrode current collector.

[0095] S105: coating the second negative electrode coating on the surface of the first negative electrode material layer and drying the coating to form a second negative electrode material layer on the surface of the first negative electrode material layer.

[0096] The following are specific embodiments of the present application:

[0097] Example 1

[0098] Prepare positive electrode sheets and negative electrode sheets, and assemble the positive electrode sheets and negative electrode sheets to form a battery. The positive electrode sheet is composed of aluminum foil and a positive electrode material layer covering the surface of the aluminum foil. The positive electrode material layer is composed of polyvinylidene fluoride and lithium iron phosphate dispersed in polyvinylidene fluoride. The preparation steps of the negative electrode sheet refer to the above steps S101 to S105. In step S101, the zirconium source is selected from zirconium nitrate, the organic solvent is selected from N,N-dimethylformamide, the tetracarboxylic acid-based ligand is selected from [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid, the acid is selected from hydrochloric acid, the mass of N,N-dimethylformamide is 2g, the molar ratio of zirconium nitrate to N,N-dimethylformamide is 2:1, the mass ratio of N,N-dimethylformamide to hydrochloric acid is 3:1, the temperature of the thermal reaction is 80°C, and the time of the thermal reaction is 24h; in step S102, The second adhesive is selected from polyvinylidene fluoride, the average particle size of the particles of the second metal organic framework material is 100nm, and the slurry method is used for blending and stirring, the stirring speed is 60rpm / min, and the stirring time is 1h; in step S103, the first carbon material is selected from natural graphite, the ratio of the average particle size of the particles of the first carbon material to the average particle size of the particles of the second metal organic framework material is 100, the first adhesive is selected from polyvinylidene fluoride, and the slurry method is used for blending and stirring, the stirring speed is 60rpm / min, and the stirring time is 1h; in step S104, the negative electrode current collector is selected from copper foil.

[0099] Comparative Example 1

[0100] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that the second negative electrode material layer is not formed on the surface of the negative electrode current collector of Comparative Example 1.

[0101] The above-mentioned Example 1 and Comparative Example 1 were subjected to a cycle performance test, a capacity retention rate test and a capacity recovery rate test.

[0102] Figure 6 The cycle performance test diagram of the two batteries provided in the embodiments of the present application. Curve a corresponds to the battery of Example 1, and curve b corresponds to the battery of Example 1. The cycle performance test conditions are: charging and discharging at a temperature of 45°C and a charge and discharge power of 1P, with a cycle voltage of 2.5V to 3.65V, and the number of cycles is 800.

[0103] Figure 7 This is a test graph of the capacity retention rate of two batteries provided in the embodiments of the present application. Curve c corresponds to the battery of Example 1, and curve d corresponds to the battery of Example 1. The test temperature is 55°C and the test time is 90 days.

[0104] Figure 8This is a test graph of the capacity recovery rate of two batteries provided in the embodiments of the present application. Curve e corresponds to the battery of Example 1, and curve f corresponds to the battery of Example 1. The test temperature is 55°C and the test time is 90 days.

[0105] refer to Figures 6 to 8 It can be found that compared with the battery in Comparative Example 1 in which the second negative electrode material layer is not arranged on the surface of the negative electrode collector, the battery provided in this embodiment has better cycle performance, capacity retention rate and capacity recovery rate. The battery and the preparation method of the battery provided in the embodiment of the present application can improve the stability of the lithium iron phosphate battery.

[0106] The preparation methods of Examples 2 to 5 are basically the same as the preparation method of Example 1, except that the average particle size of the particles of the second metal organic framework material or the average particle size of the particles of the first carbon material in different embodiments is different. The resistivity test of the negative electrode sheet in the above embodiments is performed, as shown in the following table:

[0107]

[0108] According to Examples 1 to 3, it is found that when the average particle size of the particles of the second metal organic framework material and the average particle size of the particles of the first carbon material are both within an appropriate range, and the ratio of the average particle size of the particles 221 of the first carbon material to the average particle size of the particles 231 of the second metal organic framework material is within an appropriate range, it can be beneficial to the reversible deintercalation of lithium ions, thereby making the resistivity of the negative electrode sheet lower. According to Examples 4 and 5, it is found that when the average particle size of the particles of the second metal organic framework material and the average particle size of the particles of the first carbon material are both within an appropriate range, but the ratio of the average particle size of the particles 221 of the first carbon material to the average particle size of the particles 231 of the second metal organic framework material is not within an appropriate range, it is easy to cause uneven coating problems, resulting in the inability to form an effective conductive network, thereby making the resistivity of the negative electrode sheet higher.

[0109] The preparation methods of Examples 6 to 9 are basically the same as the preparation method of Example 1, except that in step S103 of Examples 6 to 9, a first metal organic framework material is further added to blend to obtain a first negative electrode coating, the first metal organic framework material is the same as the second metal organic framework material, and the mass of the first metal organic framework material in different embodiments accounts for a different proportion B1 of the total mass of the first metal organic framework material and the first carbon material; in step S102 of Examples 6 to 9, a second carbon material is further added to blend to obtain a second negative electrode coating, the second carbon material is the same as the first carbon material, and the mass of the second metal organic framework material in different embodiments accounts for a different proportion B2 of the total mass of the second metal organic framework material and the second carbon material. The rate performance test was performed on Examples 6 to 9, and the test results are shown in the following table:

[0110] B1 B2 2P capacity retention rate Example 6 0.2 0.7 97.2% Example 7 0.15 0.9 95.6% Example 8 0.35 0.5 92.2% Example 9 0.5 0.2 89.1%

[0111] According to Examples 6 to 8, it is found that when the ratio B1 of the mass of the first metal-organic framework material to the total mass of the first metal-organic framework material and the first carbon material is within an appropriate range, the ratio B2 of the mass of the second metal-organic framework material to the total mass of the second metal-organic framework material and the second carbon material is within an appropriate range, and the ratio B1 of the mass of the first metal-organic framework material to the total mass of the first metal-organic framework material and the first carbon material is less than the ratio B2 of the mass of the second metal-organic framework material to the total mass of the second metal-organic framework material and the second carbon material, it is beneficial to the diffusion of lithium ions, thereby improving the rate performance.

[0112] According to Example 9, it is found that when the ratio B1 of the mass of the first metal-organic framework material to the total mass of the first metal-organic framework material and the first carbon material is within an appropriate range, and the ratio B2 of the mass of the second metal-organic framework material to the total mass of the second metal-organic framework material and the second carbon material is within an appropriate range, but the ratio B1 of the mass of the first metal-organic framework material to the total mass of the first metal-organic framework material and the first carbon material is greater than the ratio B2 of the mass of the second metal-organic framework material to the total mass of the second metal-organic framework material and the second carbon material, it is not conducive to the diffusion of lithium ions, resulting in a decrease in the rate performance.

[0113] The preparation method of Example 10 is basically the same as the preparation method of Example 1, except that in step S102 of Example 10, different masses of second carbon materials are further added to blend to obtain a variety of second negative electrode coatings; in step S105 of Example 10, the second negative electrode coatings with different second carbon material contents are coated layer by layer on the surface of the first negative electrode material layer, so that a plurality of sub-negative electrode material layers stacked in sequence are formed on the surface away from the first negative electrode material layer, and in the direction away from the first negative electrode material layer, the ratio of the mass of the second metal organic framework material to the total mass of the second carbon material and the second metal organic framework material in the corresponding sub-negative electrode material layer increases successively.

[0114] The preparation method of Example 11 is basically the same as the preparation method of Example 1, except that in step S102 of Example 11, different masses of second carbon materials are further added to blend to obtain a variety of second negative electrode coatings; in step S105 of Example 11, the second negative electrode coatings with different second carbon material contents are coated layer by layer on the surface of the first negative electrode material layer, so that a plurality of sub-negative electrode material layers stacked in sequence are formed on the surface away from the first negative electrode material layer, and in the direction away from the first negative electrode material layer, the ratio of the mass of the second metal organic framework material to the total mass of the second carbon material and the second metal organic framework material in the corresponding sub-negative electrode material layer decreases successively.

[0115] The negative electrode plates of the above-mentioned Examples 10 and 11 were subjected to a liquid absorption test. The solvent of the electrolyte in the liquid absorption test was EC (ethylene carbonate): DEC (diethyl carbonate): EMC (ethyl methyl carbonate) = 1:1:1 (molar ratio), and the lithium salt was LiPF6 (lithium hexafluorophosphate) with a concentration of 1 mol / L; the injection volume of the microinjector was 1 μL.

[0116] The liquid absorption time of Example 10 is 5s to 10s, and the liquid absorption time of Example 11 is 20s to 30s. It can be seen that in the direction away from the first negative electrode material layer, the ratio of the mass of the second metal-organic framework material to the total mass of the second carbon material and the second metal-organic framework material in the corresponding sub-negative electrode material layer increases successively, which is beneficial to the absorption of the electrolyte.

[0117] In the battery prepared by the preparation method of the battery provided in the embodiment of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer covering the surface of the positive electrode current collector, and the material of the positive electrode material layer is lithium iron phosphate; the negative electrode plate includes a negative electrode current collector, a first negative electrode material layer and a second negative electrode material layer, the material of the first negative electrode material layer includes a first carbon material, and the material of the second negative electrode material layer includes a second metal organic framework material, and the second metal organic framework material is a zirconium-based metal organic framework material (Zr-MOF-(COOH)) composed of zirconium metal and tetracarboxylic acid-based ligands n ), thus forming a lithium iron phosphate battery. Among them, the second metal organic framework material has good acid and alkali resistance and high stability, and there are uncoordinated, exposed carboxylic acid groups in the second metal organic framework material, and the carboxylic acid groups can capture and chelate metal ions. In this way, the second metal organic framework material, as the outermost layer of the negative electrode plate, can use the carboxylic acid groups to capture the iron ions dissolved from the positive electrode to avoid the iron ions from undergoing redox reactions and depositing on the surface of the negative electrode plate, thereby avoiding the SEI film on the surface of the negative electrode plate from being destroyed or piercing the diaphragm, so as to improve the high temperature working life of the lithium iron phosphate battery and improve the stability of the lithium iron phosphate battery.

[0118] Those skilled in the art will appreciate that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes may be made to the embodiments in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present application, and therefore the scope of protection of the present application shall be subject to the scope defined in the claims.

Claims

1. A battery, It is characterized in that include: A positive electrode sheet and a negative electrode sheet, wherein the material of the positive electrode sheet comprises lithium iron phosphate, and the negative electrode sheet comprises: Anode current collector; A first negative electrode material layer, the first negative electrode material layer covers the surface of the negative electrode current collector, and the material of the first negative electrode material layer includes a first carbon material; A second negative electrode material layer, wherein the second negative electrode material layer covers the surface of the first negative electrode material layer, wherein the material of the second negative electrode material layer comprises a second metal organic framework material, wherein the metal of the second metal organic framework material is zirconium metal, and the organic ligand of the second metal organic framework material is a tetracarboxylic acid-based ligand, and the tetracarboxylic acid-based ligand is connected to the zirconium metal through a coordination bond.

2. The battery according to claim 1, It is characterized in that The ratio of the average particle size of the first carbon material to the average particle size of the second metal organic framework material is 40-200.

3. The battery according to claim 2, It is characterized in that The particle size of the second metal organic framework material is 100nm to 500nm; the particle size of the first carbon material is 5μm to 20μm.

4. The battery according to claim 1, It is characterized in that The second negative electrode material layer includes multiple sub-negative electrode material layers stacked in sequence along a direction away from the first negative electrode material layer, and the material of each sub-negative electrode material layer includes a second carbon material and a second metal-organic framework material, and in the direction away from the first negative electrode material layer, the ratio of the mass of the second metal-organic framework material to the total mass of the second carbon material and the second metal-organic framework material in the corresponding sub-negative electrode material layer increases successively.

5. The battery according to claim 1, It is characterized in that The material of the first negative electrode material layer also includes a first metal-organic framework material; the material of the second negative electrode material layer also includes a second carbon material; wherein, in the first negative electrode material layer, the ratio of the mass of the first metal-organic framework material to the total mass of the first carbon material and the first metal-organic framework material is a first ratio; in the second negative electrode material layer, the ratio of the second metal-organic framework material to the total mass of the second carbon material and the second metal-organic framework material is a second ratio, and the second ratio is greater than the first ratio.

6. The battery according to claim 5, It is characterized in that The first ratio is 0.15-0.35; the second ratio is 0.5-0.

9.

7. A method for preparing a battery, It is characterized in that include: Prepare the positive electrode sheet and the negative electrode sheet, and the process steps for preparing the negative electrode sheet include: Preparing a second metal organic framework material, the preparation steps comprising: dispersing a zirconium source in an organic solvent, adding a tetracarboxylic acid-based ligand and then performing ultrasonic treatment, adding an acid and then performing a thermal reaction to obtain a reaction solution, and cooling, filtering and washing the reaction solution to obtain the second metal organic framework material; The second metal organic framework material is mixed with a second adhesive to obtain a second negative electrode coating; the first carbon material is mixed with a first adhesive to obtain a first negative electrode coating; Applying the first negative electrode coating to the surface of the negative electrode current collector and drying it to form a first negative electrode material layer on the surface of the negative electrode current collector; Applying the second negative electrode coating on the surface of the first negative electrode material layer and drying it to form a second negative electrode material layer on the surface of the first negative electrode material layer; The positive electrode sheet and the negative electrode sheet are assembled.

8. The method for preparing a battery according to claim 7, It is characterized in that The tetracarboxylic acid-based ligand is selected from one or more of [1,1':4',1"]terphenyl-3,3",5,5"-tetracarboxylic acid, 3,3',5,5'-biphenyltetracarboxylic acid, pyromellitic acid, 9,10-di(3',5'-dicarboxyphenyl)anthracene, 2',5'-difluoro-[1,1':4',1"-terphenyl]-3,3",5,5"-tetracarboxylic acid or pyrene-1,3,6,8-tetracarboxylic acid.

9. The method for preparing a battery according to claim 7, It is characterized in that The zirconium source is selected from one or more of zirconium nitrate, zirconium sulfate, zirconium phosphate, zirconium chloride or zirconium citrate.

10. The method for preparing a battery according to claim 7, It is characterized in that In the step of preparing the second metal organic framework material, the molar ratio of the zirconium source to the tetracarboxylic acid-based ligand is 1:1 to 4:1, the mass ratio of the solvent to the acid is 2:1 to 5:1, the temperature of the thermal reaction is 60°C to 100°C, and the time of the thermal reaction is 12h to 48h.

Citation Information